A method for making metal graphics

By designing the layout of the target pattern and compensation pattern during electron beam exposure, and using the preset exposure dose for regional exposure, a gently sloped mask layer is formed, which solves the problem of low duty cycle pattern transfer distortion and achieves high fidelity. The preparation of metal patterns provides an application basis for electron beam exposure technology.

CN118244570BActive Publication Date: 2024-10-22SHANGHAI INST OF MICROSYSTEM & INFORMATION TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410676373.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-29
Publication Date
2024-10-22
Estimated Expiration
2044-05-29

AI Technical Summary

Technical Problem

In the existing technology, electron beam exposure has limited dose modulation capabilities for deep sub-micron patterns with low duty cycles, and cannot effectively correct the problem of pattern transfer distortion in corner areas.

Method used

In the electron beam exposure, by designing the layout of the target pattern and the compensation pattern, using the first preset exposure dose and the second preset exposure dose to perform regional exposure on the target pattern and the compensation pattern respectively, forming a gently sloped mask layer, and then Form high-fidelity metal graphics.

Benefits of technology

It achieves high-fidelity transfer of graphics with low duty cycle and corners, avoids complex proximity effect calculations, improves the shape accuracy of graphics, and provides electron beam exposure technology in fields such as topological lasers and new superconducting quantum devices. Provides application foundation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118244570B_ABST
    Figure CN118244570B_ABST
Patent Text Reader

Abstract

The present invention provides a method for making a metal pattern, which comprises the following steps: using a layout design tool to make a layout including at least one target pattern and a compensation pattern, the target pattern including at least one corner, the compensation pattern being located at the periphery of each corner of the target pattern, and introducing the layout into an electron beam exposure system; providing a substrate, forming an electron beam resist layer on the upper surface of the substrate, and then placing the substrate in an electron beam exposure system; performing regional exposure on the target pattern and the corresponding area of ​​the compensation pattern with a first and a second preset exposure dose, respectively, and developing the exposed electron beam resist layer to form a mask layer with a pattern; forming a metal layer covering the mask layer; and removing the metal layer and the mask layer covering the upper surface of the mask layer. The present invention belongs to the field of electron beam lithography technology, and uses the compensation pattern area to perform exposure with a second preset exposure dose to compensate for the exposure dose of the target pattern area, thereby realizing high-fidelity pattern transfer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electron beam lithography and relates to a method for manufacturing a metal pattern. Background Art

[0002] Electron beam lithography has been widely used in submicron, deep submicron and nanostructure processing due to its advantages such as high resolution, high precision and no need for masks. It is the best choice for current micro-nano device research and small-batch manufacturing.

[0003] In electron beam exposure, the proximity effect is caused by forward scattering and back scattering of high-energy electron beams when incident on electron beam resists and substrates, resulting in deviations in the size and shape of the exposed graphics. In response to this, people usually use the point spread function (PSF) model to correct the proximity effect. In order to reduce the complexity of the calculation, the commonly used commercial proximity effect correction software uses function approximation when describing the electron beam energy distribution function and solving the integral equation. This method is suitable for correcting the proximity effect between graphics and within graphics in electron beam exposure of micron-level graphics or dense graphics. However, for deep submicron and low duty cycle square graphics exposure, on the one hand, the calculation error of using function approximation is large, and the given dose modulation cannot effectively correct the deviations in size and shape caused by the proximity effect; on the other hand, for low duty cycle graphics, the proximity effect between adjacent graphics is very weak, mainly the proximity effect within the graphics. When the graphics size is further reduced to submicron size, the current commonly used commercial software cannot effectively perform exposure dose correction within the graphics. For example, when commercial software performs dose correction for a square array with a side length of 200nm, when the duty cycle reaches less than 10%, the calculated dose stratification has only one layer, that is, the square graphic area is exposed with the same dose, then the corner area of ​​the square graphic can only superimpose 1 / 4 of the scattered energy in the middle area, and the side can superimpose 1 / 2 of the scattered energy in the middle area. This uneven energy deposition in a single dose exposure causes the four corners of the exposed square graphic to have obvious arc features, such as Figure 1 The figure shows a scanning electron microscope (SEM) image of a 200 nm square pattern made based on a layout corrected by proximity effect software, including substrate 01 and square pattern 02. The smaller the pattern size, the more obvious the arc degree. When the scale is reduced to the nanometer scale, the exposed pattern even becomes a circle. If this distorted glue pattern is used as a mask for pattern transfer, it is impossible to obtain a square pattern with high fidelity on the substrate.

[0004] Therefore, there is an urgent need to find a method for producing a metal pattern that can achieve high-fidelity transfer of a low-duty-cycle pattern with a corner. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for producing a metal pattern, which is used to solve the problem that the current proximity effect correction software in the prior art has limited dose modulation capability for deep submicron patterns with low duty cycle and cannot solve the problem of pattern transfer distortion in corner areas.

[0006] To achieve the above object and other related objects, the present invention provides a method for making a metal pattern, comprising the following steps:

[0007] Using a layout design tool to create a layout including at least one target pattern and a compensation pattern, wherein the target pattern includes at least one corner, and the compensation pattern is at least located at the periphery of each corner of the target pattern and adjacent to the target pattern, and the layout is introduced into an electron beam exposure system;

[0008] Providing a substrate, forming an electron beam resist layer with a preset thickness on the upper surface of the substrate, and then placing the substrate in the electron beam exposure system;

[0009] Performing regional exposure on the electron beam resist layer regions corresponding to the target pattern and the compensation pattern with a first preset exposure dose and a second preset exposure dose, respectively, and developing the exposed electron beam resist layer to form a mask layer having a pattern whose bottom surface exposes the substrate, wherein the first preset exposure dose is greater than the second preset exposure dose, and the dose value of the second preset exposure dose gradually decreases from an edge adjacent to the region corresponding to the target pattern in a direction away from the region corresponding to the target pattern, and a top region of a side wall of the pattern in the mask layer is gently sloped;

[0010] forming a metal layer covering the upper surface of the mask layer and the metal layer on the upper surface of the substrate where the pattern is exposed based on the patterned mask layer;

[0011] The metal layer covering the upper surface of the mask layer and the mask layer are removed to obtain a target metal pattern.

[0012] Optionally, the layout design tools include L-edit and GDSⅡ.

[0013] Optionally, before importing the layout into the electron beam exposure system, the method further includes using the layout design tool to convert the file format of the layout into a file format corresponding to the electron beam exposure system.

[0014] Optionally, the duty cycle of the target pattern ranges from 1% to 20%.

[0015] Optionally, a minimum ratio of a size of an edge of the compensation pattern adjacent to a corner of the target pattern relative to the edge of the target pattern increases as a size of the target pattern decreases.

[0016] Optionally, the substrate is made of insulating material, and before forming the electron beam anti-etching layer on the upper surface of the substrate, a conductive layer is formed on the upper surface of the substrate.

[0017] Optionally, the material of the substrate is one of Si, SiO2 / Si, Si3N4 / Si, MgO, and sapphire.

[0018] Optionally, the metal layer is formed by magnetron sputtering, electron beam evaporation, and thermal evaporation.

[0019] Optionally, the bottom of the sidewall of the pattern in the mask layer is vertical, and the height h of the vertical region is in the range of 100 nm to 300 nm.

[0020] Optionally, the thickness of the metal layer is not greater than the height h of the vertical region of the sidewall of the pattern.

[0021] As described above, the method for making a metal pattern of the present invention improves the electron beam etching process to make the compensation pattern at the periphery of the corner in the target pattern. During the exposure process, the corresponding area of ​​the target pattern is exposed with the first preset exposure dose, and the corresponding area of ​​the compensation pattern is exposed with the second preset exposure dose that is smaller than the first preset exposure dose, and the second preset exposure dose gradually decreases from the edge where the compensation pattern is adjacent to the corresponding area of ​​the target pattern in the direction away from the corresponding area of ​​the target pattern, so as to compensate the exposure dose of the corresponding area at the corner of the target pattern by exposing the corresponding area of ​​the compensation pattern, and at the same time, the corresponding area of ​​the compensation pattern in the mask layer is gently sloped, so as to avoid the metal layer covering the corresponding area of ​​the compensation pattern affecting the shape of the target metal pattern, thereby improving the fidelity of the target metal pattern formed subsequently, without the need for complex proximity effect calculation, and using this method, the preparation of patterns with low duty cycle and corners can be achieved, laying a foundation for the application of electron beam exposure technology in topological lasers, new superconducting quantum devices, etc., and having high industrial utilization value. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Shown is a SEM image of a 200 nm square pattern made based on a layout corrected by proximity effect software.

[0023] Figure 2 Shown is a process flow chart of the method for making the metal pattern of the present invention.

[0024] Figure 3 Shown is a partial structural schematic diagram of a layout of a method for making a metal pattern of the present invention.

[0025] Figure 4 The cross-sectional structure schematic diagram of the substrate of the method for manufacturing the metal pattern of the present invention is shown.

[0026] Figure 5 It is a schematic diagram showing the cross-sectional structure after forming an electron beam resist layer in the method for producing a metal pattern of the present invention.

[0027] Figure 6 It is a schematic diagram showing the cross-sectional structure after forming a patterned mask layer in the method for manufacturing a metal pattern of the present invention.

[0028] Figure 7 Display as Figure 6 Schematic diagram of the structure at section aa of the middle structure.

[0029] Figure 8 Display as Figure 6 Schematic diagram of the structure at section bb in the middle structure.

[0030] Fig. 9 It is a schematic diagram showing the cross-sectional structure after forming a metal layer in the method for manufacturing a metal pattern of the present invention.

[0031] Fig.10 It is a schematic diagram showing the cross-sectional structure after forming a target metal pattern in the method for producing a metal pattern of the present invention.

[0032] Fig.11 Shown is a SEM image of a target metal pattern produced by the method for producing a metal pattern of the present invention.

[0033] Explanation of the accompanying drawings: 01 substrate, 02 square pattern, 1 layout, 11 target pattern, 12 compensation pattern, 2 substrate, 3 electron beam resist layer, 31 mask layer, 32 pattern, 4 metal layer, 41 target metal pattern. DETAILED DESCRIPTION

[0034] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0035] See also Figures 2 to 11It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0036] This embodiment provides a method for making a metal pattern, such as Figure 2 FIG. 1 is a process flow chart of the method for making the metal pattern, which includes the following steps:

[0037] S1: using a layout design tool to create a layout including at least one target pattern and a compensation pattern, wherein the target pattern includes at least one corner, and the compensation pattern is at least located at the periphery of each corner of the target pattern and is adjacent to the target pattern, and the layout is introduced into an electron beam exposure system;

[0038] S2: providing a substrate, forming an electron beam resist layer of a preset thickness on the upper surface of the substrate, and then placing the substrate in the electron beam exposure system;

[0039] S3: performing regional exposure on the electron beam resist layer regions corresponding to the target pattern and the compensation pattern with a first preset exposure dose and a second preset exposure dose respectively, and developing the exposed electron beam resist layer to form a mask layer having a pattern whose bottom surface exposes the substrate, wherein the first preset exposure dose is greater than the second preset exposure dose, and the dose value of the second preset exposure dose gradually decreases from an edge adjacent to the region corresponding to the target pattern in a direction away from the region corresponding to the target pattern, and the top region of the side wall of the pattern in the mask layer is gently sloped;

[0040] S4: forming a metal layer covering the upper surface of the mask layer and the metal layer on the upper surface of the substrate where the pattern is exposed based on the patterned mask layer;

[0041] S5: removing the metal layer and the mask layer covering the upper surface of the mask layer to obtain a target metal pattern.

[0042] See also Figures 3 to 5 , perform the step S1 and the step S2: use a layout design tool to produce a layout including at least one target pattern 11 and a compensation pattern 12 Figure 1 The target pattern 11 includes at least one corner, the compensation pattern 12 is at least located at the periphery of each corner of the target pattern 11 and is adjacent to the target pattern 11, and the plate Figure 1An electron beam exposure system is introduced; a substrate 2 is provided, an electron beam resist layer 3 of a preset thickness is formed on the upper surface of the substrate 2, and then the substrate 2 is placed in the electron beam exposure system.

[0043] As an example, the layout design tool includes L-edit, GDSⅡ or other suitable layout making software.

[0044] As an example, Figure 3 As shown, the version Figure 1 A schematic diagram of the local structure of the plate Figure 1 Before the electron beam exposure system is introduced, the layout design tool is used to Figure 1 The step of converting the file format into a file format corresponding to the electron beam exposure system.

[0045] Specifically, different electronic exposure devices in the electron beam exposure system usually correspond to different file formats. For example, when using JEOL's electronic exposure device for exposure, the file format of its layout needs to be converted into a V30 file; when using Elionix's electronic exposure device for exposure, the file format of its layout needs to be converted into a SCON file; when using Raith's electronic exposure device for exposure, the file format of its layout needs to be converted into a GPF file. In this embodiment, the electronic exposure device used in the electron beam exposure system is a JEOL JBX-6300FS electron beam exposure machine.

[0046] As an example, the shape of the target pattern 11 includes a triangle, a quadrilateral, a pentagon or other suitable shapes with corners. In this embodiment, a square is used as the target pattern 11.

[0047] Specifically, the size of the target pattern 11 is within the deep submicron range, that is, the size of the target pattern 11 is not greater than 250 nm. In this embodiment, the side length of the square target pattern 11 is 200 nm.

[0048] As an example, the duty cycle of the target pattern 11 ranges from 1% to 20%. Figure 1 The duty cycle of the target pattern 11 is 20%.

[0049] Specifically, the compensation pattern 12 is used to compensate for the exposure dose of the corresponding area at the corner of the target pattern 11 during the exposure of the electron beam resist layer 3, and does not affect the graphic shape of the corresponding area of ​​the non-corner part of the target pattern 11, thereby avoiding the problem of insufficient exposure dose in the corresponding area at the corner of the target pattern 11 when the electron beam resist layer 3 is subsequently exposed, and at the same time ensuring the fidelity of the pattern obtained after the subsequent transfer of the target pattern.

[0050] Specifically, under the condition that the exposure dose of the corresponding area at the corner of the target pattern 11 is sufficient in the subsequent exposure process, the shape of the compensation pattern 12 can be selected according to the actual situation, and no limitation is given here. In this embodiment, the compensation pattern 12 is a triangular arrow shape located outside the corner of the target pattern 11.

[0051] As an example, the minimum ratio of the size of the edge adjacent to the compensation pattern 12 at the corner of the target pattern 11 to the edge of the target pattern 11 increases as the size of the target pattern 11 decreases, that is, within the range allowed by the process technology, due to the influence of the proximity effect, as the size of the target pattern 11 decreases, the minimum ratio of the edge length shared by the compensation pattern 12 and the target pattern 11 to the edge length at the corner of the target pattern 11 that can achieve minimum exposure dose compensation is larger.

[0052] Specifically, the compensation pattern 12 may also surround the target pattern 11 while ensuring that the compensation pattern 12 can compensate for the exposure dose at the corner of the target pattern 11 and does not affect the non-corner area pattern of the target pattern 11. The corner here refers to the area at the corner affected by the proximity effect, and the non-corner area refers to the area outside the corner of the target pattern.

[0053] Specifically, Figure 4 As shown, it is a schematic diagram of the cross-sectional structure of the substrate 2. The material of the substrate 2 is one of Si, SiO2 / Si, Si3N4 / Si, MgO, sapphire, or other suitable materials. Here, SiO2 / Si and Si3N4 / Si refer to a laminated substrate structure composed of two material film layers. In this embodiment, a Si substrate is used as the substrate 2.

[0054] Specifically, under the condition of ensuring the quality of the target metal pattern to be formed subsequently, the thickness, shape and size of the substrate 2 can be selected according to actual conditions, and are not limited here.

[0055] Specifically, Figure 5 , which is a schematic diagram of the cross-sectional structure after the electron beam resist layer 3 is formed, wherein the electron beam resist layer 3 is a positive electron beam resist film layer, and the electron beam resist includes but is not limited to ZEP520A, ARP6200, and PMMA950A4. In this embodiment, the film layer formed by the ZEP520A electron beam resist is used as the electron beam resist layer 3.

[0056] As an example, the material of the substrate 2 is an insulating material. Before forming the electron beam anti-etching layer 3 on the upper surface of the substrate 2, it also includes the step of forming a conductive layer on the upper surface of the substrate 2, so that the electrons that have not reacted with the electron beam anti-etching layer 3 at the graphic position can be timely discharged, thereby preventing these unreacted electrons from gathering and moving near the exposure graphic, and reacting with the electron beam anti-etching agent around the exposed graphic to affect the exposure effect.

[0057] Specifically, under the condition of ensuring the quality of the mask layer formed subsequently, the thickness and material of the conductive layer formed on the upper surface of the substrate 2 can be selected according to actual conditions, and are not limited here.

[0058] Specifically, the method of forming the electron beam resist layer 3 on the upper surface of the substrate 2 includes coating or other suitable methods.

[0059] Specifically, under the condition of ensuring the quality of the pattern formed after the pattern transfer in the layout, the thickness of the electron beam resist layer 3 can be selected according to the actual situation, and no restriction is made here. In the present embodiment, the substrate 2 is first fixed on the spin coating device, and then a preset amount of electron beam resist ZEP520A is coated on the upper surface of the substrate 2, and then spin coating is performed to make the electron beam resist uniformly distributed on the upper surface of the substrate 2, and the uniform coating speed during the spin coating process is 3500 rpm, the uniform coating time is 45s, and the thickness of the electron beam resist film layer covering the upper surface of the substrate 2 is 600nm. Finally, the substrate 2 with the electron beam resist spin-coated on the upper surface is placed on a hot plate for pre-baking, the baking temperature is 180°C, and the baking time is 5min, so as to dry the electron beam resist covering the substrate 2, and the electron beam resist film layer after drying is used as the electron beam resist layer 3.

[0060] Specifically, the method of placing the substrate 2 with the electron beam resist layer 3 on the upper surface thereof in the electron beam exposure system may be manually placed using auxiliary tools or transferred by mechanized equipment, which will not be described in detail here.

[0061] Please see again Figures 6 to 11, executing the step S3, the step S4 and the step S5: performing regional exposure on the electron beam resist layer 3 corresponding to the target pattern 11 and the compensation pattern 12 with a first preset exposure dose and a second preset exposure dose respectively, and developing the exposed electron beam resist layer 3 to form a mask layer 31 having a pattern 32 whose bottom surface exposes the substrate 2, and the first preset exposure dose is greater than the second preset exposure dose, the dose value of the second preset exposure dose gradually decreases from the edge adjacent to the corresponding area of ​​the target pattern 11 in the direction away from the corresponding area of ​​the target pattern 11, and the top area of ​​the side wall of the pattern 32 in the mask layer 31 is gently sloped; based on the patterned mask layer 31, a metal layer 4 covering the upper surface of the mask layer 31 and the metal layer 4 on the upper surface of the substrate 2 where the pattern 32 is exposed are formed; the metal layer 4 covering the upper surface of the mask layer 31 and the mask layer 31 are removed to obtain a target metal pattern 41.

[0062] Specifically, before starting the electron beam exposure device in the electron beam exposure system, the method further includes: Figure 1 The step of setting the exposure dose is to set the first exposure dose and the second exposure dose in an exposure device.

[0063] Specifically, the dose value of the first exposure dose needs to be comprehensively considered based on the material and thickness of the electron beam resist layer 3 and the electron beam resist contrast curve under the selected exposure and development conditions.

[0064] Specifically, the exposure dose of the area corresponding to the compensation pattern 12 is less than the exposure dose of the area corresponding to the target pattern 11, so as to avoid the area corresponding to the compensation pattern 12 from exposing the bottom surface of the substrate 2 after development, resulting in distortion of the image of the area corresponding to the compensated target pattern 11 after development.

[0065] Specifically, the exposure dose of the compensation pattern 12 area gradually decreases from the edge adjacent to the target pattern 11 to the edge away from the target pattern 11. In this embodiment, before the electron beam resist layer 3 is exposed, the electron beam acceleration voltage is set to 100 kV, the beam current is set to 100 pA, and the exposure dose of the target pattern 11 corresponding area is 600 μC / cm 2 The exposure dose of the area corresponding to the compensation pattern 12 is increased from 300 μC / cm at the adjacent boundary with the area corresponding to the target pattern 11. 2 Decrease to 60 μC / cm at the edge of the compensation pattern 12 away from the corresponding area of ​​the target pattern 11 2 .

[0066] Specifically, during the exposure of the electron beam resist layer 3, affected by the proximity effect, the electron beam resist layer 3 corresponding to the corner of the target graphic 11 is difficult to completely react with electrons, resulting in unreacted electron beam resist remaining at the bottom of the electron beam resist layer 3 corresponding to the corner of the target graphic 11. By exposing the corresponding area of ​​the compensation graphic 12 outside the corner of the target graphic 11, the electron beam resist in the corresponding bottom area at the corner of the target graphic 11 that has not reacted with electrons can be completely reacted with electrons, and because the exposure dose of the corresponding area of ​​the compensation graphic 12 is small, the electron beam resist at the bottom of the corresponding area of ​​the compensation graphic 12 cannot react with electrons, thereby ensuring that the electron beam resist in the corresponding area of ​​the target graphic 11 can completely react with electrons while preventing the electron beam resist at the bottom of the corresponding area of ​​the compensation graphic 12 from reacting with electrons.

[0067] Specifically, Figure 6 , Figure 7 and Figure 8 As shown in the figure, they are schematic diagrams of the structure after the mask layer 31 is formed, Figure 6 Structural diagram of the middle structural section and Figure 6 The schematic diagram of the structure at the cross section of the structure bb in the middle, the development of the electron beam resist layer 3 after exposure comprises the following steps: Figure 1 The exposed sample is placed in a developer for a first preset time; the sample is taken out of the developer and placed in a fixer for a second preset time; the sample is taken out of the fixer and dried. The sample here refers to the substrate 2 with the electron beam resist layer 3 formed on the upper surface.

[0068] Specifically, the developer includes amyl acetate solution, methyl isobutyl ketone-isopropyl alcohol mixed solution, AR600-546 solution or other suitable materials capable of developing the electron beam resist; the first preset time is related to the type, concentration and environment of the developer, and is not limited here. In this embodiment, at room temperature, the exposed electron beam resist layer 3 is placed in the amyl acetate solution for development for 60 s.

[0069] Specifically, the fixing solution includes isopropyl alcohol or other suitable electron beam resist fixing materials; the second preset time is related to the type, concentration and environment of the fixing solution, and is not limited here. In this embodiment, at room temperature, the developed electron beam resist layer 3 is placed in isopropyl alcohol for 60 seconds.

[0070] Specifically, the method for drying the sample after fixing can be selected according to actual conditions while ensuring the quality of the formed mask layer 31. In this embodiment, nitrogen is used to dry the sample after fixing.

[0071] As an example, the bottom of the side wall of the pattern 32 in the mask layer 31 is vertical, and the height h of the vertical region ranges from 100 nm to 300 nm, that is, the side wall of the pattern 32 in the region corresponding to the target graphic 11 is vertical.

[0072] Specifically, since the exposure dose of the area corresponding to the compensation pattern 12 changes gradually, and the exposure dose of the area corresponding to the compensation pattern 12 decreases from the edge adjacent to the area corresponding to the target pattern 11 away from the area corresponding to the target pattern 11, the electron beam resist remaining at the corner of the area corresponding to the target pattern 11 can be completely reacted with the electrons, and the amount of electrons reacting with the electron beam resist from the edge adjacent to the area corresponding to the compensation pattern 12 and the target pattern 11 to the edge of the area corresponding to the compensation pattern 12 away from the area corresponding to the target pattern 11 is less and less, and then the mask layer 31 of the area corresponding to the compensation pattern 12 after development is gently sloped, and the edge adjacent to the area corresponding to the compensation pattern 12 and the target pattern 11 has the electron beam resist layer 3 with a thickness of h. The gentle slope here refers to the morphology from the edge adjacent to the area corresponding to the compensation pattern 12 and the target pattern 11 to the edge area of ​​the area corresponding to the compensation pattern 12 away from the target pattern 11, and the thickness of the electron beam resist layer 3 in this area that reacts with the developer becomes thinner and thinner.

[0073] As an example, Fig. 9 , which is a schematic diagram of the cross-sectional structure after the metal layer 4 is formed, and the method of forming the metal layer 4 is one of magnetron sputtering, electron beam evaporation, thermal evaporation, or other suitable methods. In this embodiment, the developed sample is placed in a magnetron sputtering instrument to deposit the metal layer 4.

[0074] Specifically, the material of the metal layer 4 includes Pt, Au, Cu, Ti, Cr, Nb or other suitable metal materials. In this embodiment, a platinum (Pt) layer is used as the metal layer 4.

[0075] As an example, the thickness of the metal layer 4 is not greater than the height h of the vertical region of the sidewall of the pattern 32, so that the metal layer 4 covering the upper surface of the substrate 2 in the pattern is separated from the metal layer 4 covering the exposed surface of the mask layer 31, which facilitates the subsequent stripping of the metal layer 4 covering the exposed surface of the mask layer 31. In this embodiment, the thickness of the metal layer 4 is 20 nm.

[0076] Specifically, Fig.10As shown in the figure, it is a schematic diagram of the cross-sectional structure after the target metal pattern 41 is formed. Removing the metal layer 4 covering the upper surface of the mask layer 31 and the mask layer 31 includes the following steps: soaking the sample after the metal layer 4 is formed in N-methylpyrrolidone (NMP) at a temperature of 90°C for 30 minutes and then ultrasonically cleaning it for 5 minutes; ultrasonically cleaning it with deionized water, acetone and isopropanol for 5 minutes respectively, so as to peel off and remove the mask layer 31 (that is, the electron beam resist layer 3) and the metal layer 4 covering the exposed surface of the mask layer 31.

[0077] Specifically, after removing the metal layer 4 and the mask layer 31 covering the upper surface of the mask layer 31 , the method further includes a step of inspecting the morphology of the obtained target metal pattern 41 .

[0078] Specifically, the morphology of the target metal pattern 41 is inspected by an auxiliary inspection tool to ensure the quality of the target metal pattern 41 .

[0079] Specifically, Fig.11 As shown, it is a SEM image of the target metal pattern 41. The auxiliary tool for detecting the morphology of the target metal pattern 41 includes a scanning electron microscope or other suitable auxiliary observation equipment. In this embodiment, the quality of the target metal pattern 41 is observed by a scanning electron microscope.

[0080] Specifically, by improving the electron beam etching process, in the production of the plate Figure 1 During the process of exposing the electron beam resist layer 3, the exposure dose of the area corresponding to the compensation pattern 12 is controlled, and the area corresponding to the compensation pattern 12 is exposed with the second preset exposure dose. While exposing, the exposure dose at the corner of the area corresponding to the target pattern 11 is compensated, and the electron beam resist layer 3 of the preset thickness of the bottom layer of the area corresponding to the compensation pattern 12 cannot react with electrons, thereby improving the fidelity of the target metal pattern 41 formed subsequently, and eliminating the need for complex proximity effect calculation.

[0081] Specifically, by making the second exposure dose gradually distributed and gradually decreasing from the edge where the compensation pattern 12 is adjacent to the corresponding area of ​​the target pattern in the direction away from the corresponding area of ​​the target pattern 11, after development, the corresponding area of ​​the compensation pattern 12 in the mask layer 31 is in a gentle slope shape, thereby avoiding the metal layer 4 covering the corresponding area of ​​the compensation pattern 12 from affecting the shape of the target metal pattern 41.

[0082] Specifically, by combining the compensation pattern 12 with the target pattern 11, and then performing normal dose exposure and grayscale exposure on the corresponding areas of the target pattern 11 and the compensation pattern 12 respectively, the preparation of low duty cycle and angled patterns can be achieved, laying the foundation for the application of electron beam exposure technology in topological lasers, new superconducting quantum devices, etc.

[0083] In summary, the method for making metal patterns of the present invention improves the electron beam etching process, and makes compensation patterns at the periphery of the corner of the target pattern in the layout. During the exposure process, the compensation pattern corresponding area is exposed with a second preset exposure dose smaller than the first preset exposure dose, and the second preset exposure dose is gradually reduced from the edge adjacent to the compensation pattern and the target pattern corresponding area along the direction away from the target pattern corresponding area, while realizing the exposure dose compensation of the corresponding area at the corner of the target pattern, the thickness of the electron beam resist layer at the bottom of the compensation pattern corresponding area that cannot react with electrons is gradually increased along the direction away from the target pattern corresponding area, and then the compensation pattern corresponding area in the mask layer is gently sloped, so as to avoid the metal layer covering the corresponding area of ​​the compensation pattern affecting the shape of the target metal pattern, and improve the fidelity of the target metal pattern formed subsequently, without complex proximity effect calculation. In addition, the method can realize the preparation of low duty cycle and cornered patterns, and lay the foundation for the application of electron beam exposure technology in topological lasers, novel superconducting quantum devices, etc. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.

[0084] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for producing a metal pattern, characterized in that: The following steps are involved: Using a layout design tool to create a layout including at least one target pattern and a compensation pattern, wherein the target pattern includes at least one corner, and the compensation pattern is at least located at the periphery of each corner of the target pattern and adjacent to the target pattern, and the layout is introduced into an electron beam exposure system; Providing a substrate, forming an electron beam resist layer with a preset thickness on the upper surface of the substrate, and then placing the substrate in the electron beam exposure system; Performing regional exposure on the electron beam resist layer regions corresponding to the target pattern and the compensation pattern with a first preset exposure dose and a second preset exposure dose, respectively, and developing the exposed electron beam resist layer to form a mask layer having a pattern whose bottom surface exposes the substrate, wherein the first preset exposure dose is greater than the second preset exposure dose, and the dose value of the second preset exposure dose gradually decreases from an edge adjacent to the region corresponding to the target pattern in a direction away from the region corresponding to the target pattern, and a top region of a side wall of the pattern in the mask layer is gently sloped; forming a metal layer covering an upper surface of the mask layer and the metal layer on an upper surface of the substrate where the pattern is exposed based on the patterned mask layer; The metal layer covering the upper surface of the mask layer and the mask layer are removed to obtain a target metal pattern.

2. The method for making a metal pattern according to claim 1, characterized in that: The layout design tools include L-edit and GDSⅡ.

3. The method for making a metal pattern according to claim 1, characterized in that: Before the layout is imported into the electron beam exposure system, the method further includes using the layout design tool to convert the file format of the layout into a file format corresponding to the electron beam exposure system.

4. The method for making a metal pattern according to claim 1, characterized in that: The duty cycle range of the target pattern is 1% to 20%.

5. The method for making a metal pattern according to claim 1, characterized in that: The minimum ratio of the size of the edge of the compensation pattern adjacent to the corner of the target pattern relative to the edge of the target pattern increases as the size of the target pattern decreases.

6. The method for making a metal pattern according to claim 1, characterized in that: The material of the substrate is an insulating material. Before forming the electron beam anti-etching layer on the upper surface of the substrate, a conductive layer is formed on the upper surface of the substrate.

7. The method for making a metal pattern according to claim 1, characterized in that: The material of the substrate is one of Si, SiO2 / Si, Si3N4 / Si, MgO and sapphire.

8. The method for making a metal pattern according to claim 1, characterized in that: The metal layer is formed by magnetron sputtering, electron beam evaporation, and thermal evaporation.

9. The method for making a metal pattern according to claim 1, characterized in that: The bottom of the sidewall of the pattern in the mask layer is vertical, and the height h of the vertical region is in the range of 100 nm to 300 nm.

10. The method for making a metal pattern according to claim 9, characterized in that: The thickness of the metal layer is not greater than the height h of the vertical region of the sidewall of the pattern.