A flotation process for spodumene mineral
By using highly active OH- modifiers and strong oxidants to dissociate the minerals in the spodumene mineral flotation process, combined with modification treatment using anionic dispersants and metal ion activators, the problem of low separation efficiency in spodumene mineral flotation at low temperatures was solved, achieving efficient and low-energy spodumene mineral separation and improving lithium recovery rate and separation selectivity.
Patent Information
- Application Number
- CN202410568650.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-09
AI Technical Summary
Existing spodumene mineral flotation separation technology has low lithium recovery rate and poor separation selectivity at low temperatures. It is also difficult to separate lithium efficiently in high and low temperature environments, resulting in serious waste of lithium resources. In addition, the existing technology has high energy consumption and does not meet the needs of low-carbon and green development.
Highly active OH- modifiers and strong oxidants are used to dissociate minerals during grinding. Combined with anionic dispersants, metal ion activators and spodumene mineral collectors, the flotation process is modified and mineralized. This includes the combined use of anionic and cationic active components and emulsifiers to optimize the differences in mineral surface properties and improve the efficiency of low-temperature flotation.
The technology significantly improves the recovery rate and sorting selectivity of spodumene minerals under low-temperature conditions, increases the recovery rate and grade of spodumene concentrate, reduces energy consumption and reagent costs, and meets the requirements of low-carbon and green technology.
Abstract
Description
Technical Field
[0001] This invention relates to the field of mineral sorting and processing technology, specifically to a flotation process for spodumene mineral. Background Technology
[0002] Spodumene mineral is one of the important raw materials for lithium metal materials. Currently, mineral separation and processing mainly include flotation, gravity separation, magnetic separation, heavy media separation, hand separation, and combined processes. However, for fine-grained spodumene minerals, flotation separation remains the most effective and widely studied method. The essence of mineral flotation separation is to utilize the differences in the physicochemical properties of mineral surfaces. Various surfactants are used to selectively regulate and mineralize the mineral surface, followed by separation using aerated flotation to obtain different mineral products. However, since the target mineral and gangue minerals in spodumene ore are mostly in the form of silicate or aluminosilicate minerals, the surface physicochemical properties of many types of minerals are similar. Furthermore, during the grinding and flotation process, they are easily affected by factors such as the characteristics of the slurry medium and the abrasive effects of grinding and dissociation, making the floatability of different minerals in the separation system even more similar and difficult to selectively separate. Therefore, the selective separation of the target mineral is one of the current challenges in spodumene separation technology. Secondly, many pegmatite-type lithium deposits both domestically and internationally are located in fragile environments characterized by high altitude, low temperatures, and water scarcity. These areas are characterized by consistently low temperatures, low oxygen levels, and drought, resulting in relatively harsh production conditions. This places high demands on the technology for separating and classifying spodumene minerals. However, existing flotation separation technologies rely heavily on temperature-sensitive reagents, leading to poor lithium recovery efficiency at low temperatures and significant resource waste. To achieve better lithium recovery rates, heated flotation of the slurry is necessary. However, heated flotation involves high energy consumption and reagent costs, which is inconsistent with the requirements of low-carbon and green technology development. Therefore, finding a flotation process that can achieve high efficiency under both low and normal temperature conditions is one of the most challenging problems that urgently needs to be overcome in the separation and recovery of spodumene minerals. Summary of the Invention
[0003] Therefore, the technical problem to be solved by the present invention is to overcome the defects of existing spodumene mineral flotation separation technology in terms of low lithium recovery rate and poor separation selectivity at low temperature, thereby providing a spodumene mineral flotation process to solve the above problems.
[0004] To achieve the above objectives, the present invention provides the following technical solution:
[0005] A flotation process for spodumene mineral, comprising:
[0006] The spodumene ore to be sorted is crushed to obtain crushed mineral materials;
[0007] Water is added to crushed mineral materials and the mixture is ground to dissociate the minerals. A grinding modifier is added during the grinding process to obtain a grinding slurry. The grinding modifier includes highly active OH groups. - Modifiers and strong oxidizing agents;
[0008] The grinding slurry is conditioned, and then an anionic dispersant is added sequentially for modification, followed by the addition of a metal ion activator for ion activation. Finally, a spodumene mineral collector is added for mineralization, and the spodumene concentrate and flotation tailings are obtained by flotation separation.
[0009] The spodumene mineral collector comprises anionic collecting active components, cationic collecting active components, and an emulsifier; the anionic collecting active components are at least one of aminocarboxylate, polyoxyethylene sulfate, alkyl sulfonate, and succinate; the cationic collecting active components are halogenated modified organic amine salts and / or halogenated pyridine organic compounds.
[0010] Preferably, the anion-trapping active component is at least one selected from α-amino acid, N,N-dihydroxyethylglycine, benzyloxycarbonyl amino acid, 1-benzyl D-glutamate, N-hydroxyethyllinoleic acid amide, sodium alkylphenol polyoxyethylene ether sulfate, sodium lauryl polyoxyethylene ether sulfate, sodium α-alkenyl sulfonate, sodium lauryl sulfoacetate, disodium lauryl polyoxyethylene ether sulfosuccinate, and sodium dioctyl succinate sulfonate.
[0011] And / or, the cation-trapping active component is at least one of dodecylammonium bromide, benzalkonium bromide, hexadecyltrimethylammonium chloride, hexadecylpyridine chloride, and hexadecylpyridine bromide;
[0012] And / or, the emulsifier is a neutral oil or / and ester organic compound.
[0013] Preferably, the emulsifier is at least one of kerosene, diesel oil, propylene glycol monostearate, propylene glycol alginate, ethylene glycol monostearate, glyceryl monostearate, and sorbitol fatty acid ester.
[0014] Preferably, the mass ratio of the anion-trapping active component, the cationic-trapping active component, and the emulsifier is 1:(0.2-0.05):(0.02-0.1);
[0015] And / or, the functional group -CH2- that affects the organic molecular chain length in the cation-collecting active component differs from that in the anion-collecting active component by 2-6 positions. (Studies have shown that dodecylamine and oleic acid (octadecyl carboxylic acid) can form a complex organic component on the mineral surface, which is beneficial for flotation separation. Therefore, based on practical experience, when cation and anion combinations are used for synergistic effects, a carbon chain difference of 2-6 -CH2- positions has a certain advantage.)
[0016] Preferably, the maximum particle size of the crushed mineral material is 1-12 mm;
[0017] And / or, the content of minerals with a fineness of -0.074 mm (maximum particle size of 0.074 mm) after grinding is 50-95%;
[0018] And / or, the highly active OH - The modifier is at least one of sodium hydroxide, potassium hydroxide, ammonia, or organic amines;
[0019] And / or, the strong oxidizing agent is at least one of persulfate, permanganate, and perchlorate; preferably, the persulfate is at least one of potassium persulfate, potassium peroxymonosulfate, sodium persulfate, and ammonium persulfate; the permanganate is at least one of potassium permanganate, sodium permanganate, and ammonium permanganate; and the perchlorate is at least one of sodium perchlorate, potassium perchlorate, magnesium perchlorate, and manganese perchlorate.
[0020] Preferably, based on 1 ton of dry spodumene ore to be separated, the amount of grinding modifier used is 100-2500 g, wherein the highly active OH group is... - The dosage of the modifier is 100-2000g, and the dosage of the strong oxidant is 40-500g;
[0021] And / or, the mass concentration of the grinding slurry is 50-85%.
[0022] Preferably, the mass concentration of the slurry after the slurry conditioning treatment is 25-50%;
[0023] And / or, the anionic dispersant is at least one of carbonate, bicarbonate, organic carboxylate, and lignin sulfonate, preferably at least one of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium lignin sulfonate, magnesium lignin sulfonate, ammonium lignin sulfonate, sodium citrate, disodium EDTA, and potassium sodium tartrate.
[0024] And / or, based on 1 t of dry spodumene ore to be sorted, the anionic dispersant is 100-1000 g;
[0025] And / or, the duration of the modification treatment is 2-10 minutes.
[0026] Preferably, the metal ion activator is a manganese salt ion modifier, preferably at least one of manganese sulfate, manganese nitrate, and manganese chloride; other types of metal ion activators may also be used, such as Ca... 2+ Mg 2+ Fe 3+ However, in the solution equilibrium of the low-temperature separation system, Mn 2+It is more beneficial for subsequent mineralization and harvesting when it exists mostly in the form of Mn(OH)2 precipitate.
[0027] And / or, based on the weight of 1 t of dry spodumene ore to be sorted, the amount of the metal ion activator is 100-1000g;
[0028] And / or, the duration of the ion activation treatment is 2-10 min.
[0029] Preferably, the amount of spodumene mineral collector used is 100-4000g, based on 1t of dry spodumene ore to be sorted.
[0030] And / or, a foaming agent is also added during the mineralization process; when collecting and flotating spodumene minerals, since the collector generally has a foaming function, it is often not necessary to add a foaming agent separately. Therefore, the addition of a foaming agent is optional.
[0031] And / or, the duration of the mineralization treatment is 2-10 min.
[0032] Preferably, the foaming agent is at least one of No. 2 oil, 4-methyl-2-pentanol (MIBC), and fusel oil;
[0033] And / or, the mass ratio of the foaming agent to the spodumene mineral collector is 1:(20-200).
[0034] Preferably, the flotation separation adopts a mineral flotation process combining roughing, cleaning, and scavenging.
[0035] And / or, the flotation separation is followed by concentration and compression processing;
[0036] And / or, the temperature of the flotation pulp in the flotation separation is 5-60℃, preferably 5-19℃.
[0037] Preferably, each coarse selection segment takes 3-6 minutes;
[0038] And / or, the selected segment is sorted for 2-4 minutes each;
[0039] And / or, the scanning process for each segment takes 3-6 minutes.
[0040] The technical solution of this invention has the following advantages:
[0041] A flotation process for spodumene mineral includes: crushing the spodumene ore to be separated to obtain crushed ore; adding water to the crushed ore and grinding it to achieve mineral liberation, while adding a grinding modifier during the grinding process to obtain a grinding slurry; wherein the grinding modifier includes highly active OH... -The process involves adjusting the grinding slurry with a modifier and a strong oxidant, followed by modification with an anionic dispersant, ion activation with a metal ion activator, and finally mineralization with a spodumene mineral collector. The spodumene mineral collector is then separated by flotation to obtain spodumene concentrate and flotation tailings. The spodumene mineral collector comprises anionic and cationic active components, and an emulsifier. The anionic active component is at least one of aminocarboxylate, polyoxyethylene sulfate, alkyl sulfonate, and succinate. The cationic active component is a halogenated modified organic amine salt or / and a halogenated pyridine organic compound. This invention optimizes the flotation process from the perspectives of grinding mineral surface modification, mineral dispersion and activation, and mineral collection and mineralization. The interconnected process significantly improves the lithium recovery rate and separation selectivity (grade) of spodumene minerals in low-temperature flotation. Specifically: 1) A highly active OH group is added during the mineral grinding process. - Modifiers and strong oxidizing agents, thereby utilizing highly active OH groups. - (instead of CO3) 2- ) and high oxidation reaction driving force, enhance the mediating performance of the Si dissolution process at the mineral interface, rapidly promote the hydroxylation of exposed species on the mineral surface, form an active surface with strong expression of hydroxylated negative charge, and simultaneously reduce the viscosity of the slurry with high oxidation state separation, enhance the tendency of selective modification of the mineral surface, increase the difference in surface properties between the target mineral and gangue minerals, and improve the efficiency of low-temperature flotation separation; 2) After grinding and slurry conditioning, anionic dispersant is added to reduce the resistance of reagent molecules to movement in solution with solution ionic active components, improve the material carrying capacity and dissolution activity of low-temperature slurry, adjust and optimize the slurry dispersion trend, and further enhance the expression of ionic characteristics of mineral surface by selective and directional adsorption of active anions, thereby increasing the difference in surface properties between the target mineral and gangue minerals. 3) After modification, metal ion activators are added to selectively compete for adsorption on the surface of strongly hydroxylated and anion-adsorbed minerals, thereby activating the mineral surface by selectively expressing characteristic metal ion properties; 4) In the mineralization and collection step, aminocarboxylate salts, polyoxyethylene sulfates, alkyl sulfonates, and succinates are used as anion-collecting active components, and halogen-modified organic amine salts and / or halogenated pyridine organic compounds are used as cationic-collecting active components. At the same time, emulsifiers are added for combined collection. Based on the synergistic effect of enhanced chemical dissolution and structure-activity relationship, the low-temperature dissolution, separation, and emulsification performance of the collector are enhanced, the low-temperature reaction activity of the collector is enhanced, the mineralization efficiency of the mineral is improved, and thus the spodumene separation efficiency is improved. Detailed Implementation
[0042] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0043] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0044] Example 1
[0045] This embodiment provides a low-temperature flotation process for spodumene minerals, separating low-grade spodumene ore from a high-altitude, cold region in Xinjiang. The raw ore has a Li₂O content of 0.83%, and 90% of the lithium-containing minerals are spodumene. The flotation pulp temperature is 10℃-12℃, and the process includes the following steps:
[0046] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed by a three-stage jaw crusher to obtain crushed mineral material with a maximum particle size of 3mm;
[0047] (2) Grinding treatment: Water and grinding modifier are added to the crushed mineral material in step (1), and the material is ground using a ball mill until the content of -0.074mm is 75%. Water is added to adjust the concentration of the grinding slurry to 65%. The amount of grinding modifier used is 1000g / t based on the dry spodumene ore. The grinding modifier is composed of highly active OH... - The mixture consists of a modifier (800g / t sodium hydroxide) and a strong oxidant (200g / t potassium permanganate) to selectively dissolve the surface and regulate the low-temperature water environment, thus obtaining the grinding slurry.
[0048] (3) Slurry conditioning and modification: Water is added to the grinding slurry in step (2) to condition the slurry mass concentration to 33%. Then, sodium lignosulfonate with a concentration of 200 g / t based on the dry spodumene ore to be separated is added as an anionic dispersant to selectively disperse mineral particles, so as to improve the viscosity of the low-temperature slurry and its mineral surface activity. The dispersion and stirring modification reaction time is 3 min to obtain the surface-controlled dispersion modified slurry.
[0049] (4) Ion activation treatment: Add 200 g / t of manganese chloride as a metal ion activator to the dispersed modified slurry in step (3), and stir for 3 min to obtain ion activated slurry.
[0050] (5) Mineral mineralization and collection: Add sodium lauryl sulfoacetate + hexadecyl bromide + propylene glycol monostearate as spodumene mineral collectors, based on 600+100+30g / t of dry spodumene ore to be separated, to the ion-activated slurry in step (4), and stir for 3 minutes to collect and mineralize the spodumene minerals to obtain the mineralized separation slurry.
[0051] (6) Low-temperature flotation separation and recovery of lithium minerals: The mineralized slurry from step (5) was separated using a closed-circuit flotation process consisting of one roughing stage, three cleaning stages, and two scavenging stages. The resulting spodumene-containing concentrate and flotation tailings were then separated. The roughing stage lasted 4 minutes per segment, the scavenging stage lasted 4 minutes per segment, and the cleaning stage lasted 3 minutes per segment. The resulting spodumene-containing concentrate and flotation tailings were then concentrated and filtered to obtain and recover the spodumene concentrate and flotation tailings. Under low-temperature conditions of 10℃-12℃, the Li2O recovery rate in the spodumene concentrate obtained in this embodiment was 77.3%, and the Li2O grade was 5.98%.
[0052] Example 2
[0053] The difference between this embodiment and Example 1 is that the flotation pulp temperature is 25℃-26℃, while other conditions are the same as in Example 1. In the spodumene concentrate product obtained in this embodiment, the Li₂O recovery rate is 78.7%, and the Li₂O grade is 5.63%.
[0054] Example 3
[0055] This embodiment provides a low-temperature flotation process for spodumene minerals, separating spodumene from a high-altitude methylka spodumene mine in western Sichuan. The raw ore has a Li₂O content of 1.43%, and 92% of the lithium-containing minerals are spodumene. The flotation pulp temperature is 10℃-12℃, and the process includes the following steps:
[0056] (1) Crushing process: The above spodumene ore raw material is crushed twice by a jaw crusher and once by a double roller crusher to obtain crushed mineral material with a maximum particle size of 2mm.
[0057] (2) Grinding treatment: Water and grinding modifier are added to the crushed ore in step (1) and ground using a ball mill until the content of the material fineness is -0.074mm accounts for 70%. Among them, water is added to adjust the concentration of the grinding slurry to 67%. The amount of grinding modifier used is 2000g / t based on the dry ore of spodumene. The grinding modifier is composed of highly active OH - The mixture consists of a modifier (1800g / t ammonia water) and a strong oxidant (200g / t sodium perchlorate) to selectively dissolve the surface and regulate the low-temperature water environment, thus obtaining the grinding slurry.
[0058] (3) Slurry conditioning and modification: Water is added to the grinding slurry in step (2) to condition the slurry concentration to 38%, and then sodium bicarbonate of 600 g / t based on the dry spodumene ore to be separated is added as an anionic dispersant to selectively disperse mineral particles, so as to improve the viscosity of the low-temperature slurry and its mineral surface activity. The dispersion and stirring modification reaction time is 5 min to obtain the surface-controlled dispersion modified slurry.
[0059] (4) Ion activation treatment: Add 100 g / t of manganese sulfate as a metal ion activator to the dispersed modified slurry in step (3), and stir for 5 min to obtain ion activated slurry.
[0060] (5) Mineral mineralization and collection: Add 1000+200+60g / t of benzyloxycarboxyl amino acid + dodecyl ammonium bromide + diesel oil as spodumene mineral collector to the ion-activated slurry in step (4), and stir for 3 minutes to collect and mineralize the spodumene mineral collector to obtain the mineralized slurry.
[0061] (6) Low-temperature flotation separation and recovery of lithium minerals: The mineralized slurry from step (5) is separated using a closed-circuit flotation process consisting of one roughing stage, three cleaning stages, and one scavenging stage. The resulting spodumene-containing concentrate and flotation tailings are then separated. The roughing stage lasts 3 minutes per segment, the scavenging stage lasts 3 minutes per segment, and the cleaning stage lasts 2 minutes per segment. The resulting spodumene-containing concentrate and flotation tailings are then concentrated and filtered to obtain and recover the spodumene concentrate and flotation tailings. Under low-temperature conditions of 10℃-12℃, the Li2O recovery rate in the spodumene concentrate obtained in this embodiment is 83.5%, and the Li2O grade is 5.78%.
[0062] Example 4
[0063] The difference between this embodiment and Embodiment 3 is that the flotation pulp temperature is 25℃-26℃, while other conditions are the same as in Embodiment 3. In the spodumene concentrate product obtained in this embodiment, the Li₂O recovery rate is 85.7%, and the Li₂O grade is 5.94%.
[0064] Example 5
[0065] The difference between this embodiment and Example 3 is that calcium chloride is used as the metal ion activator in the ion activation treatment; other conditions are the same as in Example 3. In the spodumene concentrate product obtained in this embodiment, the Li₂O recovery rate is 80.3%, and the Li₂O grade is 5.72%.
[0066] Example 6
[0067] This embodiment provides a low-temperature flotation process for spodumene minerals, separating spodumene from a high-altitude methylka spodumene mine in western Sichuan. The raw ore has a Li₂O content of 1.43%, and 92% of the lithium-containing minerals are spodumene. The flotation pulp temperature is 5℃-10℃, and the process includes the following steps:
[0068] (1) Crushing process: The above spodumene ore raw material is crushed twice by a jaw crusher and once by a double roller crusher to obtain crushed mineral material with a maximum particle size of 1mm.
[0069] (2) Grinding treatment: Water and grinding modifier are added to the crushed mineral material in step (1), and the material is ground using a ball mill until the content of -0.074mm is 50%. Water is added to adjust the concentration of the grinding slurry to 50%. The amount of grinding modifier used is 2500g / t based on the dry spodumene ore. The grinding modifier is composed of highly active OH... - The mixture consists of a modifier (2000g / t ammonia water) and a strong oxidant (500g / t sodium persulfate) to selectively dissolve the surface and regulate the low-temperature water environment, thus obtaining the grinding slurry.
[0070] (3) Slurry conditioning and modification: Water is added to the grinding slurry in step (2) to condition the slurry concentration to 25%, and then sodium carbonate is added at a rate of 100 g / t based on the dry spodumene ore to be separated as an anionic dispersant to selectively disperse mineral particles, so as to improve the viscosity of the low-temperature slurry and its mineral surface activity. The dispersion and stirring modification reaction time is 10 min to obtain the surface-controlled dispersion modified slurry.
[0071] (4) Ion activation treatment: Add 100 g / t of manganese nitrate as a metal ion activator to the dispersed modified slurry in step (3), and stir for 10 min to obtain ion-activated slurry.
[0072] (5) Mineral mineralization and collection: Add 3000+600+180g / t of sodium lauryl polyoxyethylene ether sulfate + cetyl pyridine chloride + kerosene as spodumene mineral collector to the ion-activated slurry in step (4), and stir for 2 minutes to collect and mineralize the spodumene minerals to obtain the mineralized slurry.
[0073] (6) Low-temperature flotation separation and recovery of lithium minerals: The mineralized slurry from step (5) is separated using a closed-circuit flotation process consisting of one roughing stage, three cleaning stages, and one scavenging stage. The resulting spodumene-containing concentrate and flotation tailings are then separated. The roughing stage lasts 6 minutes per segment, the scavenging stage lasts 6 minutes per segment, and the cleaning stage lasts 4 minutes per segment. The resulting spodumene-containing concentrate and flotation tailings are then concentrated and filtered to obtain and recover the spodumene concentrate and flotation tailings. Under low-temperature conditions of 5℃-10℃, the Li2O recovery rate in the spodumene concentrate obtained in this embodiment is 83.4%, and the Li2O grade is 5.78%.
[0074] Example 7
[0075] This embodiment provides a low-temperature flotation process for spodumene minerals, separating spodumene from a high-altitude methylka spodumene mine in western Sichuan. The raw ore has a Li₂O content of 1.43%, and 92% of the lithium-containing minerals are spodumene. The flotation pulp temperature is 12℃-15℃, and the process includes the following steps:
[0076] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed twice by a jaw crusher and once by a double roller crusher to obtain crushed mineral material with a maximum particle size of 12mm.
[0077] (2) Grinding treatment: Water and grinding modifier are added to the crushed ore in step (1) and ground using a ball mill until the content of the material fineness is -0.074mm accounts for 95%. Among them, water is added to adjust the concentration of the grinding slurry to 85%. The amount of grinding modifier used is 140g / t based on the dry ore of spodumene. The grinding modifier is composed of highly active OH - The mixture consists of a modifier (100g / t potassium hydroxide) and a strong oxidant (40g / t sodium perchlorate) to selectively dissolve the surface and regulate the low-temperature water environment, thus obtaining the grinding slurry.
[0078] (3) Slurry conditioning and modification: Water is added to the grinding slurry in step (2) to condition the slurry concentration to 50%, and sodium bicarbonate of 1000 g / t based on the dry spodumene ore to be separated is added as an anionic dispersant to selectively disperse mineral particles, so as to improve the viscosity of the low-temperature slurry and its mineral surface activity. The dispersion and stirring modification reaction time is 2 min to obtain the surface-controlled dispersion modified slurry.
[0079] (4) Ion activation treatment: Add 1000 g / t of manganese sulfate as a metal ion activator to the dispersed modified slurry in step (3), and stir for 2 min to obtain ion activated slurry.
[0080] (5) Mineral mineralization and collection: Add sodium dioctyl succinate sulfonate + hexadecyl bromopyridine + propylene glycol monostearate as spodumene mineral collector to the ion-activated slurry in step (4) with 300+50+15g / t of dry spodumene ore to be separated as spodumene mineral collector, and stir for 10min to collect and mineralize the spodumene mineral collection reaction to obtain the mineralized separation slurry.
[0081] (6) Low-temperature flotation separation and recovery of lithium minerals: The mineralized slurry from step (5) was separated using a closed-circuit flotation process consisting of one roughing stage, three cleaning stages, and one scavenging stage. The resulting spodumene concentrate and flotation tailings were separated. The roughing stage lasted 3 minutes per segment, the scavenging stage lasted 3 minutes per segment, and the cleaning stage lasted 2 minutes per segment. Under low-temperature conditions of 10℃~12℃, the Li2O recovery rate in the spodumene concentrate obtained in this embodiment was 85.8%, and the Li2O grade was 5.84%.
[0082] Comparative Example 1
[0083] This comparative example provides a flotation process for existing spodumene minerals. The difference between this comparative example and Example 1 is that only 1000 g / t sodium carbonate is added in the grinding step, 200 g / t sodium hydroxide is used in the modification step, 200 g / t magnesium chloride is used in the ion activation step, and a combined collector of 1800 g / t (paraffin soap + naphthenic acid soap + diesel oil) is used in the mineralization and collection step. Other conditions are the same as in Example 1. At a room temperature of 25°C, the spodumene concentrate obtained has a Li₂O recovery rate of 81.2% and a Li₂O content of 5.61%. At a flotation pulp temperature of 10-12°C, the spodumene concentrate obtained has a Li₂O recovery rate of 63.6% and a Li₂O grade of 5.21%.
[0084] Comparative Example 2
[0085] This comparative example provides a flotation process for spodumene mineral. The process route is: sodium carbonate grinding - sodium hydroxide modification - metal ion activation treatment - mineralization and collection. The difference between this comparative example and Example 1 is that in the grinding step, 800 g / t sodium hydroxide + 200 g / t potassium permanganate is replaced with 1000 g / t sodium carbonate, and in the modification step, 200 g / t sodium lignosulfonate is replaced with 200 g / t sodium hydroxide. Other conditions are the same as in Example 1. In the spodumene concentrate product obtained in this comparative example, the Li2O recovery rate is 65.6%, and the Li2O grade is 5.48%.
[0086] Comparative Example 3
[0087] This comparative example provides a flotation process for spodumene mineral. The process route is as follows: sodium carbonate grinding - sodium lignosulfonate modification - metal ion activation treatment - mineralization and collection. The difference between this comparative example and Example 1 is that in the grinding step, sodium hydroxide + potassium permanganate = 800 g / t + 200 g / t is replaced with 1000 g / t sodium carbonate, while other conditions are the same as in Example 1. In the spodumene concentrate product obtained in this comparative example, the Li2O recovery rate is 72.2%, and the Li2O grade is 5.34%.
[0088] Comparative Example 4
[0089] The difference between this comparative example and Example 1 is that no strong oxidant was added during the grinding process; all other conditions were the same as in Example 1. The spodumene concentrate product obtained in this comparative example had a Li₂O recovery rate of 70.2% and a Li₂O grade of 5.40%.
[0090] Comparative Example 5
[0091] The difference between this comparative example and Example 1 is that hexadecylpyridine bromide (the active ingredient for cation trapping) was replaced with dodecylamine; all other conditions were the same as in Example 1. In the spodumene concentrate product obtained in this comparative example, the Li₂O recovery rate was 72.3%, and the Li₂O grade was 4.52%.
[0092] Comparative Example 6
[0093] The difference between this comparative example and Example 1 is that a combined collector of cocoagulant (cation-collecting active component) + sodium dodecyl sulfate (anion-collecting active component) + kerosene (emulsifier) = 1000 + 400 + 60 g / t was used for flotation separation. Other conditions were the same as in Example 1. The above combined collector showed no mineral separation selectivity in spodumene flotation. In the spodumene concentrate obtained in this comparative example, the Li2O recovery rate was only 32.1%, and the Li2O content was only 1.18%.
[0094] Comparative Example 7
[0095] The difference between this comparative example and Example 1 is that flotation separation was performed using a combined collector of oxidized paraffin soap + dodecylamine + diesel oil = 2000 + 400 + 100 g / t. Other conditions were the same as in Example 1. In the spodumene concentrate product obtained in this comparative example, the Li2O recovery rate was 70.2% and the Li2O content was 5.55%.
[0096] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A flotation process for spodumene mineral, characterized in that, include: The spodumene ore to be sorted is crushed to obtain crushed mineral materials; Water is added to crushed mineral materials and the mixture is ground to dissociate the minerals. A grinding modifier is added during the grinding process to obtain a grinding slurry. The grinding modifier includes highly active OH groups. - Modifier and strong oxidizing agent; the highly active OH - The modifier is at least one of sodium hydroxide, potassium hydroxide, ammonia, or organic amines; The grinding slurry is subjected to slurry conditioning treatment, followed by modification treatment with an anionic dispersant, ion activation treatment with a metal ion activator, and finally mineralization treatment with a spodumene mineral collector. The spodumene concentrate and flotation tailings are obtained by flotation separation. The metal ion activator is a manganese salt ion modifier. The spodumene mineral collector comprises an anion-collecting active component, a cationic-collecting active component, and an emulsifier; the anion-collecting active component is at least one of aminocarboxylate, polyoxyethylene sulfate, alkyl sulfonate, and succinate; the cationic-collecting active component is a halogen-modified organic amine salt or / and a halogenated pyridine organic compound; the mass ratio of the anion-collecting active component, the cationic-collecting active component, and the emulsifier is 1:(0.2-0.05):(0.02-0.1).
2. The flotation process according to claim 1, characterized in that, The anion-trapping active component is at least one of the following: α-amino acid, N,N-dihydroxyethylglycine, benzyloxycarbonyl amino acid, 1-benzyl D-glutamate, N-hydroxyethyllinoleic acid amide, sodium alkylphenol polyoxyethylene ether sulfate, sodium lauryl polyoxyethylene ether sulfate, sodium α-alkenyl sulfonate, sodium lauryl sulfoacetate, disodium lauryl polyoxyethylene ether sulfosuccinate, and sodium dioctyl succinate sulfonate. And / or, the cation-trapping active component is at least one of dodecylammonium bromide, benzalkonium bromide, hexadecyltrimethylammonium chloride, hexadecylpyridine chloride, and hexadecylpyridine bromide; And / or, the emulsifier is a neutral oil or / and ester organic compound.
3. The flotation process according to claim 2, characterized in that, The emulsifier is at least one of kerosene, diesel oil, propylene glycol monostearate, propylene glycol alginate, ethylene glycol monostearate, glyceryl monostearate, and sorbitol fatty acid ester.
4. The flotation process according to any one of claims 1-3, characterized in that, The maximum particle size of the crushed mineral material is 1-12 mm; And / or, the grinding process is performed to achieve a mineral fineness of -0.074 mm, with the content of minerals comprising 50-95%; And / or, the strong oxidizing agent is at least one of persulfate, permanganate, and perchlorate.
5. The flotation process according to claim 4, characterized in that, The persulfate is at least one of potassium persulfate, potassium peroxymonosulfate, sodium persulfate, and ammonium persulfate; the permanganate is at least one of potassium permanganate, sodium permanganate, and ammonium permanganate; and the perchlorate is at least one of sodium perchlorate, potassium perchlorate, magnesium perchlorate, and manganese perchlorate.
6. The flotation process according to claim 1, characterized in that, Based on a weight of 1 ton of dry spodumene ore to be separated, the amount of grinding modifier used is 100-2500 g, of which highly active OH... - The dosage of the modifier is 100-2000 g, and the dosage of the strong oxidant is 40-500 g; And / or, the mass concentration of the grinding slurry is 50-85%.
7. The flotation process according to claim 1, characterized in that, The mass concentration of the slurry after the slurry conditioning treatment is 25-50%; And / or, the anionic dispersant is at least one of carbonate, bicarbonate, organic carboxylate, and lignin sulfonate; And / or, based on 1 t of dry spodumene ore to be sorted, the anionic dispersant is 100-1000 g; And / or, the duration of the modification treatment is 2-10 min.
8. The flotation process according to claim 7, characterized in that, The anionic dispersant is at least one of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium lignosulfonate, magnesium lignosulfonate, ammonium lignosulfonate, sodium citrate, disodium EDTA, and sodium potassium tartrate.
9. The flotation process according to claim 1, characterized in that, The manganese salt ion modifier is at least one of manganese sulfate, manganese nitrate, and manganese chloride; And / or, based on the weight of 1 t of dry spodumene ore to be sorted, the amount of the metal ion activator is 100-1000 g; And / or, the duration of the ion activation treatment is 2-10 min.
10. The flotation process according to claim 1, characterized in that, Based on a weight of 1 t of dry spodumene ore to be sorted, the amount of spodumene mineral collector used is 100-4000 g. And / or, the duration of the mineralization treatment is 2-10 min.
11. The flotation process according to claim 1, characterized in that, The flotation separation adopts a mineral flotation process combining roughing, cleaning, and scavenging. And / or, the flotation separation is followed by concentration and compression processing; And / or, the temperature of the flotation pulp in the flotation separation is 5-60℃.
12. The flotation process according to claim 11, characterized in that, The temperature of the flotation pulp in the flotation separation is 5-19℃.
Citation Information
Patent Citations
Flotation stirring device, flotation system and method for conducting zinc flotation
CN107008574A
Novel low-grade spodumene ore flotation collecting agent and spodumene ore beneficiation method
CN111250269A
Rapid flotation process for efficiently recycling coarse-grain copper slag
CN115999781A
Method for grinding and floating separation of lithium ore and lithium concentrate product
CN117019407A