A spinel-type lithium titanate electrochromic thin film and its preparation method
By combining the sol-gel method and the blade coating method at low temperatures, the problem of lithium loss caused by high-temperature processing was solved, and a high-performance LTO thin film with excellent optical modulation performance and cycle stability was prepared.
Patent Information
- Application Number
- CN202410296516.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Existing methods for preparing lithium titanate thin films require prolonged high-temperature treatment, which leads to coarsening of particles and loss of lithium content, affecting ion conductivity. Furthermore, existing methods are difficult to use for preparing high-performance nano-LTO materials.
LTO precursor solution was prepared by sol-gel method, and dense LTO film was prepared at low temperature by blade coating method. Single-phase spinel structure LTO film was prepared by controlling the heat treatment temperature at 400-500℃.
A high-performance LTO thin film with low energy consumption and no pollution was prepared. The film has an optical modulation amplitude of 40% in the range of 400 to 1100 nm, a fast coloring/fading response time, and good cycling stability. After 1000 cycles, it still maintains an optical modulation amplitude of 38%.
Smart Images

Figure CN118184167B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochromic device fabrication, specifically to a spinel-type lithium titanate electrochromic thin film and its preparation method. Background Technology
[0002] Electrochromism is a phenomenon where the optical properties of a material (reflectivity, transmittance, absorptivity, etc.) undergo stable and reversible color changes under the influence of an applied electric field, manifesting as reversible changes in color and transparency. Therefore, electrochromic materials have high practical application value in building curtain walls, smart windows, anti-glare rearview mirrors, and spacecraft thermal control devices. Lithium titanate (LTO) electrochromic films possess excellent electronic and ionic conductivity, high coloring efficiency, and large optical modulation amplitude. Furthermore, due to its "zero strain" characteristic and excellent reversible lithium insertion and extraction, LTO is one of the most promising cathode electrochromic materials currently under research.
[0003] The quality of electrochromic material preparation significantly affects the performance of electrochromic devices. Currently, due to different preparation methods and conditions, the performance of LTO thin films varies considerably, making the search for optimal LTO film preparation methods and conditions a major focus. Currently, there are two main methods for LTO preparation: solid-state and liquid-state methods. Solid-state methods can be further subdivided into high-temperature solid-state methods, melt impregnation methods, and microwave chemical methods; liquid-state methods include sol-gel methods and hydrothermal reaction methods. On the other hand, the performance of electrochromic devices depends on their size and crystallinity. Nanoscale LTO materials can effectively shorten the Li-Li ratio. + The diffusion path is improved, and the larger specific surface area allows for sufficient contact between the negative electrode material and the electrolyte, which is beneficial for electron transport. These factors can greatly improve the electrochemical performance of LTO.
[0004] However, current methods for preparing lithium titanate (LTO) materials require prolonged high-temperature processing, which can lead to particle coarsening and lithium loss, reducing their ionic conductivity. Therefore, it is desirable to develop a simple low-temperature synthesis method for preparing LTO nanomaterials. Summary of the Invention
[0005] To address the aforementioned issues, a low-temperature, non-toxic, and environmentally friendly method is provided to prepare LTO precursor solution and combine it with a blade coating method to prepare a high-performance LTO electrochromic film. This method offers lower heat treatment temperatures compared to existing processes, and the blade coating method yields a dense LTO film, which can greatly benefit the practical application of lithium titanate materials.
[0006] To achieve the above objectives, the specific technical solution is as follows:
[0007] The present invention provides a method for preparing a spinel-type lithium titanate electrochromic thin film, comprising the following steps:
[0008] Step 1: Prepare the LTO precursor solution using the sol-gel method:
[0009] Ti{OCH(CH3)2}4 was dissolved in deionized water to obtain solid titanium hydroxide. After centrifugation, it was redispersed in deionized water and ultrasonically dispersed. H2O2 solution and solid LiOH were added sequentially under stirring to obtain lithium titanate precursor solution.
[0010] Step 2: Prepare LTO electrochromic thin films using a blade coating method:
[0011] Cut a small piece of tape and stick it to one end of the treated substrate to serve as an electrode. Place the substrate, which serves as the electrode, on a glass substrate and fix it in place. Use a dropper to draw up the LTO precursor solution prepared in step one and drop it onto one end near the tape. Quickly slide the coater placed on the substrate to make the added solution form a film. After heat treatment, an LTO thin film is obtained.
[0012] Furthermore, the molar ratio of Ti{OCH(CH3)2}4 to LiOH in step one is (0.096-1.8):(0.12-2.0).
[0013] Furthermore, the number of centrifugation cycles in step one is 2-3, the centrifugation speed range is 500-10000 r / m, and the ultrasonic dispersion time is 20-30 min.
[0014] Furthermore, the stirring described in step one is magnetic stirring, and the magnetic stirring time is 4-6 hours. During the stirring process, H2O2 solution is added dropwise. When the liquid changes from a turbid state to an orange transparent state, LiOH solid is added to obtain a yellow transparent clear lithium titanate precursor solution.
[0015] Furthermore, the substrate described in step two is FTO conductive glass.
[0016] Further, the substrate processing procedure in step two is as follows: First, fluorine-doped SnO2 (FTO) conductive glass is immersed in deionized water, and ultrasonic cleaning is performed for 8 minutes with the addition of photoelectric cleaning agent to remove organic stains on the substrate surface; then, the FTO conductive glass is transferred to a clean petri dish, and deionized water is added to cover the surface of the FTO conductive glass, and ultrasonic cleaning is performed again for 8 minutes to remove residual photoelectric cleaning agent; then, the FTO conductive glass is transferred to a clean petri dish, and anhydrous ethanol is added to cover the FTO surface, and ultrasonic cleaning is performed for 8 minutes to remove residual anhydrous ethanol, resulting in cleaned FTO conductive glass; the cleaned FTO conductive glass is dried and then placed in a plasma device for 15 minutes to obtain an FTO substrate with good wettability, which is the processed substrate.
[0017] Furthermore, the thickness of the film described in step two is related to the specifications of the coater, which is 60-120 μm.
[0018] Furthermore, the coating speed of the coating device described in step two is 10-15 mm / s, and 5-15 layers are coated.
[0019] Furthermore, the heat treatment temperature in step two is 400-500℃, and the heat treatment time is 3-4 hours, ensuring that the substrate is made of conductive glass.
[0020] A spinel-type lithium titanate (LTO) electrochromic thin film, wherein the thin film has a single-phase spinel crystal structure and exhibits an optical modulation amplitude of 40% in the spectral range of 400–1100 nm; the thin film has a rapid on / off response time, with on / off response times of 5–10 s and 8–15 s respectively at an adjustable voltage of -2.5 V / +1 V; and the thin film has excellent cycling stability, maintaining an optical modulation amplitude of 38% after 1000 cycles.
[0021] The beneficial effects of this invention are:
[0022] 1) This invention uses the sol-gel method to prepare spinel-type "zero-strain" electrochromic thin films. The above method is suitable for synthesis at low temperatures and has the advantages of low energy consumption, no pollution and good reproducibility, which is conducive to large-scale industrial production.
[0023] 2) The present invention uses a blade coating method to prepare a dense and seamless LTO film.
[0024] 3) The spinel-type "zero-strain" electrochromic thin film prepared by this invention has good optical modulation performance, with an optical modulation amplitude of 40% in the spectral range of 400-1100 nm; the film has a rapid color-changing / color-changing response time, with color-changing / color-changing response times of 5-10 s and 8-15 s respectively under an adjustment voltage of -2.5V / +1V; the film has excellent cycling stability, and still maintains 38% optical modulation amplitude after 1000 cycles. Attached Figure Description
[0025] Figure 1 X-ray diffraction patterns of samples prepared in Examples 1, 2, and 3 and Comparative Examples 1 and 2 of the present invention;
[0026] Figure 2 This is a 30,000x SEM image of the LTO thin film prepared in Example 1 of the present invention;
[0027] Figure 3 Optical modulation amplitude curves of LTO thin films prepared in Examples 1, 2, and 3 of the present invention and Comparative Example 1;
[0028] Figure 4 The cyclic voltammetry curves are for the LTO thin films prepared in Examples 1, 2, and 3 of this invention and Comparative Example 1. Detailed implementation method:
[0029] The technical solutions presented in the embodiments of the invention will be clearly explained and fully described below with reference to the accompanying drawings. It is worth emphasizing that the examples described below are merely some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0030] Furthermore, the embodiments and features described herein can be combined with each other without conflict.
[0031] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but this is not intended to limit the scope of the invention.
[0032] Example 1
[0033] 1) Using a dropper, slowly add 3 ml of tetraisopropoxide to a beaker containing 60 ml of deionized water and stir magnetically for 20 min to initiate the hydrolysis reaction. Wash and centrifuge the hydrolysis product twice. Add the centrifuged product to 60 ml of deionized water and disperse using an ultrasonic cell disruptor for 30 min. Stir the disrupted solution magnetically, add 5 ml of hydrogen peroxide to form an orange transparent solution, and then add 0.203 g of lithium hydroxide monohydrate solid. After stirring magnetically for 6 h, a yellow, transparent, and clear precursor solution is obtained.
[0034] 2) First, cut a small piece of tape and stick it to one end of the cleaned and plasma-activated FTO to serve as an electrode. Then, place the FTO with the electrode on a glass substrate and fix it in place. Use a dropper to draw the prepared LTO precursor solution and drop it onto the end near the tape. Slide the coater placed on the substrate to allow the added solution to form a film. The coater sliding speed is 15 mm / s, and the coater specification is 90 μm. Coat 10 layers to obtain a thin film. Then, heat-treat the LTO film at 500℃ for 2 hours. The film prepared in this example is denoted as a. Figure 2 The image obtained by SEM at 30,000x magnification is shown in the image of the LTO thin film.
[0035] 3) To test the optical modulation amplitude of the thin film, the LTO thin film was subjected to coloring and fading tests in a 1 mol / L PC / LiClO4 electrolyte. For the colored state, the LTO thin film was tested after being exposed to -2.5V for 40 seconds; for the fading state, the potential was set to +1V for 20 seconds. The optical modulation amplitude of the LTO coated thin film was obtained. Figure 3 As shown, the optical modulation amplitude of the thin film reaches its maximum when the wavelength is around 860 nm, and the optical modulation amplitude of the LTO thin film is around 60%.
[0036] 4) The current-voltage characteristics of the thin film were tested. The test system was a three-electrode system. The reference electrode was Ag / AgCl, the counter electrode was a platinum electrode, and the chronopotential method was used. The low potential was -2.5V, the high potential was +1V, and the scan rate was 100mv / s.
[0037] Example 2
[0038] 1) Using a dropper, slowly add 3 ml of tetraisopropoxide to a beaker containing 60 ml of deionized water and stir magnetically for 20 min to initiate the hydrolysis reaction. Wash and centrifuge the hydrolysis product twice. Add the centrifuged product to 60 ml of deionized water and disperse using an ultrasonic cell disruptor for 30 min. Stir the disrupted solution magnetically, add 5 ml of hydrogen peroxide to form an orange transparent solution, and then add 0.208 g of lithium hydroxide monohydrate solid. After stirring magnetically for 6 h, a yellow, transparent, and clear precursor solution is obtained.
[0039] 2) First, cut a small piece of tape with scissors and stick it to one end of the cleaned and plasma-activated FTO to serve as an electrode. Then, place the FTO with the electrode on a glass substrate and fix it. Use a dropper to draw the prepared LTO precursor solution and drop it onto one end near the tape. Slide the coater placed on the substrate to make the added solution form a film. The coater sliding speed is 15 mm / s. Select a coater specification of 90 μm and coat 15 layers to obtain a thin film. Then, prepare the LTO thin film under the condition of heat treatment at 400℃ for 2 hours. The thin film prepared in this example is denoted as b.
[0040] 3) Testing the optical modulation amplitude of the thin film. The LTO thin film was subjected to coloring and fading tests in a 1 mol / L PC / LiClO4 electrolyte. For the colored state, the LTO thin film was tested at -2.5V for 40 seconds; for the fading state, the potential was set to +1V for 20 seconds. The optical modulation amplitude of the LTO coated thin film was obtained.
[0041] 4) Testing the voltammetric characteristics of the thin film. The testing system is a three-electrode system, using Ag / AgCl as the reference electrode and a platinum electrode as the counter electrode. The chronopotential method is used, with a low potential of -2.5V and a high potential of +1V, and a scan rate of 100mV / s.
[0042] Example 3
[0043] 1) Using a dropper, slowly add 3 ml of tetraisopropoxide to a beaker containing 60 ml of deionized water and stir magnetically for 20 min to initiate the hydrolysis reaction. Wash and centrifuge the hydrolysis product twice. Add the centrifuged product to 60 ml of deionized water and disperse using an ultrasonic cell disruptor for 30 min. Stir the disrupted solution magnetically, add 5 ml of hydrogen peroxide to form an orange transparent solution, and then add 0.212 g of lithium hydroxide monohydrate solid. After stirring magnetically for 6 h, a yellow, transparent, and clear precursor solution is obtained.
[0044] 2) First, cut a small piece of tape with scissors and stick it to one end of the cleaned and plasma-activated FTO to serve as an electrode. Then, place the FTO with the electrode on a glass substrate and fix it. Use a dropper to draw the prepared LTO precursor solution and drop it onto one end near the tape. Slide the coater placed on the substrate to make the added solution form a film. The coater sliding speed is 10 mm / s. Select a coater specification of 90 μm and coat 5 layers to obtain a thin film. Then, prepare the LTO thin film under the condition of heat treatment at 400℃ for 2 hours. The thin film prepared in this example is denoted as c.
[0045] 3) Testing the optical modulation amplitude of the thin film. The LTO thin film was subjected to coloring and fading tests in a 1 mol / L PC / LiClO4 electrolyte. For the colored state, the LTO thin film was tested at -2.5V for 40 seconds; for the fading state, the potential was set to +1V for 20 seconds. The optical modulation amplitude of the LTO coated thin film was obtained.
[0046] 4) Testing the voltammetric characteristics of the thin film. The testing system is a three-electrode system, using Ag / AgCl as the reference electrode and a platinum electrode as the counter electrode. The chronopotential method is used, with a low potential of -2.5V and a high potential of +1V, and a scan rate of 100mV / s.
[0047] Example 4
[0048] 1) Using a dropper, slowly add 3 ml of tetraisopropoxide to a beaker containing 60 ml of deionized water and stir magnetically for 20 min to initiate the hydrolysis reaction. Wash and centrifuge the hydrolysis product twice. Add the centrifuged product to 60 ml of deionized water and disperse using an ultrasonic cell disruptor for 30 min. Stir the disrupted solution magnetically, add 5 ml of hydrogen peroxide to form an orange transparent solution, and then add 0.217 g of lithium hydroxide monohydrate solid. After stirring magnetically for 6 h, a yellow, transparent, and clear precursor solution is obtained.
[0049] 2) First, cut a small piece of tape with scissors and stick it to one end of the cleaned and plasma-activated FTO to serve as an electrode. Then, place the FTO with the electrode on the glass substrate and fix it. Use a dropper to draw the prepared LTO precursor solution and drop it onto one end near the tape. Slide the coater placed on the substrate to make the added solution form a film. The coater sliding speed is 10 mm / s. Select a coater specification of 90 μm and coat 15 layers to obtain a thin film. Then, prepare the LTO thin film under the condition of heat treatment at 400℃ for 2 hours.
[0050] 3) Testing the optical modulation amplitude of the thin film. The LTO thin film was subjected to coloring and fading tests in a 1 mol / L PC / LiClO4 electrolyte. For the colored state, the LTO thin film was tested at -2.5V for 40 seconds; for the fading state, the potential was set to +1V for 20 seconds. The optical modulation amplitude of the LTO coated thin film was obtained.
[0051] 4) The current-voltage characteristics of the thin film were tested. The test system was a three-electrode system. The reference electrode was Ag / AgCl, the counter electrode was a platinum electrode, and the chronopotential method was used. The low potential was -2.5V, the high potential was +1V, and the scan rate was 100mv / s.
[0052] Comparative Example 1
[0053] This comparative example is basically the same as Example 2. The difference is that the heat treatment temperature of the thin film is 300°C. Figure 1 The X-ray diffraction pattern shown indicates that no obvious LTO diffraction peaks were found in Comparative Example 1. Therefore, it can be preliminarily concluded that a heat treatment temperature of 400-500℃ can yield a pure-phase spinel-type LTO thin film. The thin film prepared in this way is denoted as d.
[0054] Figure 3 The optical modulation amplitude curves are shown for the LTO thin films prepared in Examples 1, 2, and 3 of this invention, as well as Comparative Example 1. Figure 4 The cyclic voltammetry curves of the LTO thin films prepared in Examples 1, 2, and 3 of this invention, and Comparative Example 1, show that the films exhibit a transmittance of 42% in the colored state and 90% in the faded state at a wavelength of 660 nm, with a maximum optical modulation amplitude of 40%. They also demonstrate rapid color-changing / fading response and good cycling stability. During the color-changing / fading process, observations corresponding to lithium insertion and extraction from spinel Li₄Ti₅O₂ can be made. 12 The extracted redox pairs showed symmetrical and reversible redox peak positions in the thin film at all scan rates, indicating that Li+ implantation / extraction of Li4Ti5O... 12 / Li7Ti5O 12 The typical Ti4+ / Ti3+ redox peaks in the structure prove that the film can effectively complete the corresponding redox process, exhibiting a complete and thorough coloring / fading phenomenon.
[0055] Comparative Example 2
[0056] This comparative example is essentially the same as Example 1. Since changing the coating agent specifications can alter the film thickness, a 60 μm coating agent was used in this comparative example, and the heat treatment temperature was maintained at 500°C. Measurements of the optical modulation amplitude of the film in the comparative example revealed a relatively small amplitude, suggesting that a larger film thickness results in a lighter film color, leading to a smaller optical modulation amplitude.
[0057] Comparative Example 3
[0058] This comparative example is basically the same as Example 1. The difference is that the heat treatment temperature of the thin film is changed to 600℃. It was found that the peak current and closed curve area of the LTO thin film changed little, and the positions of the reduction peak at around -0.9V and the oxidation peak at around -1.8V remained basically unchanged. That is, the LTO thin film at the heat treatment temperature of 500℃ has the best CV cycle stability and lithium-ion capacity.
[0059] The above description is merely a preferred embodiment of the present invention and does not limit the implementation method and protection scope of the present invention. Those skilled in the art should realize that any equivalent substitutions and obvious changes made based on the description and illustrations of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a spinel-type lithium titanate electrochromic thin film, characterized in that, Includes the following steps: Step 1: Prepare the precursor solution of lithium titanate (LTO) using the sol-gel method: Ti{OCH(CH3)2}4 was hydrolyzed in deionized water to obtain solid titanium hydroxide. After centrifugation, it was redispersed in deionized water and ultrasonically dispersed. H2O2 solution and solid LiOH were added sequentially under stirring to obtain a lithium titanate precursor solution. The stirring was magnetic stirring for 4-6 hours. H2O2 solution was added dropwise during stirring. When the liquid changed from a turbid state to an orange transparent state, solid LiOH was added to obtain a yellow transparent clear lithium titanate precursor solution. Step 2: Prepare LTO electrochromic thin films using a blade coating method: Cut a small piece of tape and stick it to one end of the treated substrate to serve as an electrode. Place the substrate, which serves as the electrode, on a glass substrate and fix it. Use a dropper to draw up the LTO precursor solution prepared in step one and drop it onto one end near the tape. Quickly slide the coater placed on the substrate to make the added solution form a film. After heat treatment, an LTO thin film is obtained. The substrate is FTO conductive glass; the thickness of the film is related to the specifications of the coater, which is 60-120μm; the coating speed of the coater is 10-15mm / s, and 5-15 layers are coated; the heat treatment temperature is 400-500℃, and the heat treatment time is 3-4h.
2. The method for preparing a spinel-type lithium titanate electrochromic thin film according to claim 1, characterized in that, The molar ratio of Ti{OCH(CH3)2}4 to LiOH mentioned in step one is (0.096-1.8):(0.12-2.0).
3. The method for preparing a spinel-type lithium titanate electrochromic thin film according to claim 1, characterized in that, The centrifugation in step one is performed 2-3 times, with a centrifugation speed range of 500-10000 r / min and an ultrasonic dispersion time of 20-30 min.
4. The method for preparing the spinel-type lithium titanate electrochromic thin film according to claim 1, characterized in that, The substrate processing procedure described in step two is as follows: First, fluorine-doped SnO2 (FTO) conductive glass is immersed in deionized water, and ultrasonic cleaning is performed for 8 minutes with the addition of photoelectric cleaning agent to remove organic stains on the substrate surface; then, the FTO conductive glass is transferred to a clean petri dish, and deionized water is added to cover the surface of the FTO conductive glass, and ultrasonic cleaning is performed again for 8 minutes to remove residual photoelectric cleaning agent; then, the FTO conductive glass is transferred to a clean petri dish, and anhydrous ethanol is added to cover the FTO surface, and ultrasonic cleaning is performed for 8 minutes to obtain cleaned FTO conductive glass; the cleaned FTO conductive glass is dried to remove residual anhydrous ethanol, and then placed in a plasma device for 15 minutes to obtain an FTO substrate with good wettability, which is the processed substrate.
5. A spinel-type lithium titanate (LTO) electrochromic thin film, prepared by the method according to any one of claims 1-4, characterized in that, The thin film has a single-phase spinel crystal structure and exhibits 40% optical modulation amplitude in the spectral range of 400–1100 nm. The thin film has a rapid application / fading response time, with application / fading response times of 5–10 s and 8–15 s respectively under an adjustment voltage of -2.5V / +1V. The thin film also exhibits excellent cycling stability, maintaining 38% optical modulation amplitude after 1000 cycles.
Citation Information
Patent Citations
Preparation method of lithium titanate electrochromic film
CN110627372A
Linear hierarchical structure lithium titanate material, preparation and application thereof
US20200083528A1