A curved solid-state accelerator neutron source target material and preparation method thereof
By designing the target layer and the substrate layer to be curved, the deformation problem caused by the difference in thermal expansion coefficient is solved, the service life of the target layer is extended, and the stability and cost-effectiveness of BNCT treatment are improved.
Patent Information
- Application Number
- CN202410231908.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-07-07
- Filing Date
- 2024-02-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-02-29
AI Technical Summary
The existing targets are deformed at high temperature due to differences in thermal expansion coefficients, which shortens their service life and affects the BNCT treatment effect and facility costs.
The substrate layer and the target layer are designed to be curved, and the opposite curved shape is pre-processed to compensate for the accumulation of thermal stress and extend the service life of the target layer.
It effectively compensates for the thermal stress accumulation of the target layer at high temperature, extends its service life, and improves the stability and cost-effectiveness of BNCT treatment.
Smart Images

Figure CN118175717B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of engineering technology, and in particular to a curved solid-state accelerator neutron source target material and a preparation method thereof. Background Art
[0002] Accelerator based boron neutron capture therapy (AB-BNCT) is a new type of tumor radiotherapy. This method first requires the injection of tumor-targeted drugs containing 10B into the patient's body. After the drug is enriched in the tumor area, the neutron beam is used to irradiate the area containing the tumor. Since the capture reaction cross section of 10B and neutrons is thousands of times higher than that of human tissue elements, neutrons will react with boron drugs in tumor tissue to form 10B(n, a)7Li. The range of the secondary particles α particles and 7Li released by this reaction is less than 1 cell diameter. Therefore, precise destruction can be produced inside tumor cells. Compared with traditional radiotherapy methods, it can kill cancer cells while minimizing damage to normal tissue cells. Therefore, this treatment method has excellent targeting and has achieved significant clinical application results.
[0003] The target is an important component of the AB-BNCT system. Its main function is to generate neutrons required for treatment. It is arranged at the end of the entire high-energy beam line and before the beam shaper. Protons accelerated by RFQ pass through the high-energy beam line to the target station. High-energy protons bombard the target to produce nuclear reactions and generate neutrons.
[0004] For target materials (such as lithium targets and beryllium targets), after a period of proton irradiation, the neutron yield and neutron flux will decrease, which will directly affect the treatment effect of BNCT. In addition, during the target shooting process, the existing target layer is prone to expansion at high temperatures due to the difference in thermal expansion coefficients between the target layer and the substrate structure and substrate layer, which causes the target layer to accumulate thermal stress and then deform, further reducing the service life of the target. Therefore, the target material currently used for BNCT needs to be replaced after a short period of irradiation. The short service life of the target material greatly affects the planning of the treatment plan and increases the operating cost of the BNCT facility, which is not conducive to the further promotion of the technology.
[0005] In view of this, it is necessary to improve the target material in the prior art to solve the above problems. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a curved solid-state accelerator neutron source target material and a preparation method thereof. The present invention designs the substrate layer and the target layer to be curved surfaces with consistent curvature radii, which can effectively compensate for the thermal stress accumulation deformation of the target layer at high temperatures, thereby ensuring the integrity of the target layer at high temperatures and ultimately effectively extending its service life.
[0007] The specific technical scheme of the present invention is:
[0008] In the first aspect, the present invention provides a curved solid-state accelerator neutron source target material, comprising: a substrate structure, a substrate layer disposed on the upper surface of the substrate structure, a target material layer disposed on the upper surface of the substrate layer, and a protective layer disposed on the periphery of the target material layer. The substrate layer and the protective layer can be removed or retained according to actual needs; the substrate layer (if any) and the target material layer are curved.
[0009] As described in the background technology section of this application, due to the difference in thermal expansion coefficients between the existing target material layer and the substrate structure and substrate layer (for example, the thermal expansion coefficient of the lithium target material layer is larger, while the thermal expansion coefficients of the copper substrate structure and the tantalum substrate layer are smaller), the target material layer is prone to expansion under high temperatures during the target shooting process, causing the target material layer to accumulate thermal stress and then deform, further reducing the service life of the target material layer.
[0010] To this end, the present invention sets the substrate layer (if any) and the target layer to be curved. The inventors have found that pre-processing the surface of the basic structure into a curved surface shape opposite to the deformation before plating the target layer can compensate for the deformation of the target layer, thereby ensuring the integrity of the target layer at high temperatures and ultimately effectively extending its service life.
[0011] Preferably, when the thermal expansion coefficient of the substrate structure is smaller than that of the target material layer, the curved surface is concave at the top and convex at the bottom (concave curved surface); when the thermal expansion coefficient of the substrate structure is larger than that of the target material layer, the curved surface is convex at the top and concave at the bottom (convex curved surface).
[0012] Preferably, the sagittal height of the target layer is P±10%:
[0013]
[0014] In the present invention, the sagitta refers to the vertical distance from a point on the curved surface to the lowest point (bottom of the valley) on the curved surface. Where: P is the sagitta to be compensated, t f With t s are the target layer thickness and substrate structure thickness respectively, D is the target layer diameter, α f With α sare the thermal expansion coefficients of the target layer and the substrate structure, T1 is the highest temperature of the target layer during target shooting, and T0 is room temperature. Since the substrate layer (if any) is usually thin and has a small thermal expansion coefficient, its thermal stress accumulation can be ignored here. It is ideal to determine the arrow height within the range of P error ±10%.
[0015] Preferably, the target layer is a lithium target layer or a beryllium target layer; the material of the substrate layer is selected from tantalum, vanadium, palladium, platinum, titanium, niobium or their alloys.
[0016] Preferably, the shape of the surface of the substrate structure on one side in contact with the target layer or substrate layer (if any) matches the shape of the lower surface of the target layer or substrate layer. That is, if the lower surface of the target layer or substrate layer is a concave curved surface, the upper surface of the substrate structure is a convex curved surface; if the lower surface of the target layer or substrate layer is a convex curved surface, the upper surface of the substrate structure is a concave curved surface.
[0017] Preferably, the shape of the surface of the protective layer in contact with the upper surface of the target layer matches the shape of the upper surface of the target layer. That is, if the upper surface of the target layer is a concave curved surface, the protective layer is a convex curved surface; if the upper surface of the target layer is a convex curved surface, the protective layer is a concave curved surface; the other side of the protective layer can be a plane, a concave curved surface or a convex curved surface.
[0018] Preferably, the substrate layer and the target material layer are in a disc structure and are arranged in concentric circles.
[0019] Preferably, the substrate layer and the target layer have the same curvature radius.
[0020] In a second aspect, the present invention provides a method for preparing a curved solid-state accelerator neutron source target material, comprising the following steps: S1: preparing a substrate layer on the upper surface of a substrate structure;
[0021] S2: preparing a target material layer on the upper surface of the substrate layer;
[0022] S3: preparing a protective layer on the upper surface of the target layer.
[0023] Preferably, in S1, the substrate layer is prepared by a magnetron sputtering coating method; in S2, the target layer is prepared by a thermal evaporation deposition method; in S3, the protective layer is prepared by a magnetron sputtering coating method.
[0024] Further preferably, in S2, the thermal evaporation deposition method specifically comprises the following steps: placing the substrate into the evaporation device, turning on the vacuum coating device, first pumping the pressure in the chamber to below 10Pa, then turning on the molecular pump, and after the molecular pump reaches the maximum speed and runs stably, pumping the pressure in the chamber to 8.0×10 -4Pa, turn on the evaporation source and film thickness meter, and after the evaporation rate stabilizes, open the substrate baffle and start coating.
[0025] Compared with the prior art, the beneficial effect of the present invention is that the target material layer is set to a curved surface in the present invention, and this design can effectively compensate for the thermal stress accumulation deformation of the target material layer at high temperature, thereby ensuring the integrity of the target material layer at high temperature and ultimately effectively extending its service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A cross-sectional view of a curved solid-state accelerator neutron source target material having a concave curved surface in Example 1 of the present invention (for ease of display, the thickness of each layer is not shown in actual proportion);
[0027] Figure 2 This is an overall schematic diagram of the curved solid-state accelerator neutron source target material in Example 1 of the present invention (anatomical diagram, for ease of display, the thickness of each layer is not shown in actual proportion);
[0028] Figure 3 An exploded view of the curved solid-state accelerator neutron source target material in Example 1 of the present invention;
[0029] Figure 4 This is a schematic structural diagram of a cooling component in a curved solid-state accelerator neutron source target in Example 1 of the present invention;
[0030] Figure 5 A cross-sectional view of a curved solid-state accelerator neutron source target material having a concave curved surface in Example 2 of the present invention (for ease of display, the thickness of each layer is not shown in actual proportion);
[0031] Figure 6 This is an overall schematic diagram of the curved solid-state accelerator neutron source target material in Example 2 of the present invention (anatomical diagram, for ease of display, the thickness of each layer is not shown in actual proportion);
[0032] Figure 7 This is an exploded view of the curved solid-state accelerator neutron source target material in Example 2 of the present invention.
[0033] The figures are marked as follows: 1-substrate structure; 11-upper shell of substrate structure; 12-lower shell of substrate structure; 13-cooling component; 2-substrate layer; 3-lithium diffusion barrier layer; 4-target layer; 5-protective layer; 6-cooling medium inlet; 7-cooling medium outlet. DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with the various embodiments shown in the accompanying drawings, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.
[0035] It should be understood that, in the present application, the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "axial", "radial", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the present technical solution and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present technical solution.
[0036] It is particularly important to note that in the following embodiments, boron neutron capture therapy (Boron NeutronCapture The principle of BNCT is to use the nuclear reaction that occurs in tumor cells to destroy tumor cells. First, a compound containing 10B is introduced into the patient's body. Since this compound has a strong affinity with tumor cells, it quickly accumulates in tumor cells after entering the body, and is rarely distributed in other normal tissues. Then, a neutron beam is used to irradiate the tumor site, so that neutrons react with 10B accumulated in tumor cells. After 10B captures neutrons, an unstable composite nucleus 11B is generated. 11B then spontaneously splits into an alpha particle with a kinetic energy of 1.78MeV and a 7Li recoil nucleus with a kinetic energy of 1.01MeV (reaction cross section is 6.3%); or an alpha particle with a kinetic energy of 1.47MeV and a 7Li recoil nucleus with a kinetic energy of 0.84MeV and emits a photon with an energy of 0.48MeV (reaction cross section is 93.7%). 11B spontaneously splits into alpha particles and 7Li recoil nuclei through the following two reactions. The reaction formula is as follows:
[0037] 10B+nth→11B→7Li(1.01MeV)+4He(1.78MeV) 6.3%
[0038] 10B+nth→11B→7Li(0.84MeV)+4He(1.47MeV)+γ(0.48MeV) 93.7%
[0039] The reaction products of this process, α particles and 7Li recoil nuclei, have the characteristics of high linear energy transfer (LET) and low oxygen enhancement ratio, which can kill tumor cells with high selectivity and intensity while minimizing damage to surrounding normal tissues.
[0040] The term "AB-BNCT" refers to accelerator based boronneutron capture therapy (AB-BNCT).
[0041] AB-BNCT is an accelerator-based boron neutron capture therapy technology that combines the principles of ion accelerator and boron neutron capture therapy. In AB-BNCT, an ion accelerator is first used to generate a high-energy ion beam, usually a proton or deuterium ion beam. These ion beams are accelerated to a certain energy and then injected into a specific target material, such as a boride, at a high speed. When the ion beam interacts with the target material, high-energy neutrons are produced. The generated neutrons are guided to the tumor area in the patient's body, into which a compound enriched in the boron-10 isotope has been injected. Boron-10 undergoes a neutron capture reaction with the incident neutrons to produce high-energy alpha particles and nuclear fission fragments, thereby destroying tumor cells.
[0042] Example 1 (without lithium diffusion barrier layer)
[0043] like Figure 1-3 As shown, a curved solid-state accelerator neutron source target material comprises: a substrate structure 1, a substrate layer 2 arranged on the substrate structure, the substrate structure 1 being in contact with the substrate layer 2; a target material layer 4 arranged on the substrate layer, the substrate layer being in contact with the target material layer 4; and a protective layer 5 arranged on the periphery of the target material layer 4, the substrate layer and the protective layer 5 being arranged around the periphery of the target material layer 4; the substrate layer 2 and the target material layer 4 are both arranged in a curved surface shape with a consistent curvature radius (such as Figure 1 shown).
[0044] The substrate structure 1 includes a substrate structure upper shell 11 and a substrate structure lower shell 12 which are assembled, clamped, welded or integrally formed. The materials of the substrate structure 1 can be selected as follows: silicon substrate, quartz substrate, ceramic substrate: ceramic materials such as alumina (Alumina), aluminum nitride (Aluminum Nitride), etc., metal substrate: metal materials such as aluminum, copper, silver, nickel, iron, stainless steel, etc. Polymer substrate: polymer materials such as polyimide (Polyimide), polymethyl methacrylate (PMMA), etc. Of course, it is not limited to those listed. Considering the cost and heat dissipation performance, copper is preferably used in this embodiment.
[0045] like Figure 4As shown, a cooling component 13 for cooling the target layer is provided on the upper shell 11 of the substrate structure. The cooling component in the present application is not particularly limited. From the perspective of cooling efficiency, it is preferably an array cooling structure, which includes a cooling medium, a heat dissipation component for the cooling medium to contact, and a substrate structure upper shell 11 for accommodating the heat dissipation component. The cooling medium can be selected as cooling water, liquid nitrogen and other cooling media. Preferably, the arrangement of the heat dissipation component is an array arrangement. Specifically, the array arrangement heat dissipation component arranges multiple identical or similar heat dissipation components together in a certain regularity or pattern. The heat dissipation components can have the same size, shape, etc., or be appropriately adjusted and optimized according to specific needs. Preferably, the distance between the heat dissipation components is less than 5 mm, and more preferably, the distance between the heat dissipation components is less than 2 mm. For the heat dissipation component, a cylindrical or rectangular shape or the like can be selected, and more preferably, the heat dissipation component is a cylinder with a diameter of 2 mm; the material of the heat dissipation component can be a material that can dissipate heat, such as metal, and more specifically, copper can be listed.
[0046] The array cooling structure provides a larger surface area and contact area, enhancing the heat transfer and heat dissipation capabilities. In addition, due to the close arrangement between the heat dissipation components, the heat transfer is more uniform, helping to avoid the formation of hot spots.
[0047] like Figure 3 As shown, a cooling medium inlet 6 and a cooling medium outlet 7 are respectively provided on the lower shell 12 of the substrate structure. The cooling medium enters from the cooling medium inlet 6 , then flows in the space between the heat dissipation components, and then flows out through the cooling medium outlet 7 .
[0048] The number of the cooling medium inlet 6 and the cooling medium outlet 7 is preferably 3 or more. A design of 3 or more can make the flow of the cooling medium more uniform, thereby resulting in more uniform heat dissipation, thereby preventing the target layer 4 from melting under the irradiation of particles.
[0049] The substrate layer 2 is provided on the substrate structure (it can be selected whether to be provided according to the situation). The material of the substrate layer 2 can be selected from tantalum, vanadium, palladium, platinum, titanium, niobium or their alloys. In this embodiment, metal tantalum is preferred. Tantalum is a metal material that is corrosion-resistant, has a high melting point and high thermal stability. Therefore, it is used as the substrate layer in this application. It is prepared by a magnetron sputtering coating method, that is, a thin film or coating is deposited on the substrate structure using magnetron sputtering technology. The thickness of the substrate layer 2 can be selected from 10-40 μm (micrometers), and 20 μm (micrometers) is more preferred in this embodiment.
[0050] It should be noted that the magnetron sputtering coating method is a method known in the art. For example, in the magnetron sputtering process, an inert gas (such as argon) is used to form a low-pressure environment, and then an ionized particle is generated on the target material by applying a magnetic field. These ionized particles are sputtered on the surface of the target material and deposited on the substrate structure to form a substrate layer.
[0051] The preparation of the metal tantalum substrate layer by magnetron sputtering can provide a solid substrate for the subsequent process steps, which can improve the adhesion and structural stability of the substrate. Since the threshold of hydrogen bubbling under proton bombardment of the substrate layer material is much higher than that of copper, the main function of the substrate layer is to make the incident protons finally stay in this layer instead of entering the copper substrate structure, thereby preventing the occurrence of hydrogen bubbling and improving the service life of the target.
[0052] The target material layer 4 disposed on the substrate layer is preferably a lithium target in this embodiment, but its protection scope is not limited to the lithium target. For example, without departing from the concept of the present invention, the beryllium target still constitutes an equivalent arrangement to the lithium target.
[0053] Compared with the beryllium target, the lithium target requires lower proton energy to produce the desired neutrons. Therefore, in this embodiment, the lithium target is preferably used.
[0054] For the target material, after a period of proton irradiation, the neutron yield will decrease and the neutron flux will decrease, which will directly affect the treatment effect of AB-BNCT. Therefore, the target material currently used for AB-BNCT needs to be replaced after a short period of irradiation. The short service life of the target material affects the planning of the treatment plan and increases the operating cost of the AB-BNCT equipment. It is not conducive to the promotion of AB-BNCT therapy. The factor affecting the neutron yield is the thickness of the target material layer. During the process of proton bombardment of the target material layer, the thickness of the target material layer will decrease and become uneven, such as sputtering of the target material layer under proton bombardment, mutual diffusion of the target material layer and the substrate layer when the temperature rises, etc. A series of factors reduce the service life of the target material layer.
[0055] At the same time, due to the low melting point of lithium, if the heat accumulation caused by proton irradiation cannot be removed in time, the temperature of the substrate layer will rise and the target layer will melt, reducing the service life of the target layer.
[0056] In addition, in the present invention, the target material layer is prepared by thermal evaporation deposition.
[0057] Specifically, the target layer is deposited by thermal evaporation method, which includes the following steps: placing the substrate into the evaporation equipment, turning on the vacuum coating equipment, first pumping the pressure in the chamber to below 10Pa, then turning on the molecular pump, and after the molecular pump reaches the maximum speed and runs stably, pumping the pressure in the chamber to 8.0×10 -4Pa, turn on the evaporation source and film thickness meter, and after the evaporation rate stabilizes, open the substrate baffle and start coating.
[0058] More specific steps are:
[0059] Prepare the substrate: Place the substrate to be coated into the evaporation equipment. The substrate is cleaned in advance to ensure that the surface is clean, dust-free and free of impurities.
[0060] Turn on the vacuum coating equipment: Turn on the evaporation equipment and make sure the chamber is sealed.
[0061] Vacuuming: Use a vacuum pump to reduce the pressure in the chamber to below 10 Pa. Usually, a mechanical pump is used to exhaust most of the gas first, and then a molecular pump is used to further reduce the pressure.
[0062] Start the molecular pump: Turn on the molecular pump and adjust its speed so that it gradually reaches the maximum speed and runs stably. The role of the molecular pump is to further reduce the pressure in the chamber.
[0063] Further vacuuming: Using the molecular pump, the pressure in the chamber is further reduced to 8.0×10 -4 Pa. Higher vacuum conditions help reduce the collision of gas molecules and provide a better deposition environment.
[0064] Turn on the evaporation source and film thickness meter: Turn on the evaporation source, usually by heating the lithium target to the evaporation temperature through a heating source. At the same time, turn on the film thickness meter to monitor the thickness of the coating in real time.
[0065] Stabilize the evaporation rate: After the evaporation source starts to heat up, wait for the evaporation rate to stabilize.
[0066] Open the substrate baffle: After the evaporation rate is stable, open the substrate baffle to start evaporating and depositing lithium particles on the substrate. The function of the substrate baffle is to block the lithium particles before the evaporation source is turned on to avoid contaminating the substrate.
[0067] Coating: After the substrate shutter is opened, lithium particles will be deposited on the substrate surface. The evaporation source and film thickness meter will continue to work to maintain a stable evaporation rate and monitor the thickness of the coating.
[0068] The thin film prepared by thermal evaporation deposition method often exhibits tensile stress, and because the thermal expansion coefficient of lithium is large, if the thermal expansion coefficient of the substrate structure and the substrate layer is small, the lithium film will expand when the temperature rises due to proton bombardment of the lithium target, causing the lithium film to be subjected to compressive stress and then deformed, further reducing the service life of the lithium target layer.
[0069] In order to solve this technical problem, the inventors of the present application further improved the design, and set the substrate layer, the lithium diffusion barrier layer and the lithium target layer to have a curved surface with a consistent curvature radius, as shown in FIG. Figure 1 As shown, the curved surface can be designed as a concave curved surface or a convex curved surface according to the situation (if the thermal expansion coefficient of the substrate structure is smaller than that of the target material layer, the curved surface is a concave curved surface with a concave top and a convex bottom; if the thermal expansion coefficient of the substrate structure is larger than that of the target material layer, the curved surface is a convex curved surface with a convex top and a concave bottom). The inventors found that when the compressive stress exceeds the limit of the lithium film, the film will bend. Before coating, the substrate layer is pre-processed into the opposite shape of the film deformation, which can compensate for the deformation of the lithium film, thereby ensuring the integrity of the lithium film at high temperature.
[0070] In this embodiment, if Figure 3 As shown, it is preferably a concave surface, and the surface sagitta is calculated by the following formula (allowable error ±10%):
[0071]
[0072] Where P is the vector height that needs to be compensated, t f With t s are the target layer thickness and substrate structure thickness respectively, D is the target layer diameter, α f With α g are the thermal expansion coefficients of the target layer and the substrate structure, T1 is the highest temperature of the target layer during target shooting, and T o is room temperature. Since the substrate layer is thin and has a small thermal expansion coefficient, its thermal stress accumulation can be ignored. The preferred range of the sagitta of the concave surface is 120-200 microns, and in this embodiment, it is further preferably 150 microns. The "sagitta of the concave surface" refers to the vertical distance from a point on the surface to the lowest point (valley bottom) on the surface.
[0073] like Figure 2 As shown, the substrate layer and the target layer disposed on the substrate layer in this embodiment are in a disc structure and are arranged in concentric circles. Of course, they can also be arranged in other shapes, and the present invention is not limited to the disc structure design.
[0074] The protective layer 5 is disposed on the periphery of the target layer 4 , and the substrate layer and the protective layer 5 are disposed around the periphery of the target layer to cover the target layer 4 .
[0075] The protective layer 5 is used, firstly, to avoid sputtering of the target layer due to proton bombardment. The protective layer can serve as a physical isolation layer to reduce the effects of sputtering and corrosion. Secondly, the integrity of the target layer is protected. The protective layer can prevent impurities, gases or liquids in the external environment from entering the target layer to ensure the integrity and purity of the target layer. Thirdly, it can provide structural support for the curved solid target, enhance the overall stability and strength, and reduce the effects of external vibration or stress on the target layer.
[0076] The protective layer 5 is usually made of a material with high heat resistance, corrosion resistance and chemical stability to ensure its reliability and durability in environments such as proton bombardment. Common material choices include metals (such as stainless steel, titanium alloy), ceramics (such as aluminum oxide, silicon nitride) or high-temperature polymers (such as polyimide).
[0077] Further preferably, the protective layer can be selected to be carbide ceramics, nitride ceramics or high entropy alloys.
[0078] Examples of carbide ceramics include any one or more combinations of zirconium carbide, silicon carbide, titanium carbide, tungsten carbide, boron carbide, aluminum carbide, silicon carbide nitrogen, molybdenum carbide, niobium carbide, hafnium carbide, chromium carbide, tantalum carbide, and vanadium carbide.
[0079] Examples of nitride ceramics include any one or more combinations of silicon nitride, aluminum nitride, titanium nitride, molybdenum nitride, and tungsten nitride.
[0080] Most preferably, the protective layer in this embodiment is zirconium carbide.
[0081] The applicant has found that the protective layer is preferably zirconium carbide covering the surface of the target layer to avoid sputtering caused by proton bombardment, help maintain the integrity of the target layer, and has good radiation resistance, and can maintain the effectiveness of the protective layer in a proton bombardment environment.
[0082] It should be noted that the side of the protective layer 5 in contact with the target layer 4 has a shape matching that of the target layer 4, that is, presenting a convex surface, and the other side of the protective layer 5 may be a plane, a concave surface or a convex surface.
[0083] The method for preparing the curved solid-state accelerator neutron source target material as described above comprises the following steps:
[0084] Preparing a substrate structure; a cooling component is arranged in the substrate structure;
[0085] One side of the substrate structure is processed into a concave surface according to a predetermined curvature, and a substrate layer, a target material layer and a protective layer are sequentially prepared on the concave surface;
[0086] The substrate layer is prepared by a magnetron sputtering coating method;
[0087] The target material layer is prepared by a thermal evaporation deposition method;
[0088] The protective layer is prepared by a magnetron sputtering coating method, and the substrate layer and the protective layer are arranged around the periphery of the target material layer.
[0089] In a preferred embodiment, the specific concept of the method of magnetron sputtering coating the substrate layer is: during the magnetron sputtering process, an inert gas (such as argon) is used to form a low-pressure environment, and then ionized particles are generated on the target material by applying a magnetic field. These ionized particles are sputtered on the surface of the target material and deposited on the substrate structure to form a substrate layer.
[0090] Preferably, the substrate layer is prepared by a magnetron sputtering coating method, and the specific concept is as follows:
[0091] (1) Equipment preparation: Prepare the magnetron sputtering equipment and ensure the normal operation and vacuum state of the equipment, and ensure that the target material (such as tantalum or molybdenum) in the equipment has been installed on the target gun.
[0092] (2) Target material preparation: The target material is cut into blocks of appropriate size, cleaned and placed on the target gun of the magnetron sputtering equipment.
[0093] (3) Vacuum pumping: Start the magnetron sputtering equipment and pump the pressure in the chamber to below the required vacuum level (usually within 10 -4 -10 -6 Pa).
[0094] (4) Gas injection: Inject inert gas (such as argon) into the chamber to create an inert atmosphere and maintain a stable working gas pressure.
[0095] (5) Target gun adjustment: Adjust the position and angle of the target gun to align it with the substrate layer.
[0096] (6) Target sputtering: The target gun is powered on to generate a high-energy particle beam that hits the target material. The atoms in the target material will be knocked out and deposited on the substrate layer to form a lithium diffusion barrier.
[0097] (7) Film thickness control: The thickness of the lithium diffusion barrier layer can be controlled and adjusted by controlling the sputtering time and power, as well as by monitoring the film thickness (such as a film thickness meter).
[0098] (8) End of sputtering: After the required sputtering time is completed, the target gun is powered off and the sputtering process ends.
[0099] Preferably, the target layer is deposited by thermal evaporation method, which specifically includes the following steps: placing the substrate into the evaporation equipment, turning on the vacuum coating equipment, first pumping the pressure in the chamber to below 10Pa, then turning on the molecular pump, and after the molecular pump reaches the maximum speed and runs stably, pumping the pressure in the chamber to 8.0×10 -4 Pa, turn on the evaporation source and film thickness meter, and after the evaporation rate stabilizes, open the substrate baffle and start coating.
[0100] Example 2 (including lithium diffusion barrier layer)
[0101] This embodiment provides another curved solid-state accelerator neutron source target material, such as Figure 5-7 As shown, the difference from Example 1 is that it also includes a lithium diffusion barrier layer 3, which specifically includes: a substrate structure 1 (copper), a substrate layer 2 (tantalum) arranged on the substrate structure, and the substrate structure 1 is in contact with the substrate layer 2; the lithium diffusion barrier layer 3 is arranged on the substrate layer, and the other side of the substrate layer 2 (that is, the opposite side in contact with the substrate structure 1) is in contact with the lithium diffusion barrier layer 3; a target layer 4 (lithium target material) is arranged on the lithium diffusion barrier layer 3, and the lithium diffusion barrier layer 3 is in contact with the target layer 4; and a protective layer 5 is arranged on the periphery of the target layer 4, and the lithium diffusion barrier layer 3 and the protective layer 5 are surrounded by the periphery of the target layer 4.
[0102] Among them, the substrate layer, lithium diffusion barrier layer and target layer are curved surfaces with the same curvature radius (concave surface with concave top and convex bottom, the size parameters of each layer except the lithium diffusion barrier layer are the same as those in Example 1, and the vector height of the lithium diffusion barrier layer is the same as that of the target layer).
[0103] In this embodiment, the lithium diffusion barrier is used to prevent the diffusion of lithium in the target layer from escaping the target layer, while maintaining the integrity and stability of the target layer. The lithium diffusion barrier is usually made of a material with high lithium diffusion resistance and chemical stability. For example, the material is a metal or alloy, such as tantalum (Ta) or molybdenum (Mo), which has a low diffusion coefficient and high corrosion resistance. These materials hinder the diffusion of lithium by forming an isolation layer between the target layer and other environments. When the material of the substrate layer is the same as that of the lithium diffusion barrier (for example, when both are tantalum), they can be merged into the same layer.
[0104] The inventors have found that replacing the lithium diffusion barrier with rare earth metal oxides such as silicon carbide, aluminum nitride, yttrium oxide, and erbium oxide can better prevent the diffusion of lithium, making it difficult for the target material to diffuse at high temperatures, thereby maintaining the integrity of the lithium layer and preventing the thickness of the lithium film from decreasing.
[0105] Optionally, the lithium-blocking diffusion layer 3 can be set as a silicon carbide layer. And the thickness of the lithium-blocking diffusion layer 3 is not easy to be too thick, preferably less than 5 μm (micrometer), and 1 μm (micrometer) is most preferably used in this embodiment; if the lithium-blocking diffusion layer 3 is too thick, the transmission path of lithium ions will become longer, which will increase the resistance and time of transmission and reduce the diffusion rate of lithium ions in the target layer. In addition, an overly thick lithium-blocking diffusion layer may produce a large stress difference, resulting in structural deformation. To solve this technical problem, on the one hand, by setting the thickness of the lithium-blocking diffusion layer 3, and on the other hand, by controlling the thickness ratio of the substrate layer 2, the lithium-blocking diffusion layer 3, and the target layer 4 to (10-40): 1: (140-160), further preferably, when the material of the substrate layer is tantalum or palladium, the thickness ratio of the substrate layer, the lithium-blocking diffusion layer and the lithium target layer is (18-22): 1: (140-160); when the material of the substrate layer is vanadium, the thickness ratio of the substrate layer, the lithium-blocking diffusion layer and the lithium target layer is (27 -33)∶1∶(140-160); when the material of the substrate layer is platinum, the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (13-17)∶1∶(140-160); when the material of the substrate layer is titanium, the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (31-39)∶1∶(140-160); when the material of the substrate layer is niobium, the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (22-28)∶1∶(140-160). In this embodiment, the substrate layer is tantalum, and the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is preferably 20:1:150. The method for preparing the curved solid-state accelerator neutron source target material as described above comprises the following steps:
[0106] Preparing a substrate structure; a cooling component is arranged in the substrate structure;
[0107] One side of the substrate structure is processed into a concave surface according to a predetermined curvature, and a substrate layer, a lithium diffusion barrier layer, a target material layer and a protective layer are sequentially prepared on the concave surface;
[0108] The substrate layer and the lithium diffusion barrier layer are both prepared by magnetron sputtering coating method;
[0109] The target material layer is prepared by a thermal evaporation deposition method;
[0110] The protective layer is prepared by a magnetron sputtering coating method, and the lithium diffusion barrier layer and the protective layer are arranged around the periphery of the target material layer.
[0111] Example 3 (target layer is beryllium target layer)
[0112] This embodiment provides another curved solid-state accelerator neutron source target material. The difference from the first embodiment is that the target layer is a beryllium target layer, and the substrate structure is also copper. Since the thermal expansion coefficient of beryllium is smaller than that of copper, the upper surface of the substrate structure needs to be processed into a convex curved surface, that is, the substrate layer and the beryllium target layer are curved surfaces with convex upper surface and concave lower surface, and the sagittal height is also calculated by the following formula (allowable error ±10%):
[0113]
[0114] Example 4 (without substrate layer)
[0115] This embodiment provides another curved solid-state accelerator neutron source target material, which is different from Embodiment 1 only in that no substrate layer is provided, that is, the target material layer is directly deposited on the surface of the substrate structure.
[0116] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0117] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A curved solid-state accelerator neutron source target, characterized in that include: Substrate structure; A substrate layer disposed on the upper surface of the substrate structure; A lithium diffusion barrier layer disposed on the upper surface of the substrate layer; A target material layer is arranged on the upper surface of the lithium diffusion barrier layer; the target material layer is a lithium target layer; The substrate layer, the lithium diffusion barrier layer and the target layer are in a curved surface shape; The material of the lithium diffusion barrier layer is selected from one or more of silicon carbide, aluminum nitride, yttrium oxide, erbium oxide, tantalum and molybdenum; The thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (10-40):1:(140-160).
2. The curved solid-state accelerator neutron source target according to claim 1, characterized in that: The thermal expansion coefficient of the substrate structure is smaller than that of the target material layer, and the curved surface is concave at the top and convex at the bottom; or The thermal expansion coefficient of the substrate structure is greater than that of the target material layer, and the curved surface is convex upward and concave downward.
3. The curved solid-state accelerator neutron source target according to claim 1 or 2, characterized in that: The target layer has a sagittal height of P ± 10%: Where: P is the arrow height, t f With t s are the thickness of the target layer and substrate structure respectively, D is the diameter of the target layer, α f With α s are the thermal expansion coefficients of the target layer and substrate structure respectively, T1 is the highest temperature of the target layer during shooting, and T0 is the room temperature.
4. The curved solid-state accelerator neutron source target according to claim 1, characterized in that: The material of the substrate layer is selected from tantalum, vanadium, palladium, platinum, titanium, niobium or alloys thereof.
5. The curved solid-state accelerator neutron source target according to claim 1, characterized in that: The substrate layer, the lithium diffusion barrier layer and the target material layer have the same curvature radius.
6. The curved solid-state accelerator neutron source target according to claim 1, characterized in that: A protective layer is provided on the periphery of the target material layer.
7. The curved solid-state accelerator neutron source target according to claim 1, characterized in that: The thickness of the lithium diffusion barrier layer is less than 5 microns.
8. The curved solid-state accelerator neutron source target according to claim 1, characterized in that: The material of the substrate layer is tantalum or palladium, and the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (18-22):1:(140-160); or The material of the substrate layer is vanadium, and the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (27-33):1:(140-160); or The substrate layer is made of platinum, and the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (13-17):1:(140-160); or The substrate layer is made of titanium, and the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (31-39):1:(140-160); or The substrate layer is made of niobium, and the thickness ratio of the substrate layer, the lithium diffusion barrier layer and the lithium target layer is (22-28):1:(140-160).
9. A method for preparing a curved solid-state accelerator neutron source target according to claim 1, characterized in that The following steps are involved: S1: preparing a substrate layer on the upper surface of the substrate structure; S2: preparing a lithium diffusion barrier layer on the upper surface of the substrate layer; S3: preparing a target material layer on the upper surface of the lithium diffusion barrier layer; S4: preparing a protective layer on the upper surface of the target layer.
10. The preparation method according to claim 9, characterized in that: In S1, the substrate layer and the lithium diffusion barrier layer are prepared by magnetron sputtering coating method; In S2, the target material layer is prepared by thermal evaporation deposition; In S3, the protective layer is prepared by a magnetron sputtering coating method.