A flotation method for spodumene minerals
By using a solution buffer combination and a highly active OH- modifier in the flotation of spodumene minerals, combined with a metal ion activator, the synergistic effect of mineral surface modification and collector is optimized, thus solving the problem of low separation efficiency of spodumene minerals and achieving efficient separation and reagent saving.
Patent Information
- Application Number
- CN202410568652.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-09
AI Technical Summary
In existing spodumene mineral sorting processes, the sorting efficiency is low, it is difficult to effectively separate spodumene from gangue minerals, and the reagent consumption is high, with poor sorting selectivity.
The grinding modifiers, including solution buffers and unavoidable metal ion modifiers, are used to adjust the pulp pH to 7.5-9.0. The pulp is then treated with highly active OH- modifiers and metal ion activators, and flotation separation is performed in combination with spodumene mineral collectors to optimize the synergistic effect of mineral surface modification and collectors.
It improves the flotation separation efficiency of spodumene and gangue minerals, reduces reagent consumption, stabilizes the pulp solution state, improves the dispersion of fine-grained minerals, and increases the efficiency of water recycling.
Abstract
Description
Technical Field
[0001] This invention relates to the field of mineral sorting and processing technology, and specifically to a flotation method for spodumene mineral. Background Technology
[0002] Spodumene is a clinopyroxene composed of single-chain lithium aluminum silicates, typically occurring in hard rock pegmatite deposits. Pegmatite is an intrusive igneous rock primarily composed of linked mineral grains of quartz, feldspar, spodumene, and mica. Among lithium-rich pegmatite minerals, spodumene is a crucial raw material for lithium metal processing and possesses significant economic value. Current spodumene mineral sorting and processing methods include hand sorting, gravity separation, flotation, heavy media separation, or combinations thereof, but flotation remains the dominant method, especially for the enrichment and recovery of fine-grained spodumene minerals. Based on the ore properties of spodumene, various flotation technologies have been developed and applied in numerous spodumene ore enrichment and recovery processes, such as whole-sludge flotation, desliming flotation, heavy media separation-flotation, and flotation-magnetic separation. These processes are all based on the differences in the physicochemical properties of the surfaces of spodumene and gangue minerals. However, factors such as the similar floatability of the target mineral and gangue minerals, the unavoidable improper adsorption of metal ion impurities, the difficulty in controlling the surface properties of minerals, and the lack of a prominent trend of directional adsorption and capture often cause spodumene minerals and gangue minerals to exhibit similar floatability in the mineral separation system, resulting in low selectivity and efficiency of flotation separation between spodumene minerals and gangue minerals.
[0003] Currently, numerous flotation separation tests and industrial applications in spodumene ore mining demonstrate that the "three alkalis" (soda ash-hydroxide-metal ion) surface control technology possesses certain relative advantages and is the most widely used method. It consists of the following three steps: First, carbonates are added during the grinding process to act on the medium solution and the surface of newly formed minerals, thereby effectively improving the subsequent separation and sorting of minerals. The carbonate ions (CO3)... 2- The effective functions of ) include: a) avoiding or settling unavoidable metal ions (Mg) in aqueous solutions. 2+ / Ca 2+ / Al 3+ / Fe 3+ (e.g., to prevent the inevitable indiscriminate adsorption of metal ions, which would lead to a convergence of mineral surface properties; b) to modify and adjust the differences in surface properties of different minerals, enhancing the differences in surface properties between gangue minerals and spodumene minerals; c) to disperse or reduce the negative effects of fine-grained minerals, etc. During this process, CO3... 2- Metal ions are unavoidable in precipitated / modified solutions, thus the adsorption of these unavoidable metal ions should be avoided. Simultaneously, the exposed Al on the lithium mineral dissociation surface... 3+ / Li + It can also adsorb CO3 at the cation sites on the surface of lithium minerals.2- The second step is to add sodium hydroxide (OH-). - The purpose of prolonged and vigorous stirring and slurry preparation is to utilize OH... - Dissolving or scrubbing the Si sites on the surface of spodumene minerals, while simultaneously reacting with the Al sites on the surface of lithium minerals from the first step. 3+ / Li + Originally adsorbed CO3 2- Competition leads to the formation of more OH groups on the surface of spodumene minerals. - The active region is remodeled to reshape the surface of the spodumene mineral; the third step involves adding metal cations (Ca). 2+ / Mg 2+ Plasma activation utilizes metal cations to move OH groups to specific spatial positions / regions adjusted in the "second step". - The adsorption process achieves selective activation of the target mineral. However, due to the difference in the exposed active components or spatial structure of gangue minerals (feldspar, quartz, mica, etc.) compared to spodumene minerals, it is extremely difficult for the aforementioned CO3 adsorption to occur on the surface of gangue minerals. 2- Modified -OH - Active-Ca 2+ / Mg 2+ The ion-activated sequential reaction process results in differences in floatability between spodumene and gangue minerals after modification and adjustment, as well as between anionic and cationic collectors.
[0004] However, in the above-mentioned flotation modifier system, carbonate is first used as a precipitant or fine particle dispersant for unavoidable ions in the flotation system and their gangue mineral surfaces, and then caustic alkali is added to achieve high OH- ions. - The selective activation of spodumene by the dissolution and cleaning of its surface by active species typically results in a relatively high alkalinity (pH 9.5-11) in the overall solution system. This deviates from the pH range (pH 8.0-9.0) where many spodumene collectors exhibit high activity. In other words, there is a certain contradiction between existing high-alkalinity modifier systems and the segregation activity of spodumene collectors, leading to drawbacks such as excessive pressure and pull resulting in high overall reagent consumption and poor separation selectivity. Although many flotation separation technologies for spodumene have been reported, existing techniques are often limited by factors such as the similar physicochemical properties of the target mineral and gangue mineral surfaces, the complex ionic state of the separation solution medium, excessively high alkalinity of the separation solution, and low synergistic efficiency between modifiers and collectors, resulting in low flotation separation efficiency for lithium minerals. Summary of the Invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defect of low separation efficiency of existing spodumene minerals, thereby providing a flotation method for spodumene minerals that solves the above problem.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] A flotation method for spodumene minerals, comprising:
[0008] The spodumene ore to be sorted is crushed to obtain crushed mineral materials;
[0009] Water is added to crushed mineral materials and the materials are ground to dissociate the minerals. A grinding modifier is added during the grinding process to obtain a grinding slurry.
[0010] The grinding slurry is conditioned and then highly active OH groups are added sequentially. - The modifier is subjected to alkaline etching treatment, metal ion activator is added for ion activation treatment, and finally spodumene mineral collector is added for mineralization treatment and flotation separation to obtain spodumene concentrate and flotation tailings.
[0011] The grinding modifier includes a solution buffer combination and an unavoidable metal ion modifier;
[0012] The solution buffer combination is an adjuster that can adjust the pH of the slurry to the range of 7.5-9.0.
[0013] Preferably, the maximum particle size of the crushed mineral material is 1-12 mm;
[0014] And / or, the grinding process results in a mineral fineness of -0.074 mm (maximum particle size of 0.074 mm) content of 50%-95%.
[0015] Preferably, the unavoidable metal ion adjuster is a carbonate or / and bicarbonate, and more preferably at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate.
[0016] And / or, the mass ratio of the solution buffer combination to the unavoidable metal ion adjuster is (1-100):1, wherein, based on the weight of 1t of dry spodumene ore to be separated, the amount of the solution buffer combination is 100-80000g / t, and the amount of the unavoidable metal ion adjuster is 100-4000g / t.
[0017] And / or, the mass concentration of the grinding slurry is 50-85%.
[0018] Preferably, the solution buffer combination is at least one of the following: borate + hydrochloric acid combination, perboric acid + hydrochloric acid + sodium hydroxide combination, potassium dihydrogen phosphate + disodium hydrogen phosphate combination, potassium dihydrogen phosphate + sodium hydroxide combination, tris(hydroxymethyl)aminomethane + hydrochloric acid combination, and ammonium chloride + ammonia combination. The above-mentioned solution buffer combination has both the function of directional regulation of ions in the solution medium and the mineral surface, and the function of buffering and slow-release control of the solution medium and the mineral surface.
[0019] Preferably, in the borate + hydrochloric acid combination, the molar ratio of borate to hydrochloric acid is 1:(0.8-3), and the concentration of borate in the grinding slurry is 0.03-0.1 mol / L;
[0020] And / or, in the combination of perboric acid + hydrochloric acid + sodium hydroxide, the molar ratio of perboric acid, hydrochloric acid and sodium hydroxide is 1:1:(0.2-1), and the concentration of perboric acid in the grinding slurry is 0.05-0.1 mol / L;
[0021] And / or, in the potassium dihydrogen phosphate + disodium hydrogen phosphate combination, the molar ratio of potassium dihydrogen phosphate to disodium hydrogen phosphate is 1:(3-5), and the concentration of potassium dihydrogen phosphate in the grinding slurry is 0.01-0.05 mol / L;
[0022] And / or, in the potassium dihydrogen phosphate + sodium hydroxide combination, the molar ratio of potassium dihydrogen phosphate to sodium hydroxide is 1:(0.6-1.2), and the concentration of potassium dihydrogen phosphate in the grinding slurry is 0.05-0.10 mol / L;
[0023] And / or, in the tris(hydroxymethyl)aminomethane + hydrochloric acid combination, the molar ratio of tris(hydroxymethyl)aminomethane to hydrochloric acid is 1:(1-10), and the concentration of tris(hydroxymethyl)aminomethane in the grinding slurry is 0.08-0.1 mol / L;
[0024] And / or, in the ammonium chloride + ammonia combination, the molar ratio of ammonium chloride to ammonia is 1:(0.4-1), and the concentration of ammonium chloride in the grinding slurry is 0.4-1.0 mol / L.
[0025] Preferably, the mass concentration of the slurry after the slurry conditioning treatment is 25%-50%;
[0026] And / or, the highly active OH - The modifier is at least one of sodium hydroxide, potassium hydroxide, and ammonia water;
[0027] And / or, based on 1 t of dry spodumene ore to be sorted, the highly active OH... - The dosage of the modifier is 100-2000 g / t;
[0028] And / or, the duration of the alkaline etching treatment is 10-30 min;
[0029] And / or, after the alkaline etching treatment, a solution buffer mixture of 0.18-0.5 times the amount of solution buffer mixture used in the grinding treatment is added. This addition is optional; if the amount of solution buffer mixture used in the grinding treatment is sufficient, the solution buffer mixture may be selectively omitted after the alkaline etching treatment.
[0030] Preferably, the metal ion activator is at least one selected from calcium chloride, magnesium chloride, ferric chloride, magnesium sulfate, manganese sulfate, sodium nitrate, and potassium nitrate.
[0031] And / or, based on 1 t of dry spodumene ore to be sorted, the amount of the metal ion activator is 50-1000 g.
[0032] And / or, the duration of the ion activation treatment is 10-30 min.
[0033] Preferably, the spodumene mineral collector is at least one selected from the following: oxidized paraffin soap, naphthenic acid soap, sodium oleate, oleic acid, dodecylamine, tetradecylamine, benzoyl hydroxamic acid, salicylic acid, alkyl amino acids, and alkyl amides.
[0034] And / or, based on 1 t of dry spodumene ore to be sorted, the amount of spodumene mineral collector used is 100-4000 g / t.
[0035] Preferably, a frother is also added during the mineralization process; when collecting and flotating spodumene minerals, since the collector generally has a bubble-generating function, a frother is usually not added separately, so the addition of a frother is optional.
[0036] And / or, the duration of the mineralization treatment is 2-10 min.
[0037] Preferably, the foaming agent is at least one of No. 2 oil, MIBC, and fusel oil;
[0038] And / or, the mass ratio of the foaming agent to the spodumene mineral collector is 1:(20-200).
[0039] Preferably, the flotation separation adopts a mineral flotation process combining roughing, cleaning, and scavenging.
[0040] And / or, the flotation separation is followed by concentration and compression.
[0041] Preferably, the coarse selection process takes 3-6 minutes per segment;
[0042] And / or, the sorting time for each selected segment is 2-4 minutes;
[0043] And / or, the sorting time for each segment of the scanning process is 3-6 minutes.
[0044] The technical solution of this invention has the following advantages:
[0045] A flotation method for spodumene mineral includes: crushing the spodumene ore to be separated to obtain crushed ore; adding water to the crushed ore and grinding it to liberate the minerals, while adding a grinding modifier during the grinding process to obtain a grinding slurry; conditioning the grinding slurry, and then sequentially adding highly active OH groups. - The grinding modifier undergoes alkaline etching treatment, followed by ion activation treatment with the addition of a metal ion activator, and finally mineralization treatment with a spodumene mineral collector, followed by flotation separation to obtain spodumene concentrate and flotation tailings. The grinding modifier includes a solution buffer combination and an unavoidable metal ion modifier. Current technologies often reduce alkalinity by replacing the flotation agent in the "three-alkali" system with a low-alkalinity substance (e.g., sodium lignin sulfonate) to lower the alkalinity for flotation, or by adjusting the pulp pH during collection to increase the collector activity. This invention, however, uses OH... - The "three alkalis" system is improved from the perspective of buffer logic. Based on the strong supplementary or catalytic reaction advantages of the buffer system, the "three alkalis" can be used to achieve efficient modification and regulation of mineral surfaces. The modification trend and efficiency of the "three alkalis" on different mineral surfaces are optimized, thereby significantly improving the reagent efficiency of the entire flotation separation system and reducing reagent consumption, which cannot be achieved by simply adjusting the pulp pH.
[0046] Specifically, the main functions of adding a solution buffer combination agent during the grinding process in this invention are: 1) to enhance the CO3 content of the slurry during the grinding process. 2- and pH (free OH) - Each of these functions effectively enhances the efficiency of the grinding slurry, thereby improving the concentration of unavoidable Ca. 2+ / Mg 2 + / Fe 3+ The precipitation and modification efficiency in Ca2+; that is, fully utilizing the difference in solubility products between different metal ions and carbonates / hydroxides and based on the principle of precipitation / dissolution equilibrium, leveraging the buffering effect to make Ca2+... 2+ / Mg 2+ / Fe 3+ The tendency for unavoidable ions to be modified by directional precipitation is enhanced, thereby greatly reducing the negative effects of unavoidable metal ions (e.g., the solubility product of Mg(OH)2 is much smaller than that of MgCO3, so sufficient OH- can be supplemented by flotation agents with buffering effects). - Instead of adding excessive CO3 2- To adjust Mg 2+ (The modification effect is better and more selective); at the same time, the use of buffer flotation agents can effectively balance CO3 during the grinding and dissociation process. 2- OH - The effects on different minerals can help avoid the negative impact of adding excessive anions during grinding and dissociation, which inhibits the target mineral; 2) Utilizing OH- -The buffer modification system can rapidly replenish OH adsorbed on the mineral surface. - Or free OH consumed by dissolving Si - And helps to achieve OH under low alkalinity conditions. - The purpose is to rapidly dissolve Si or scrub the mineral surface, thereby increasing the OH content. - Process efficiency of modified spodumene mineral surfaces; 3) Based on buffered OH - The separation system can effectively improve the activation of Mg metal ions. 2+ / Ca 2+ The activation and adsorption effects of OH groups, and the stable OH groups - The environment allows metal ions to be more selectively and directionally adsorbed onto the active sites on the surface of spodumene minerals, reshaping a more stable and denser metal ion activation layer, which is more conducive to its mineralization and collection. Through the coupling effect of the above processes, the efficiency and selectivity of mineral surface modification are effectively improved, thus greatly enhancing the flotation separation efficiency of spodumene minerals and gangue minerals. In addition to the above-mentioned effects of improving the efficiency and selectivity of mineral surface modification, the solution buffer combination of the present invention also has the following effects: optimizing and stabilizing the solution state of the mineralized slurry, promoting the collector to be in the high segregation and high activity range, thereby effectively improving the collector's mineral-collecting activity and reducing collector reagent consumption; stabilizing and strengthening the selective modification of the surface properties of fine-grained minerals (fine mud) by the modifier, thereby improving the dispersion and agglomeration adsorption state of fine mud, reducing the influence of fine mud on mineral flotation separation, and improving separation efficiency; forming relatively stable mineral processing reclaimed water, reducing impurities and noise in the reclaimed water, enhancing the applicability of reclaimed water recycling, and improving the utilization efficiency of reclaimed water. Detailed Implementation
[0047] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0048] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0049] Example 1
[0050] A pegmatite-type spodumene mine in Jiangxi Province has a Li₂O content of 1.15% in its raw ore. Among the lithium-bearing minerals, 87% is spodumene, and the gangue minerals mainly include quartz, feldspar, mica, kaolinite, and chlorite. Moreover, the spodumene particles in the ore are unevenly distributed in terms of coarse and fine sizes. The lithium distribution rate of the product with coarse particles (>1mm) is 40%, while the lithium distribution rate of the product with fine particles (<0.05mm) is 35%.
[0051] This embodiment provides a flotation method for spodumene mineral, wherein the flotation pulp temperature is 24℃-26℃, for the flotation recovery of spodumene from the above-mentioned ore, specifically including the following steps:
[0052] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed to the feed size for grinding using a jaw crusher-cone crusher to obtain crushed mineral material with a maximum particle size of 2mm;
[0053] (2) Grinding treatment: Add tap water and grinding modifier to the crushed mineral material in step (1) and grind it with a ball mill until the content of the material fineness of -0.074mm accounts for 80%, to obtain grinding slurry. Tap water is added to adjust the concentration of the grinding slurry to 66.7%. The amount of grinding modifier is 6500g / t based on the dry ore of spodumene. The grinding modifier is composed of solution buffer combination agent (5000g / t sodium borate + 500g / t hydrochloric acid) and unavoidable metal ion modifier (1000g / t sodium carbonate). The concentration of sodium borate in the slurry is 0.03mol / L and the concentration of hydrochloric acid in the slurry is 0.025mol / L, in order to stabilize the ionic state of the solution in the flotation separation process.
[0054] (3) Preparation of grinding slurry flotation: Add water to the grinding slurry from step (2) to adjust the slurry concentration to 35%, then add sodium hydroxide at a concentration of 400 g / t based on the dry spodumene ore, so as to achieve a high free OH- concentration. -Selective alkali dissolution of the mineral surface was performed, followed by stirring and activation of the mineral surface. The stirring reaction time was 15 minutes, and the resulting slurry was obtained after the reaction. After the activation and dissolution reaction, 1000 g / t of a solution buffer combination (0.18 times the amount of solution buffer combination used in the grinding process) was added, and the mixture was stirred for 5 minutes to stabilize the buffer solution and optimize the effectiveness of the reagents, resulting in an adjusted slurry. Then, 500 g / t of calcium chloride was added to the stabilized slurry as a metal ion activator, and the mineral surface was activated with metal ions for 20 minutes, resulting in an ion-activated slurry. Then, 300 + 100 + 30 g / t of sodium oleate + benzoyl hydroxamic acid + MIBC (a foaming agent was added here because sodium oleate and benzoyl hydroxamic acid, both collectors, have low foaming properties) was added as a selective collector and foaming agent for spodumene minerals, based on the dry ore measurement of spodumene minerals, and the spodumene minerals were stirred and mineralized for 5 minutes, resulting in a mineralized separated slurry.
[0055] (4) Lithium mineral flotation separation and recovery: The mineralized slurry (pH=7.6) after step (3) was selectively separated and separated using a combination of one roughing-three cleaning-one scavenging process. The separation time for each stage of roughing was 4 min, the separation time for each stage of cleaning was 3 min, and the separation time for each stage of scavenging was 4 min. The resulting spodumene concentrate and flotation tailings were concentrated and filtered to obtain and recover spodumene concentrate and flotation tailings. The Li2O recovery rate in the obtained concentrate was 84.5%, and the Li2O grade was 6.04%.
[0056] Example 2
[0057] For the low-temperature separation (8℃-15℃) of oxidized minerals, the technology of this invention shows a significant comparative advantage, with high lithium recovery rate and good concentrate grade obtained during low-temperature flotation.
[0058] A pegmatite-type spodumene deposit in Xinjiang has a Li2O content of 1.45% in its raw ore. Of this, 96% of the lithium-bearing minerals are spodumene, and the gangue minerals mainly include quartz, feldspar, and mica. Some of the spodumene minerals have a relatively fine grain size. The mining area is located in a low-temperature and cold region, and the pulp temperature is not high throughout the year. The existing flotation technology has poor low-temperature separation performance.
[0059] This embodiment provides a flotation method for spodumene mineral to recover spodumene from the above-mentioned ore, specifically including the following steps:
[0060] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed to the feed size of grinding using a jaw crusher-roll crusher method to obtain crushed mineral material with a maximum particle size of 2mm.
[0061] (2) Grinding treatment: Add tap water and grinding modifier to the crushed mineral material in step (1) and grind it with a ball mill until the content of the material fineness of -0.074mm accounts for 70%, and obtain grinding slurry. Among them, tap water is added to adjust the concentration of grinding slurry to 55.5%. Based on the dry ore of spodumene, the amount of grinding modifier is 5600g / t. The grinding modifier is composed of solution buffer combination agent (4000g / t trihydroxymethylaminomethane + 1000g / t hydrochloric acid) and unavoidable metal ion modifier (600g / t sodium hydroxide). Among them, the concentration of trihydroxymethylaminomethane in the slurry is 0.08mol / L, and the concentration of hydrochloric acid in the slurry is 0.08mol / L, in order to stabilize-buffer-modify the ionic state of the solution in the flotation separation process.
[0062] (3) Preparation of grinding slurry flotation: Add water to the grinding slurry from step (2) to adjust the slurry concentration to 28%, then add ammonia water at a concentration of 1000 g / t based on the dry spodumene ore, with highly free OH- - Selective alkali etching of the mineral surface was performed, followed by stirring and activation of the mineral surface. The stirring reaction time was 20 minutes, and the resulting etched slurry was obtained. After the activation and etching reaction, 1500 g / t of a solution buffer combination (0.3 times the amount used in the grinding process) was added, and the mixture was stirred for 5 minutes to stabilize the buffer solution and optimize the effectiveness of the reagents, resulting in an adjusted slurry. Then, 500 g / t of magnesium chloride was added to the stabilized slurry as a metal ion activator, and the mineral surface was activated for 20 minutes to obtain an ion-activated slurry. Finally, 100 + 200 + 100 g / t of naphthenic acid soap + α-amino acid + dodecylamide (measured according to dry spodumene ore) was added as a spodumene mineral collector, and the mixture was stirred and mineralized for 5 minutes to obtain a mineralized separated slurry.
[0063] (4) Lithium mineral flotation separation and recovery: The mineralized slurry (pH=8.0) after step (3) was selectively separated and separated using a combination of one roughing-three cleaning-one scavenging process. The separation time for each stage of roughing was 3 minutes, the separation time for each stage of cleaning was 3 minutes, and the separation time for each stage of scavenging was 3 minutes. The resulting spodumene concentrate and flotation tailings were concentrated and filtered to obtain and recover spodumene concentrate and flotation tailings. The Li2O recovery rate in the obtained concentrate was 83.2%, and the Li2O grade was 6.19%.
[0064] Example 3
[0065] The difference between this embodiment and Embodiment 2 is that the flotation pulp temperature is 24℃-26℃, while other conditions are the same as in Embodiment 2. The Li2O recovery rate in the concentrate obtained in this embodiment is 85.7%, and the Li2O grade is 5.92%.
[0066] Example 4
[0067] For the low-temperature separation (8℃-15℃) of oxidized minerals, the technology of this invention shows a significant comparative advantage, with high lithium recovery rate and good concentrate grade obtained during low-temperature flotation.
[0068] A pegmatite-type spodumene deposit in Xinjiang has a Li2O content of 1.45% in its raw ore. Of this, 96% of the lithium-bearing minerals are spodumene, and the gangue minerals mainly include quartz, feldspar, and mica. Some of the spodumene minerals have a relatively fine grain size. The mining area is located in a low-temperature and cold region, and the pulp temperature is not high throughout the year. The existing flotation technology has poor low-temperature separation performance.
[0069] This embodiment provides a flotation method for spodumene mineral to recover spodumene from the above-mentioned ore, specifically including the following steps:
[0070] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed to the feed size of grinding using a jaw crusher-roll crushing method to obtain crushed mineral material with a maximum particle size of 1mm.
[0071] (2) Grinding treatment: Add tap water and grinding modifier to the crushed mineral material in step (1) and grind it with a ball mill until the content of the material fineness of -0.074mm accounts for 95%, and obtain grinding slurry. Tap water is added to adjust the concentration of the grinding slurry to 55.5%. The amount of grinding modifier is 10000g / t based on the dry ore of spodumene. The grinding modifier is composed of a solution buffer combination (4000g / t tris(hydroxymethyl)aminomethane + 6000g / t hydrochloric acid) and an unavoidable metal ion modifier (100g / t sodium bicarbonate). The concentration of tris(hydroxymethyl)aminomethane in the slurry is 0.08mol / L and the concentration of hydrochloric acid in the slurry is 0.48mol / L, in order to stabilize the ionic state of the solution in the flotation separation process.
[0072] (3) Preparation of grinding slurry flotation: Add water to the grinding slurry from step (2) to adjust the slurry concentration to 25%, then add ammonia water at a concentration of 2000 g / t based on the dry spodumene ore, with highly free OH- -Selective alkali dissolution of mineral surfaces is performed, followed by stirring and activation of the mineral surface. The stirring reaction time is 10 minutes, and the resulting slurry is obtained after the reaction. After the activation and dissolution reaction, 5000 g / t of a solution buffer combination (0.5 times the amount used in the grinding process) is added, and the mixture is stirred for 5 minutes to stabilize the buffer solution and optimize the effectiveness of the reagents, resulting in an adjusted slurry. Then, 1000 g / t of ferric chloride is added to the stabilized slurry as a metal ion activator, and the mineral surface is activated for 10 minutes to obtain an ion-activated slurry. Finally, 25 + 50 + 25 g / t of naphthenic acid soap + α-amino acid + dodecylamine (measured according to the dry ore of spodumene) is added as a spodumene mineral collector, and the spodumene mineral is stirred and mineralized for 10 minutes to obtain a mineralized separated slurry.
[0073] (4) Lithium mineral flotation separation and recovery: The mineralized slurry (pH=7.8) after step (3) was selectively separated and separated using a combination of one roughing-three cleaning-one scavenging process. The separation time for each stage of roughing was 6 min, the separation time for each stage of cleaning was 2 min, and the separation time for each stage of scavenging was 3 min. The resulting spodumene concentrate and flotation tailings were concentrated and filtered to obtain and recover spodumene concentrate and flotation tailings. The Li2O recovery rate in the obtained concentrate was 83.2%, and the Li2O grade was 6.19%.
[0074] Example 5
[0075] For the low-temperature separation (8℃-15℃) of oxidized minerals, the technology of this invention shows a significant comparative advantage, with high lithium recovery rate and good concentrate grade obtained during low-temperature flotation.
[0076] A pegmatite-type spodumene deposit in Xinjiang has a Li2O content of 1.45% in its raw ore. Of this, 96% of the lithium-bearing minerals are spodumene, and the gangue minerals mainly include quartz, feldspar, and mica. Some of the spodumene minerals have a relatively fine grain size. The mining area is located in a low-temperature and cold region, and the pulp temperature is not high throughout the year. The existing flotation technology has poor low-temperature separation performance.
[0077] This embodiment provides a flotation method for spodumene mineral to recover spodumene from the above-mentioned ore, specifically including the following steps:
[0078] (1) Crushing process: The above-mentioned spodumene ore raw material is crushed to the feed size of grinding using a jaw crusher-roll crushing method to obtain crushed mineral material with a maximum particle size of 12mm.
[0079] (2) Grinding treatment: Add tap water and grinding modifier to the crushed mineral material in step (1) and grind it with a ball mill until the content of the material fineness of -0.074mm accounts for 50%, to obtain grinding slurry. Tap water is added to adjust the concentration of the grinding slurry to 55.5%. The amount of grinding modifier is 8000g / t based on the dry ore of spodumene. The grinding modifier is composed of a solution buffer combination (4000g / t trihydroxymethylaminomethane + 1000g / t hydrochloric acid) and an unavoidable metal ion modifier (4000g / t potassium carbonate). The concentration of trihydroxymethylaminomethane in the slurry is 0.08mol / L, and the concentration of hydrochloric acid in the slurry is 0.08mol / L, in order to stabilize the ionic state of the solution in the flotation separation process.
[0080] (3) Preparation of grinding slurry flotation: Add water to the grinding slurry from step (2) to adjust the slurry concentration to 50%, then add sodium hydroxide at a concentration of 100 g / t based on the dry spodumene ore, so as to achieve a high free OH- concentration. - Selective alkali etching of the mineral surface was performed, followed by stirring and activation of the mineral surface. The stirring reaction time was 30 minutes, and the resulting etched slurry was obtained after the reaction. After the activation and etching reaction, 1200 g / t of a solution buffer combination (0.3 times the amount of solution buffer combination used in the grinding process) was added, and the mixture was stirred for 5 minutes to stabilize the buffer solution and optimize the effectiveness of the reagents, resulting in an adjusted slurry. Then, 50 g / t of magnesium chloride was added to the stabilized slurry as a metal ion activator, and the mineral surface was activated with metal ions for 30 minutes, resulting in an ion-activated slurry. Finally, 1000 + 2000 + 1000 g / t of oxidized paraffin soap + α-amino acid + dodecylamide, measured according to the dry ore of spodumene, was added as a combined collector for spodumene minerals, and the spodumene minerals were stirred and mineralized for 2 minutes, resulting in a mineralized separated slurry.
[0081] (4) Lithium mineral flotation separation and recovery: The mineralized slurry (pH=7.8) after step (3) was selectively separated and separated using a combination of one roughing-three cleaning-one scavenging process. The separation time for each stage of roughing was 3 min, the separation time for each stage of cleaning was 4 min, and the separation time for each stage of scavenging was 6 min. The resulting spodumene concentrate and flotation tailings were concentrated and filtered to obtain and recover spodumene concentrate and flotation tailings. The Li2O recovery rate in the obtained concentrate was 83.2%, and the Li2O grade was 6.19%.
[0082] Example 6
[0083] The difference between this embodiment and Example 2 is that the solution buffer combination (trihydroxymethylaminomethane + hydrochloric acid in a molar ratio of 1:1) is replaced with perboric acid + hydrochloric acid + sodium hydroxide in a molar ratio of 1:1:0.15. The concentration of perboric acid in the grinding slurry is 0.08 mol / L, the pH of the separated slurry after mineralization is 7.8, and other conditions are the same as in Example 2. The Li2O recovery rate in the concentrate obtained in this embodiment is 83.2%, and the Li2O grade is 6.07%.
[0084] Example 7
[0085] The difference between this embodiment and Example 2 is that the solution buffer combination (trihydroxymethylaminomethane + hydrochloric acid in a molar ratio of 1:1) is replaced with potassium dihydrogen phosphate + disodium hydrogen phosphate in a molar ratio of 1:4. The concentration of potassium dihydrogen phosphate in the grinding slurry is 0.03 mol / L, the pH of the separated slurry after mineralization is 7.7, and other conditions are the same as in Example 2. The Li2O recovery rate in the concentrate obtained in this embodiment is 82.8%, and the Li2O grade is 6.12%.
[0086] Example 8
[0087] The difference between this embodiment and Example 2 is that the solution buffer combination (trihydroxymethylaminomethane + hydrochloric acid in a molar ratio of 1:1) is replaced with potassium dihydrogen phosphate + sodium hydroxide in a molar ratio of 1:0.9. The concentration of potassium dihydrogen phosphate in the grinding slurry is 0.08 mol / L, the pH of the separated slurry after mineralization is 7.8, and other conditions are the same as in Example 2. The Li2O recovery rate in the concentrate obtained in this embodiment is 83.1%, and the Li2O grade is 6.08%.
[0088] Example 9
[0089] The difference between this embodiment and Example 2 is that the solution buffer combination (trihydroxymethylaminomethane + hydrochloric acid in a molar ratio of 1:1) is replaced with ammonium chloride + ammonia in a molar ratio of 1:0.7. The concentration of potassium dihydrogen phosphate in the grinding slurry is 0.7 mol / L, the pH of the separated slurry after mineralization is 7.8, and other conditions are the same as in Example 2. The Li2O recovery rate in the concentrate obtained in this embodiment is 83.1%, and the Li2O grade is 6.10%.
[0090] Comparative Example 1
[0091] The difference between this comparative example and Example 1 is that no solution buffer was added during the grinding process and after the alkaline etching process. Only 1000 g / t sodium carbonate was added during the grinding process, 400 g / t sodium hydroxide was used in the alkaline etching process, and 500 g / t calcium chloride was used in the ion activation process. Subsequently, sodium oleate + benzoic acid + MIBC = 600 + 200 + 60 g / t was added for mineralization and flotation separation (separation pulp pH = 10.3). Other conditions were the same as in Example 1. The Li2O recovery rate in the obtained concentrate was 76.5%, and the Li2O grade was 5.64%.
[0092] Comparative Example 2
[0093] The difference between this comparative example and Example 2 is that no solution buffer was added during the grinding process and after the alkaline etching process. Only 600 g / t sodium hydroxide was added during the grinding process, 1000 g / t of ammonia was used in the alkaline etching process, and 500 g / t of calcium chloride was used in the ion activation process. Subsequently, naphthenic acid soap + α-amino acid + dodecylamide = 100 + 200 + 100 g / t was added for mineralization and flotation separation (separation pulp pH = 10.3). Other conditions were the same as in Example 1. The Li2O recovery rate in the obtained concentrate was 74.7%, and the Li2O grade was 5.72%.
[0094] Comparative Example 3
[0095] The difference between this comparative example and Example 2 is that no solution buffer was added during the grinding process and after the alkaline etching treatment. Only the same amount of sodium lignosulfonate was added during the grinding process, and the final separated slurry pH was 8.5. Other conditions were the same as in Example 2. The Li2O recovery rate in the concentrate obtained in this comparative example was 65.8%, and the Li2O grade was 5.78%.
[0096] Comparative Example 4
[0097] The difference between this comparative example and Example 2 is that no solution buffer was added during the grinding process and after the alkaline etching treatment. However, a solution buffer was used during the mineralization process to adjust the pH of the separating slurry to 8.0. Other conditions were the same as in Example 2. The concentrate obtained in this comparative example had a Li2O recovery rate of 70.3% and a Li2O grade of 5.61%.
[0098] Comparative Example 5
[0099] The difference between this comparative example and Example 1 is that no solution buffering agent was added during the grinding process and after the alkaline etching process. In the mineralization process, a solution buffering agent was used to adjust the pH of the sorting slurry to 7.6. Other conditions were the same as in Example 1. The Li2O recovery rate in the obtained concentrate was 78.2%, and the Li2O grade was 5.62%.
[0100] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A flotation method for spodumene minerals, characterized in that, include: The spodumene ore to be sorted is crushed to obtain crushed mineral materials; Water is added to crushed mineral materials and the materials are ground to dissociate the minerals. A grinding modifier is added during the grinding process to obtain a grinding slurry. The grinding slurry is conditioned and then highly active OH groups are added sequentially. - The process involves alkaline etching with a modifier, ion activation with a metal ion activator, and finally mineralization with a spodumene mineral collector followed by flotation separation to obtain spodumene concentrate and flotation tailings. The flotation separation is carried out at a pulp temperature of 8℃-15℃. The highly active OH... - The modifier is at least one of sodium hydroxide, potassium hydroxide, and ammonia water; The grinding modifier includes a solution buffer combination and an unavoidable metal ion modifier; the unavoidable metal ion modifier is a carbonate and / or bicarbonate. The solution buffering agent is an adjuster that can adjust the pH of the slurry to the range of 7.5-9.0; the solution buffering agent is a combination of tris(hydroxymethyl)aminomethane and hydrochloric acid.
2. The flotation method according to claim 1, characterized in that, The maximum particle size of the crushed mineral material is 1-12 mm; And / or, the grinding process is performed to achieve a mineral fineness of -0.074 mm, with the content of minerals ranging from 50% to 95%.
3. The flotation method according to claim 1 or 2, characterized in that, The unavoidable metal ion adjuster is at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate. And / or, the mass ratio of the solution buffer combination and the unavoidable metal ion adjuster is (1-100):1, wherein, based on the weight of 1 t of dry spodumene ore to be separated, the amount of the solution buffer combination is 100-80000 g / t, and the amount of the unavoidable metal ion adjuster is 100-4000 g / t. And / or, the mass concentration of the grinding slurry is 50-85%.
4. The flotation method according to claim 1, characterized in that, In the tris(hydroxymethyl)aminomethane + hydrochloric acid combination, the molar ratio of tris(hydroxymethyl)aminomethane to hydrochloric acid is 1:(1-10), and the concentration of tris(hydroxymethyl)aminomethane in the grinding slurry is 0.08-0.1 mol / L.
5. The flotation method according to claim 1, characterized in that, The mass concentration of the slurry after the slurry conditioning treatment is 25%-50%; And / or, based on a weight of 1 t of dry spodumene ore to be sorted, the highly active OH... - The dosage of the modifier is 100-2000 g / t; And / or, the duration of the alkaline etching treatment is 10-30 min; And / or, after the alkaline etching treatment, a solution buffering agent of 0.18-0.5 times the amount of solution buffering agent used in the grinding treatment is added.
6. The flotation method according to claim 1, characterized in that, The metal ion activator is at least one of calcium chloride, magnesium chloride, ferric chloride, magnesium sulfate, manganese sulfate, sodium nitrate, and potassium nitrate. And / or, based on the weight of 1 t of dry spodumene ore to be sorted, the amount of the metal ion activator is 50-1000 g; And / or, the duration of the ion activation treatment is 10-30 min.
7. The flotation method according to claim 1, characterized in that, The spodumene mineral collector is at least one selected from the following: oxidized paraffin soap, naphthenic acid soap, sodium oleate, oleic acid, dodecylamine, tetradecylamine, benzohydroxyoxime acid, salicylic acid, alkyl amino acids, and alkyl amides. And / or, based on a weight of 1 t of dry spodumene ore to be sorted, the amount of spodumene mineral collector used is 100-4000 g / t.
8. The flotation method according to claim 1, characterized in that, A foaming agent is also added during the mineralization process; And / or, the duration of the mineralization treatment is 2-10 min.
9. The flotation method according to claim 1, characterized in that, The flotation separation adopts a mineral flotation process combining roughing, cleaning, and scavenging. And / or, the flotation separation is followed by concentration and compression.
Citation Information
Patent Citations
Derestraining activating agent for cassiterite flotation and preparation method and application thereof
CN113058749A