A method for producing kaolin using aluminum ash
Through ultrafine grinding hydrolysis, catalytic deamide, permanent magnet decomposition and liquid-solid separation, aluminum ash slag is converted into kaolin, solving the problem of harmful components in aluminum ash, and realizing resource recycling and harmlessization of aluminum ash Disposal has promoted the green development of the aluminum industry.
Patent Information
- Application Number
- CN202410355680.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-03-27
AI Technical Summary
The fluorine and chlorine content in the aluminum ash produced during aluminum processing exceeds the standard, resulting in environmental pollution and human health hazards. The existing technology is difficult to effectively deal with and utilize, so it is necessary to explore methods of harmless and resource-based utilization.
Using ultrafine grinding hydrolysis catalytic deamide, permanent magnet decomposition, liquid-solid separation and drying, aluminum ash slag is converted into kaolin, and harmful components are removed through water grinding reactors and permanent magnet decompressors to realize the resources of aluminum ash Recycling and harmless disposal.
Effectively remove harmful components in aluminum ash, produce kaolin products with high alumina content, promote the green and healthy development of the aluminum industry, and realize the resource recycling and reuse of aluminum ash.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal smelting, in particular to a method for producing kaolin using aluminum ash slag. Background Art
[0002] According to the National List of Hazardous Wastes published in 2020, aluminum ash produced during aluminum processing is listed as hazardous waste of category HW48 and code 321~(024~026)~48 in non-ferrous metal smelting waste. The fluorine and chlorine content in the aluminum ash is seriously exceeded, and it is easy to migrate into the natural environment under the influence of rain, sun and wind, causing environmental pollution and harm to human health.
[0003] Chloride salts mostly exist in the form of NaCl and KCl, which can easily cause salinization when lost into the soil, affecting plant growth; fluoride migrates into groundwater. When its mass concentration exceeds the national standard for drinking water fluoride concentration (1.0 mg / L), animal bones will become hard and brittle, and people will suffer from fluorosis and fluorosis of the bones. In severe cases, people may suffer from disabling fluorosis. Once excessive intake (5-10 mg / L) will immediately cause gastrointestinal bleeding or death; and Al4C3 and AIN in aluminum ash are easily decomposed in water to produce flammable gas (CH4) and irritating gas (NH3), which is very dangerous.
[0004] With the development of a resource-saving and environmentally friendly society, the requirements for environmental protection control are gradually increasing. The recycling and treatment of hazardous waste aluminum ash is imminent, and it is urgent to explore feasible and easy-to-implement industrial harmless and resource utilization technologies. To this end, it is necessary to design a method for producing kaolin from aluminum ash slag to solve the above problems. Summary of the invention
[0005] In order to overcome the above-mentioned shortcomings, the present invention provides a technical solution that can solve the above-mentioned problems.
[0006] A method for producing kaolin from aluminum ash slag comprises the following steps:
[0007] Step S1, ultrafine grinding hydrolysis catalytic deamination: putting the secondary aluminum ash into a water mill reactor, adding water into the water mill reactor for water grinding, and then introducing a trace amount of catalyst aid according to proportion, and using the water mill reactor to perform hydrolysis catalytic deamination reaction;
[0008] Step S2, permanent magnetic impurity removal: the material after the deamination reaction is completed is transported to the permanent magnetic impurity remover through the auger in the water mill reactor, and water is added to the material again, and the permanent magnetic impurity remover is used to transport it slowly and evenly to remove iron oxide, manganese oxide, chromium oxide and oxides of dyeing metals in the material;
[0009] Step S3, liquid-solid separation: the material after deammoniation and permanent magnetic impurity removal is input into a liquid-solid separator for liquid-solid separation, and the residual moisture content of the material after liquid-solid separation is 10-40%;
[0010] Step S4, drying: the material after deammoniation, permanent magnetic impurity removal, and liquid-solid separation is sent to a drying kiln for drying. After drying, the moisture content of the material is less than 2%, and then it is bagged and packaged to obtain a kaolin product.
[0011] Further: in step S1, a catalyst aid is added in a water mill reactor at a ratio of 0.4 to 3% for hydrolysis.
[0012] Further: In step S1, the water mill reactor grinds the material to a particle size of 200-400 meshes.
[0013] Further: in step S1, water is added to the water mill reactor at a liquid-to-solid ratio of 3:1 for water milling; in step S2, water is added to the material again at a liquid-to-solid ratio of 3:1.
[0014] Further: In step S1, the aluminum hydroxide on the surface of the aluminum ash material is continuously destroyed by using a water mill reactor, so that the material can expose a new reaction surface for full deammoniation.
[0015] Further: in step S2, after permanent magnetic impurity removal, the coloring metal oxides of the material are removed to 75% to 89.6%.
[0016] Optionally: In step S3, the liquid-solid separator is a high-speed centrifugal separator, and the liquid-solid separator separates water from the material under the centrifugal force of high-speed centrifugal rotation. The remaining water content of the material after liquid-solid separation is 10-30%.
[0017] Optionally: In step S3, the liquid-solid separator is a filter press, which discharges water from the material through pressure, and the remaining moisture content of the material after liquid-solid separation is 15-40%.
[0018] Furthermore: after liquid-solid separation in step S3, the removal rate of potassium ions, sodium ions and chloride ions in the material is more than 92%, reaching the quality standard of kaolin.
[0019] Furthermore: in the kaolin product produced in step S4, the alumina content of the kaolin product is 50-85%.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. Use hazardous waste aluminum ash to produce kaolin products with an aluminum oxide content of 50-85%;
[0022] 2. Develop a complete aluminum ash treatment system that can effectively treat aluminum ash slag, which is conducive to improving the efficiency of industrialization and resource conversion of aluminum ash treatment, so that a large amount of aluminum ash generated in the aluminum metallurgical process can be recycled and reused, and promote the green and healthy development of the aluminum industry.
[0023] The present invention uses different leaching media to treat secondary aluminum ash, so that aluminum nitride can be efficiently hydrolyzed, soluble fluoride and chloride can be leached, and toxic components such as nitrogen, fluorine and chlorine can be efficiently removed to achieve harmless disposal; the present invention uses secondary aluminum ash to produce kaolin products such as industrial kaolin for ceramics.
[0024] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the specific implementation of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] A method for producing kaolin from aluminum ash slag comprises the following steps:
[0027] Step S1, ultrafine grinding hydrolysis catalytic deamination: putting the secondary aluminum ash into a water mill reactor, adding water into the water mill reactor for water grinding, and then introducing a trace amount of catalyst aid according to proportion, and using the water mill reactor to perform hydrolysis catalytic deamination reaction;
[0028] Step S2, permanent magnetic impurity removal: the material after the deamination reaction is completed is transported to the permanent magnetic impurity remover through the auger in the water mill reactor, and water is added to the material again, and the permanent magnetic impurity remover is used to transport it slowly and evenly to remove iron oxide, manganese oxide, chromium oxide and oxides of dyeing metals in the material;
[0029] Step S3, liquid-solid separation: the material after deammoniation and permanent magnetic impurity removal is input into a liquid-solid separator for liquid-solid separation, and the residual moisture content of the material after liquid-solid separation is 10-40%;
[0030] Step S4, drying: the material after deammoniation, permanent magnetic impurity removal, and liquid-solid separation is sent to a drying kiln for drying. After drying, the moisture content of the material is less than 2%, and then it is bagged and packaged to obtain a kaolin product.
[0031] Further: in step S1, a catalyst aid is added in a water mill reactor at a ratio of 0.4 to 3% for hydrolysis.
[0032] Further: In step S1, the water mill reactor grinds the material to a particle size of 200-400 meshes.
[0033] Further: in step S1, water is added to the water mill reactor at a liquid-to-solid ratio of 3:1 for water milling; in step S2, water is added to the material again at a liquid-to-solid ratio of 3:1.
[0034] Further: In step S1, the aluminum hydroxide on the surface of the aluminum ash material is continuously destroyed by using a water mill reactor, so that the material can expose a new reaction surface for full deammoniation.
[0035] Further: in step S2, after permanent magnetic impurity removal, the coloring metal oxides of the material are removed to 75% to 89.6%.
[0036] Optionally: In step S3, the liquid-solid separator is a high-speed centrifugal separator, and the liquid-solid separator separates water from the material under the centrifugal force of high-speed centrifugal rotation. The remaining water content of the material after liquid-solid separation is 10-30%.
[0037] Optionally: In step S3, the liquid-solid separator is a filter press, which discharges water from the material through pressure, and the remaining moisture content of the material after liquid-solid separation is 15-40%.
[0038] Furthermore: after liquid-solid separation in step S3, the removal rate of potassium ions, sodium ions and chloride ions in the material is more than 92%, reaching the quality standard of kaolin.
[0039] Furthermore: in the kaolin product produced in step S4, the alumina content of the kaolin product is 50-85%.
[0040] The following is a practical implementation case, including the following steps:
[0041] Step S1, ultrafine grinding hydrolysis catalytic deamination: secondary aluminum ash is placed in a water mill reactor, water is added to the water mill reactor at a liquid-solid ratio of 3:1 for water milling, and then a trace amount of catalyst aid is introduced at a ratio of 1.5%, and a hydrolysis catalytic deamination reaction is performed using a water mill reactor; water-insoluble aluminum hydroxide will be generated during the hydrolysis deamination reaction of the aluminum ash, and the aluminum hydroxide will be wrapped on the surface of the aluminum ash particles to form a blocking layer, resulting in the reaction being cut off, so that the hydrolysis deamination reaction is incomplete. The present invention is characterized in that the barrier layer can be continuously destroyed by continuous water milling in the water mill reactor to allow the aluminum ash particles to continuously expose new reaction surfaces, and the water milling can grind the particle size of the material to 200 meshes, and the ultrafine particle size can increase the surface area of the material for the deamination reaction, thereby achieving full deamination of the material;
[0042] Step S2, permanent magnetic impurity removal: the material after the deamination reaction is completed is transported to the permanent magnetic impurity remover through the auger in the water mill reactor, water is added to the material again at a liquid-to-solid ratio of 3:1, and the material is transported slowly and evenly by the permanent magnetic impurity remover to remove iron oxide, manganese oxide, chromium oxide and dyeing metal oxides in the material; after the permanent magnetic impurity removal, the dyeing metal oxides of the material are removed by 87.6%, thereby improving the whiteness of the material;
[0043] Step S3, liquid-solid separation: the material after deammoniation and permanent magnetic impurity removal is input into a liquid-solid separator for liquid-solid separation, and the residual moisture content of the material after liquid-solid separation is 20%; there are two types of liquid-solid separators, one is a high-speed centrifugal separator, which separates water from the material under the centrifugal force of high-speed centrifugal rotation; the other is a filter press, which discharges water from the material under pressure; after liquid-solid separation, the removal rate of potassium ions, sodium ions and chloride ions in the material is 98%, reaching the quality standard of kaolin;
[0044] Step S4, drying: the material after deammoniation, permanent magnetic impurity removal, and liquid-solid separation is sent to a drying kiln for drying. The moisture content of the material after drying is 1.5%, and then it is bagged and packaged to obtain a kaolin product; the alumina content of the kaolin product is 65%, which can be used as kaolin products such as industrial kaolin for ceramics.
[0045] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A method for producing kaolin using aluminum ash slag, characterized in that: The steps include: Step S1, ultrafine grinding hydrolysis catalytic deamination: putting the secondary aluminum ash into a water mill reactor, adding water into the water mill reactor for water grinding, and then introducing a trace amount of catalyst aid according to proportion, using the water mill reactor to carry out hydrolysis catalytic deamination reaction, and using the water mill reactor to continuously destroy the aluminum hydroxide on the surface of the aluminum ash material, so that the material exposes a new reaction surface for sufficient deamination; Step S2, permanent magnetic impurity removal: the material after the deamination reaction is completed is transported to the permanent magnetic impurity remover through the auger in the water mill reactor, and water is added to the material again, and the permanent magnetic impurity remover is used to transport it slowly and evenly to remove iron oxide, manganese oxide, chromium oxide and oxides of dyeing metals in the material; Step S3, liquid-solid separation: the material after deammoniation and permanent magnetic impurity removal is input into a liquid-solid separator for liquid-solid separation, and the residual moisture content of the material after liquid-solid separation is 10-40%; Step S4, drying: the material after deammoniation, permanent magnetic impurity removal, and liquid-solid separation is sent to a drying kiln for drying. After drying, the moisture content of the material is less than 2%, and then the material is bagged and packaged to obtain a kaolin product.
2. The method for producing kaolin from aluminum ash according to claim 1, characterized in that: In step S1, a catalyst aid is added in a water mill reactor at a ratio of 0.4-3% to perform hydrolysis.
3. The method for producing kaolin from aluminum ash according to claim 1, characterized in that: In step S1, the water mill reactor grinds the material to a particle size of 200-400 meshes.
4. The method for producing kaolin from aluminum ash according to any one of claims 1 to 3, characterized in that: In step S1, water is added to the water mill reactor at a liquid-to-solid ratio of 3:1 for water milling; in step S2, water is added to the material again at a liquid-to-solid ratio of 3:
1.
5. The method for producing kaolin from aluminum ash according to claim 1, characterized in that: In step S2, after permanent magnetic impurity removal, the coloring metal oxides of the material are removed to 75% to 89.6%.
6. The method for producing kaolin from aluminum ash according to claim 1, characterized in that: In step S3, the liquid-solid separator is a high-speed centrifugal separator, which separates water from the material under the centrifugal force of high-speed centrifugal rotation. The remaining water content of the material after liquid-solid separation is 10-30%.
7. The method for producing kaolin from aluminum ash according to claim 1, characterized in that: In step S3, the liquid-solid separator is a filter press, which discharges water from the material under pressure, and the remaining water content of the material after liquid-solid separation is 15-40%.
8. The method for producing kaolin from aluminum ash slag according to claim 1, characterized in that: After liquid-solid separation in step S3, the removal rate of potassium ions, sodium ions and chloride ions in the material is more than 92%, reaching the quality standard of kaolin.
9. The method for producing kaolin from aluminum ash according to claim 1, characterized in that: In the kaolin product produced in step S4, the aluminum oxide content of the kaolin product is 50-85%.
Citation Information
Cited By
Method for synergistically extracting salt from waste incineration fly ash and aluminum ash residues and increasing salt value of waste incineration fly ash and aluminum ash residues
CN121624208A