A method for preparing a high-performance natural rock asphalt base liquid
By adding paraffin oil, graphene whisker adjusting agent, modified wollastonite agent and silane coupling agent liquid into the natural rock asphalt base liquid, the poor crack resistance and heat and freeze resistance stability in the existing technology are solved. Solve the problem of poor quality and realize the configuration of high-performance asphalt base fluid, which improves the crack resistance, fracture toughness and stability of the product.
Patent Information
- Application Number
- CN202410387365.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-26
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-01
AI Technical Summary
The existing asphalt base liquid preparation method has poor crack resistance and low fracture toughness, making it difficult to achieve coordinated improvements in crack resistance and fracture performance. In addition, the heat resistance and freeze resistance cycle stability is poor, which limits the use efficiency of the product.
Use natural rock asphalt as the base material, add paraffin oil, graphene whisker adjusting agent, modified wollastonite agent, mineral powder and silane coupling agent liquid. Through the silane coupling agent KH560 and water in the silane coupling agent liquid, It is blended with ethanol, graphene whisker regulating agent and modified wollastonite agent to optimize the interface properties of raw materials and enhance the crack resistance, fracture toughness, heat resistance and freeze resistance stability of the product.
It significantly improves the crack resistance and fracture toughness of the product, coordinates and improves performance, optimizes heat resistance and anti-freeze stability, and enhances the overall performance of the product.
Smart Images

Figure BDA0004771184820000121 
Figure BDA0004771184820000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt base liquid configuration, and in particular to a method for configuring a high-performance natural rock asphalt base liquid. Background Art
[0002] Natural asphalt is formed by the long-term compression of the earth's crust and the gradual change of oil in contact with air and water. It exists in natural form and is often mixed with a certain proportion of minerals. Natural asphalt not only has the characteristics of high softening point, high asphaltene content, low temperature sensitivity, excellent high temperature performance and anti-aging performance, but also has the advantages of good ash and asphalt adsorption and strong resistance to water damage. According to the formation environment, it can be divided into natural rock asphalt, natural lake asphalt, natural seabed asphalt, etc.
[0003] The existing asphalt base liquid configuration method is simple, and the resulting product has poor crack resistance. In order to improve the product's crack resistance, the product's fracture toughness is reduced, making it difficult to achieve coordinated improvements in the product's crack resistance and fracture performance. The product's heat and freeze resistance cycle stability is poor, further limiting the product's use efficiency. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a method for preparing a high-performance natural rock asphalt base liquid to solve the problems raised in the above-mentioned background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides a method for preparing a high-performance natural rock asphalt base liquid, comprising the following steps:
[0007] Step 1: Weigh the weight of the raw materials:
[0008] 20-25 parts of natural rock asphalt, 3-6 parts of paraffin oil, 4-7 parts of graphene regulating whisker agent, 2-5 parts of modified wollastonite agent, 5-10 parts of mineral powder, 6-10 parts of silane coupling agent liquid;
[0009] Step 2: melt and stir the natural rock asphalt at 175-185°C for 1-2h for later use;
[0010] Step 3: Stir and mix the silane coupling agent KH560, water and ethanol in a weight ratio of 2:4:1, and then add 2-5% of the total amount of the silane coupling agent KH560 glycolic acid and stir to obtain a silane coupling agent liquid;
[0011] Step 4: adding the graphene regulating whisker agent, modified wollastonite agent and mineral powder to the silane coupling agent liquid and stirring evenly, then filtering and drying, and then stirring and mixing with paraffin oil to be fully mixed and set aside;
[0012] Step 5: Add the product prepared in step 4 to step 2 and stir to mix well to obtain the high-performance natural rock asphalt base liquid of the present invention.
[0013] Preferably, the mineral powder is a mineral powder with a particle size less than 0.1 mm; wherein the mineral powder is one of talc, kaolin and mica.
[0014] Preferably, the preparation method of the graphene regulating whisker agent is:
[0015] S01: Stir the silicon carbide whiskers evenly in a sufficient amount of sodium hydroxide solution, then wash and dry them, and then preheat them at 60-65°C for 5-10 minutes and keep them warm for later use;
[0016] S02: 4-7 parts of reserved silicon carbide whiskers, 2-5 parts of yttrium nitrate solution, 1-3 parts of nano-titanium dioxide and 0.25-0.35 parts of urea are mixed and ultrasonically treated at an ultrasonic power of 350-400 W for 1-2 hours. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a yttrium-doped silicon carbide whisker agent;
[0017] S03: ball-milling the yttrium-doped modified silicon carbide whisker agent and the graphene modifier in a weight ratio of 5:2. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier whisker agent.
[0018] Preferably, the mass fraction of the sodium hydroxide solution is 3-5%; the mass fraction of the yttrium nitrate solution is 4-7%.
[0019] Preferably, the ball milling speed of the ball milling reaction treatment is 1000-1500 r / min, and the ball milling time is 1-2 h.
[0020] Preferably, the preparation method of the graphene modifier is:
[0021] The graphene is first heated to 210-230°C at a rate of 1-3°C / min, kept warm for 2-5 minutes, and then cooled to 50-55°C at a rate of 2-5°C / min for standby use; 4-7 parts of the standby graphene, 1-3 parts of lanthanum chloride solution, 2-4 parts of sodium dodecylbenzene sulfonate, 5-10 parts of deionized water and 1-2 parts of chitosan solution are stirred and mixed to obtain a graphene modifier.
[0022] Preferably, the mass fraction of the lanthanum chloride solution is 2-5%; the mass fraction of the chitosan solution is 4-8%.
[0023] Preferably, the preparation method of the modified wollastonite agent is:
[0024] S101: irradiating wollastonite in a proton irradiation box, and obtaining an irradiated wollastonite agent after the irradiation is completed;
[0025] S102: 2-4 parts of irradiated wollastonite, 1-3 parts of phosphate buffer solution, 2-5 parts of sodium lignin sulfonate and 4-7 parts of deionized water are stirred and mixed, and then washed with water and dried to obtain a modified wollastonite.
[0026] Preferably, the irradiation power of the irradiation treatment is 350-450W, and the irradiation time is 1-2h.
[0027] Preferably, the pH value of the phosphate buffer solution is 5.5.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The method for preparing the natural rock asphalt base liquid of the present invention adopts natural rock asphalt as the base material, and improves it by adding paraffin oil, graphene regulating whisker agent, modified wollastonite agent, mineral powder and silane coupling agent liquid as auxiliary agents; the graphene regulating whisker agent and the modified wollastonite agent are coordinated to enhance the effect together, and are improved by coordinating the silane coupling agent liquid; the silane coupling agent KH560, water and ethanol in the silane coupling agent liquid are blended by hydroxyacetic acid to optimize the interface of the raw materials, and the paraffin oil is coordinated to jointly enhance the performance of the product, improve the crack resistance and fracture toughness performance of the product, improve the coordinated improvement of the two performances, and optimize the heat resistance and antifreeze stability effect of the product; the graphene regulating whisker agent adopts silicon carbide whiskers, which are stirred evenly in a sodium hydroxide solution, then washed with water, dried, and then preheated at 60-65°C for 5-10 minutes to optimize the activity of the whiskers, and then mixed with yttrium nitrate solution, nano titanium dioxide and urea for ultrasonic treatment, so as to The synergistic effect of the co-formulated graphene modifier is enhanced. The graphene modifier is first heated to 210-230°C at a rate of 1-3°C / min, kept warm for 2-5 minutes, and then cooled to 50-55°C at a rate of 2-5°C / min in a segmented manner. Then, it is coordinated with lanthanum chloride solution, sodium dodecylbenzene sulfonate, and chitosan solution. The graphene regulating whisker agent obtained by the coordinated blending of the raw materials is interspersed in the system, and the whisker structure is coordinated with the distribution of flaky graphene to enhance the interfacial effect of the system raw materials and improve the crack resistance and fracture toughness of the product. The wollastonite is irradiated in a proton irradiation box before being irradiated, and then stirred and mixed with phosphate buffer solution, sodium lignin sulfonate and deionized water. The coordinated synergistic effect of the modified wollastonite agent and the graphene regulating whisker agent is enhanced, the crack resistance and fracture toughness of the obtained product are coordinated and improved, and the heat resistance and antifreeze stability of the product are further enhanced. DETAILED DESCRIPTION
[0030] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] A method for preparing a high-performance natural rock asphalt base liquid in this embodiment includes the following steps:
[0032] Step 1: Weigh the weight of the raw materials:
[0033] 20-25 parts of natural rock asphalt, 3-6 parts of paraffin oil, 4-7 parts of graphene regulating whisker agent, 2-5 parts of modified wollastonite agent, 5-10 parts of mineral powder, 6-10 parts of silane coupling agent liquid;
[0034] Step 2: melt and stir the natural rock asphalt at 175-185°C for 1-2h for later use;
[0035] Step 3: Stir and mix the silane coupling agent KH560, water and ethanol in a weight ratio of 2:4:1, and then add 2-5% of the total amount of the silane coupling agent KH560 glycolic acid and stir to obtain a silane coupling agent liquid;
[0036] Step 4: adding the graphene regulating whisker agent, modified wollastonite agent and mineral powder to the silane coupling agent liquid and stirring evenly, then filtering and drying, and then stirring and mixing with paraffin oil to be fully mixed and set aside;
[0037] Step 5: Add the product prepared in step 4 to step 2 and stir to mix well to obtain the high-performance natural rock asphalt base liquid of the present invention.
[0038] The mineral powder in this embodiment is a mineral powder with a particle size less than 0.1 mm; the mineral powder is one of talcum powder, kaolin, and mica.
[0039] The preparation method of the graphene regulating whisker agent of this embodiment is:
[0040] S01: Stir the silicon carbide whiskers evenly in a sufficient amount of sodium hydroxide solution, then wash and dry them, and then preheat them at 60-65°C for 5-10 minutes and keep them warm for later use;
[0041] S02: 4-7 parts of reserved silicon carbide whiskers, 2-5 parts of yttrium nitrate solution, 1-3 parts of nano-titanium dioxide and 0.25-0.35 parts of urea are mixed and ultrasonically treated at an ultrasonic power of 350-400 W for 1-2 hours. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a yttrium-doped silicon carbide whisker agent;
[0042] S03: ball-milling the yttrium-doped modified silicon carbide whisker agent and the graphene modifier in a weight ratio of 5:2. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier whisker agent.
[0043] The mass fraction of the sodium hydroxide solution in this embodiment is 3-5%; the mass fraction of the yttrium nitrate solution is 4-7%.
[0044] The ball milling speed of the ball milling reaction treatment in this embodiment is 1000-1500r / min, and the ball milling is 1-2h.
[0045] The preparation method of the graphene modifier of this embodiment is:
[0046] The graphene is first heated to 210-230°C at a rate of 1-3°C / min, kept warm for 2-5 minutes, and then cooled to 50-55°C at a rate of 2-5°C / min for standby use; 4-7 parts of the standby graphene, 1-3 parts of lanthanum chloride solution, 2-4 parts of sodium dodecylbenzene sulfonate, 5-10 parts of deionized water and 1-2 parts of chitosan solution are stirred and mixed to obtain a graphene modifier.
[0047] The mass fraction of the lanthanum chloride solution in this embodiment is 2-5%; the mass fraction of the chitosan solution is 4-8%.
[0048] The preparation method of the modified wollastonite agent of the present embodiment is:
[0049] S101: irradiating wollastonite in a proton irradiation box, and obtaining an irradiated wollastonite agent after the irradiation is completed;
[0050] S102: 2-4 parts of irradiated wollastonite, 1-3 parts of phosphate buffer solution, 2-5 parts of sodium lignin sulfonate and 4-7 parts of deionized water are stirred and mixed, and then washed with water and dried to obtain a modified wollastonite.
[0051] The irradiation power of the irradiation treatment in this embodiment is 350-450W, and the irradiation time is 1-2h.
[0052] The pH value of the phosphate buffer solution in this example is 5.5.
[0053] Example 1.
[0054] A method for preparing a high-performance natural rock asphalt base liquid in this embodiment includes the following steps:
[0055] Step 1: Weigh the weight of the raw materials:
[0056] 20 parts of natural rock asphalt, 3 parts of paraffin oil, 4 parts of graphene regulating whisker agent, 2 parts of modified wollastonite agent, 5 parts of mineral powder, 6 parts of silane coupling agent liquid;
[0057] Step 2: melt and stir the natural rock asphalt at 175°C for 1 hour for later use;
[0058] Step 3: Stir and mix the silane coupling agent KH560, water and ethanol in a weight ratio of 2:4:1, and then add 2% of the total amount of the silane coupling agent KH560 glycolic acid and stir to obtain a silane coupling agent liquid;
[0059] Step 4: adding the graphene regulating whisker agent, modified wollastonite agent and mineral powder to the silane coupling agent liquid and stirring evenly, then filtering and drying, and then stirring and mixing with paraffin oil to be fully mixed and set aside;
[0060] Step 5: Add the product prepared in step 4 to step 2 and stir to mix well to obtain the high-performance natural rock asphalt base liquid of the present invention.
[0061] The mineral powder in this embodiment is a mineral powder with a particle size less than 0.1 mm; the mineral powder is one of talcum powder, kaolin, and mica.
[0062] The preparation method of the graphene regulating whisker agent of this embodiment is:
[0063] S01: Stir the silicon carbide whiskers evenly in a sufficient amount of sodium hydroxide solution, then wash and dry them, and then preheat them at 60°C for 5-10 minutes and keep them warm for later use;
[0064] S02: 4 parts of reserved silicon carbide whiskers, 2 parts of yttrium nitrate solution, 1 part of nano-titanium dioxide and 0.25 parts of urea are mixed and ultrasonically treated at an ultrasonic power of 350 W for 1 hour. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a yttrium-doped silicon carbide whisker agent;
[0065] S03: ball-milling the yttrium-doped modified silicon carbide whisker agent and the graphene modifier in a weight ratio of 5:2. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier whisker agent.
[0066] The mass fraction of the sodium hydroxide solution in this embodiment is 3%; the mass fraction of the yttrium nitrate solution is 4%.
[0067] The ball milling speed of the ball milling reaction treatment in this embodiment is 1000 r / min, and the ball milling is 1 hour.
[0068] The preparation method of the graphene modifier of this embodiment is:
[0069] The graphene was first heated to 210°C at a rate of 1°C / min, kept warm for 2 minutes, and then cooled to 50°C at a rate of 2°C / min for use; 4 parts of the reserved graphene, 1 part of lanthanum chloride solution, 2 parts of sodium dodecylbenzene sulfonate, 5 parts of deionized water and 1 part of chitosan solution were stirred and mixed to obtain a graphene modifier.
[0070] The mass fraction of the lanthanum chloride solution in this embodiment is 2%; the mass fraction of the chitosan solution is 4%.
[0071] The preparation method of the modified wollastonite agent of the present embodiment is:
[0072] S101: irradiating wollastonite in a proton irradiation box, and obtaining an irradiated wollastonite agent after the irradiation is completed;
[0073] S102: 2 parts of irradiated wollastonite, 1 part of phosphate buffer solution, 2 parts of sodium lignin sulfonate and 4 parts of deionized water are stirred and mixed, and then washed with water and dried to obtain a modified wollastonite.
[0074] The irradiation power of the irradiation treatment in this embodiment is 350W, and the irradiation time is 1 hour.
[0075] The pH value of the phosphate buffer solution in this example is 5.5.
[0076] Example 2.
[0077] A method for preparing a high-performance natural rock asphalt base liquid in this embodiment includes the following steps:
[0078] Step 1: Weigh the weight of the raw materials:
[0079] 25 parts of natural rock asphalt, 6 parts of paraffin oil, 7 parts of graphene regulating whisker agent, 5 parts of modified wollastonite agent, 10 parts of mineral powder, and 10 parts of silane coupling agent liquid;
[0080] Step 2: melt and stir the natural rock asphalt at 185°C for 2 hours for later use;
[0081] Step 3: Stir and mix the silane coupling agent KH560, water and ethanol in a weight ratio of 2:4:1, and then add 5% of the total amount of the silane coupling agent KH560 glycolic acid and stir to obtain a silane coupling agent liquid;
[0082] Step 4: adding the graphene regulating whisker agent, modified wollastonite agent and mineral powder to the silane coupling agent liquid and stirring evenly, then filtering and drying, and then stirring and mixing with paraffin oil to be fully mixed and set aside;
[0083] Step 5: Add the product prepared in step 4 to step 2 and stir to mix well to obtain the high-performance natural rock asphalt base liquid of the present invention.
[0084] The mineral powder in this embodiment is a mineral powder with a particle size less than 0.1 mm; the mineral powder is one of talcum powder, kaolin, and mica.
[0085] The preparation method of the graphene regulating whisker agent of this embodiment is:
[0086] S01: Stir the silicon carbide whiskers evenly in a sufficient amount of sodium hydroxide solution, then wash and dry them, and then preheat them at 65°C for 10 minutes and keep them warm for later use;
[0087] S02: 7 parts of spare silicon carbide whiskers, 5 parts of yttrium nitrate solution, 3 parts of nano-titanium dioxide and 0.35 parts of urea are mixed and ultrasonically treated at an ultrasonic power of 400 W for 2 hours. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a yttrium-doped modified silicon carbide whisker agent;
[0088] S03: ball-milling the yttrium-doped modified silicon carbide whisker agent and the graphene modifier in a weight ratio of 5:2. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier whisker agent.
[0089] The mass fraction of the sodium hydroxide solution in this embodiment is 5%; the mass fraction of the yttrium nitrate solution is 7%.
[0090] The ball milling speed of the ball milling reaction treatment in this embodiment is 1500r / min, and the ball milling is 2h.
[0091] The preparation method of the graphene modifier of this embodiment is:
[0092] The graphene was first heated to 230°C at a rate of 3°C / min, kept warm for 5 minutes, and then cooled to 55°C at a rate of 5°C / min for use; 7 parts of the reserved graphene, 3 parts of lanthanum chloride solution, 4 parts of sodium dodecylbenzene sulfonate, 10 parts of deionized water and 2 parts of chitosan solution were stirred and mixed to obtain a graphene modifier.
[0093] The mass fraction of the lanthanum chloride solution in this embodiment is 5%; the mass fraction of the chitosan solution is 8%.
[0094] The preparation method of the modified wollastonite agent of the present embodiment is:
[0095] S101: irradiating wollastonite in a proton irradiation box, and obtaining an irradiated wollastonite agent after the irradiation is completed;
[0096] S102: 4 parts of irradiated wollastonite, 3 parts of phosphate buffer solution, 5 parts of sodium lignin sulfonate and 7 parts of deionized water are stirred and mixed, and then washed with water and dried to obtain a modified wollastonite.
[0097] The irradiation power of the irradiation treatment in this embodiment is 450W, and the irradiation time is 2h.
[0098] The pH value of the phosphate buffer solution in this example is 5.5.
[0099] Example 3.
[0100] A method for preparing a high-performance natural rock asphalt base liquid in this embodiment includes the following steps:
[0101] Step 1: Weigh the weight of the raw materials:
[0102] 22.5 parts of natural rock asphalt, 4.5 parts of paraffin oil, 5.5 parts of graphene regulating whisker agent, 3.5 parts of modified wollastonite agent, 7.5 parts of mineral powder, 8 parts of silane coupling agent liquid;
[0103] Step 2: melt and stir the natural rock asphalt at 180°C for 1.5h for later use;
[0104] Step 3: Stir and mix the silane coupling agent KH560, water and ethanol in a weight ratio of 2:4:1, and then add 3.5% of the total amount of silane coupling agent KH560 glycolic acid and stir to obtain a silane coupling agent liquid;
[0105] Step 4: adding the graphene regulating whisker agent, modified wollastonite agent and mineral powder to the silane coupling agent liquid and stirring evenly, then filtering and drying, and then stirring and mixing with paraffin oil to be fully mixed and set aside;
[0106] Step 5: Add the product prepared in step 4 to step 2 and stir to mix well to obtain the high-performance natural rock asphalt base liquid of the present invention.
[0107] The mineral powder in this embodiment is a mineral powder with a particle size less than 0.1 mm; the mineral powder is one of talcum powder, kaolin, and mica.
[0108] The preparation method of the graphene regulating whisker agent of this embodiment is:
[0109] S01: Stir the silicon carbide whiskers evenly in a sufficient amount of sodium hydroxide solution, then wash and dry them, and then preheat them at 62°C for 7.5 minutes and keep them warm for later use;
[0110] S02: 5.5 parts of reserved silicon carbide whiskers, 3.5 parts of yttrium nitrate solution, 2 parts of nano-titanium dioxide and 0.30 parts of urea are mixed and ultrasonically treated at an ultrasonic power of 350-400 W for 1-2 hours. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a yttrium-doped silicon carbide whisker agent;
[0111] S03: ball-milling the yttrium-doped modified silicon carbide whisker agent and the graphene modifier in a weight ratio of 5:2. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier whisker agent.
[0112] The mass fraction of the sodium hydroxide solution in this embodiment is 4%; the mass fraction of the yttrium nitrate solution is 5.5%.
[0113] The ball milling speed of the ball milling reaction treatment in this embodiment is 1250 r / min, and the ball milling is 1.5 h.
[0114] The preparation method of the graphene modifier of this embodiment is:
[0115] The graphene was first heated to 220°C at a rate of 2°C / min, kept warm for 3.5 minutes, and then cooled to 52°C at a rate of 3.5°C / min for use; 5.5 parts of the reserved graphene, 2 parts of lanthanum chloride solution, 3 parts of sodium dodecylbenzene sulfonate, 7.5 parts of deionized water and 1.5 parts of chitosan solution were stirred and mixed to obtain a graphene modifier.
[0116] The mass fraction of the lanthanum chloride solution in this embodiment is 3.5%; the mass fraction of the chitosan solution is 6%.
[0117] The preparation method of the modified wollastonite agent of the present embodiment is:
[0118] S101: irradiating wollastonite in a proton irradiation box, and obtaining an irradiated wollastonite agent after the irradiation is completed;
[0119] S102: 3 parts of irradiated wollastonite, 2 parts of phosphate buffer solution, 3.5 parts of sodium lignin sulfonate and 5.5 parts of deionized water are stirred and mixed, and then washed with water and dried to obtain a modified wollastonite.
[0120] The irradiation power of the irradiation treatment in this embodiment is 380W, and the irradiation time is 1.5h.
[0121] The pH value of the phosphate buffer solution in this example is 5.5.
[0122] Example 4.
[0123] A method for preparing a high-performance natural rock asphalt base liquid in this embodiment includes the following steps:
[0124] Step 1: Weigh the weight of the raw materials:
[0125] 22 parts of natural rock asphalt, 4 parts of paraffin oil, 5 parts of graphene regulating whisker agent, 3 parts of modified wollastonite agent, 6 parts of mineral powder, 7 parts of silane coupling agent liquid;
[0126] Step 2: melt and stir the natural rock asphalt at 176°C for 1.2 hours for later use;
[0127] Step 3: Stir and mix the silane coupling agent KH560, water and ethanol in a weight ratio of 2:4:1, and then add 3% of the total amount of the silane coupling agent KH560 glycolic acid and stir to obtain a silane coupling agent liquid;
[0128] Step 4: adding the graphene regulating whisker agent, modified wollastonite agent and mineral powder to the silane coupling agent liquid and stirring evenly, then filtering and drying, and then stirring and mixing with paraffin oil to be fully mixed and set aside;
[0129] Step 5: Add the product prepared in step 4 to step 2 and stir to mix well to obtain the high-performance natural rock asphalt base liquid of the present invention.
[0130] The mineral powder in this embodiment is a mineral powder with a particle size less than 0.1 mm; the mineral powder is one of talcum powder, kaolin, and mica.
[0131] The preparation method of the graphene regulating whisker agent of this embodiment is:
[0132] S01: Stir the silicon carbide whiskers evenly in a sufficient amount of sodium hydroxide solution, then wash and dry them, and then preheat them at 62°C for 6 minutes and keep them warm for later use;
[0133] S02: 5 parts of spare silicon carbide whiskers, 3 parts of yttrium nitrate solution, 2 parts of nano-titanium dioxide and 0.26 parts of urea are mixed and ultrasonically treated at an ultrasonic power of 360 W for 1.2 h. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a yttrium-doped modified silicon carbide whisker agent;
[0134] S03: ball-milling the yttrium-doped modified silicon carbide whisker agent and the graphene modifier in a weight ratio of 5:2. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier whisker agent.
[0135] The mass fraction of the sodium hydroxide solution in this embodiment is 4%; the mass fraction of the yttrium nitrate solution is 5%.
[0136] The ball milling speed of the ball milling reaction treatment in this embodiment is 1200 r / min, and the ball milling is 1.2 h.
[0137] The preparation method of the graphene modifier of this embodiment is:
[0138] The graphene was first heated to 212°C at a rate of 2°C / min, kept warm for 3 minutes, and then cooled to 52°C at a rate of 3°C / min for use; 5 parts of the reserved graphene, 2 parts of lanthanum chloride solution, 3 parts of sodium dodecylbenzene sulfonate, 6 parts of deionized water and 1.2 parts of chitosan solution were stirred and mixed to obtain a graphene modifier.
[0139] The mass fraction of the lanthanum chloride solution in this embodiment is 3%; the mass fraction of the chitosan solution is 5%.
[0140] The preparation method of the modified wollastonite agent of the present embodiment is:
[0141] S101: irradiating wollastonite in a proton irradiation box, and obtaining an irradiated wollastonite agent after the irradiation is completed;
[0142] S102: 3 parts of irradiated wollastonite, 2 parts of phosphate buffer solution, 3 parts of sodium lignin sulfonate and 5 parts of deionized water are stirred and mixed, and then washed with water and dried to obtain a modified wollastonite.
[0143] The irradiation power of the irradiation treatment in this embodiment is 360W, and the irradiation time is 1.8h.
[0144] The pH value of the phosphate buffer solution in this example is 5.5.
[0145] Comparative Example 1.
[0146] The difference from Example 3 is that no graphene regulating whisker agent is added.
[0147] Comparative Example 2.
[0148] The difference from Example 3 is that SO2 treatment is not used in the preparation of the graphene regulating whisker agent.
[0149] Comparative Example 3.
[0150] The difference from Example 3 is that no graphene modifier is used in the preparation of the graphene regulating whisker agent.
[0151] Comparative Example 4.
[0152] The difference from Example 3 is that lanthanum chloride solution, 3 parts of sodium dodecylbenzene sulfonate, 6 parts of deionized water and 1.2 parts of chitosan solution are not used in the preparation of the graphene modifier.
[0153] Comparative Example 5.
[0154] The difference from Example 3 is that the graphene modifier preparation did not adopt the method of first heating to 212° C. at a rate of 2° C. / min, keeping warm for 3 minutes, and then cooling to 52° C. at a rate of 3° C. / min for standby treatment.
[0155] Comparative Example 6.
[0156] The difference from Example 3 is that no modified wollastonite agent was used for treatment.
[0157] Comparative Example 7.
[0158] The difference from Example 3 is that the modified wollastonite agent uses wollastonite raw material.
[0159] Comparative Example 8.
[0160] The difference from Example 3 is that no silane coupling agent liquid treatment is used.
[0161] The products of Examples 1-4 and Comparative Examples 1-8 were subjected to performance tests, and the products were placed at 65°C for 12 hours, and then at -5°C for 12 hours to test the heat resistance and freeze resistance stability;
[0162]
[0163]
[0164] It can be seen from Comparative Examples 1-8 and Examples 1-4 that the splitting strength and elongation at break of the product of the present invention can be improved in a coordinated manner, and the product has significant performance stability under heat and freeze conditions;
[0165] Without adding graphene whisker regulating agent, without using modified wollastonite agent treatment and without using silane coupling agent liquid treatment, the performance of the product showed a significant trend of deterioration;
[0166] The use of graphene whisker regulating agent, modified wollastonite agent treatment and silane coupling agent liquid treatment has a synergistic effect, and the performance of the products has a coordinated enhancement effect;
[0167] The graphene regulating whisker agent was not treated with S02, the graphene regulating whisker agent was not treated with graphene modifier, the graphene modifier was not treated with lanthanum chloride solution, 3 parts of sodium dodecylbenzene sulfonate, 6 parts of deionized water and 1.2 parts of chitosan solution, and the graphene modifier was not heated to 212°C at a rate of 2°C / min, kept warm for 3 minutes, and then cooled to 52°C at a rate of 3°C / min for standby treatment. The performance of the products all tended to deteriorate. The graphene regulating whisker agent prepared by the specific method of the present invention had the most significant performance effect. At the same time, the modified wollastonite agent used wollastonite raw material, and the performance of the product also showed a trend of deterioration. Only the modified wollastonite agent prepared by the method of the present invention had the most significant performance effect.
[0168] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0169] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a high-performance natural rock asphalt base liquid, characterized in that: The following steps are involved: Step 1: Weigh the weight of the raw materials: 20-25 parts of natural rock asphalt, 3-6 parts of paraffin oil, 4-7 parts of graphene regulating whisker agent, 2-5 parts of modified wollastonite agent, 5-10 parts of mineral powder, 6-10 parts of silane coupling agent liquid; Step 2: melt and stir the natural rock asphalt at 175-185°C for 1-2h for later use; Step 3: Stir and mix the silane coupling agent KH560, water and ethanol in a weight ratio of 2:4:1, and then add 2-5% of the total amount of the silane coupling agent KH560 glycolic acid and stir to obtain a silane coupling agent liquid; Step 4: adding the graphene regulating whisker agent, modified wollastonite agent and mineral powder to the silane coupling agent liquid and stirring evenly, then filtering and drying, and then stirring and mixing with paraffin oil to be fully mixed and set aside; Step 5: adding the product prepared in step 4 to step 2 and stirring to obtain the high-performance natural rock asphalt base liquid; The preparation method of the graphene regulating whisker agent is: S01: Stir the silicon carbide whiskers evenly in a sufficient amount of sodium hydroxide solution, then wash and dry them, and then preheat them at 60-65°C for 5-10 minutes and keep them warm for later use; S02: 4-7 parts of reserved silicon carbide whiskers, 2-5 parts of yttrium nitrate solution, 1-3 parts of nano-titanium dioxide and 0.25-0.35 parts of urea are mixed and ultrasonically treated at an ultrasonic power of 350-400 W for 1-2 hours. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a yttrium-doped silicon carbide whisker agent; S03: ball milling the yttrium-doped modified silicon carbide whisker agent and the graphene modifier according to a weight ratio of 5:2, and after the ball milling is completed, washing and drying are performed to obtain a graphene modifier whisker agent; The preparation method of the graphene modifier is: The graphene is first heated to 210-230° C. at a rate of 1-3° C. / min, kept warm for 2-5 minutes, and then cooled to 50-55° C. at a rate of 2-5° C. / min for standby use; 4-7 parts of the standby graphene, 1-3 parts of lanthanum chloride solution, 2-4 parts of sodium dodecylbenzene sulfonate, 5-10 parts of deionized water and 1-2 parts of chitosan solution are stirred and mixed to obtain a graphene modifier; The preparation method of the modified wollastonite agent is: S101: irradiating wollastonite in a proton irradiation box, and obtaining an irradiated wollastonite agent after the irradiation is completed; S102: 2-4 parts of irradiated wollastonite, 1-3 parts of phosphate buffer solution, 2-5 parts of sodium lignin sulfonate and 4-7 parts of deionized water are stirred and mixed, and then washed with water and dried to obtain a modified wollastonite.
2. A method for preparing a high-performance natural rock asphalt base liquid according to claim 1, characterized in that: The mineral powder is a mineral powder with a particle size less than 0.1 mm; the mineral powder is one of talcum powder, kaolin and mica.
3. A method for preparing a high-performance natural rock asphalt base liquid according to claim 1, characterized in that: The mass fraction of the sodium hydroxide solution is 3-5%; the mass fraction of the yttrium nitrate solution is 4-7%.
4. A method for preparing a high-performance natural rock asphalt base liquid according to claim 1, characterized in that: The ball milling speed of the ball milling reaction treatment is 1000-1500r / min, and the ball milling is 1-2h.
5. A method for preparing a high-performance natural rock asphalt base liquid according to claim 1, characterized in that: The mass fraction of the lanthanum chloride solution is 2-5%; the mass fraction of the chitosan solution is 4-8%.
6. A method for preparing a high-performance natural rock asphalt base liquid according to claim 1, characterized in that: The irradiation power of the irradiation treatment is 350-450W, and the irradiation time is 1-2h.
7. A method for preparing a high-performance natural rock asphalt base liquid according to claim 1, characterized in that: The pH value of the phosphate buffer solution is 5.5.
Citation Information
Patent Citations
Combined modified-asphalt root penetration resistance waterproof roll and preparation method thereof
CN103174265A
High-softening point modified asphalt and preparation method thereof
CN107383905A
Graphene composite rock asphalt anti-rutting modifier and preparation method thereof
CN109575618A
Compound dual-modified asphalt mixture additive and preparation method thereof
CN113736271A
Release agent for integrated die casting of aluminum alloy automobile
CN117620076A