A composite current lead structure based on high temperature superconducting material
By dividing the superconducting magnet current leads into sections A, B and C, and using different materials and structures, the problem that the existing technology cannot meet the current transmission and heat leakage requirements at the same time is solved, and effective control of high-temperature superconducting magnets is achieved. current delivery and temperature management.
Patent Information
- Application Number
- CN202410695023.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-31
AI Technical Summary
Existing superconducting magnet current leads cannot simultaneously meet the needs of current transmission and heat leakage from low to high temperatures. They must use conductive materials with low resistivity and include low thermal conductivity material structures.
A composite current lead structure based on high-temperature superconducting materials is designed. The current lead is divided into segment A, segment B and segment C. Section A uses a base material of high thermal conductivity material to encapsulate the superconducting tape, and segment B uses a base material of low thermal conductivity material. The base and C section adopt high thermal conductivity conventional conductors, which work in different temperature zones respectively, and realize current transmission and thermal management through mechanical connection and welding structure.
Effective current transmission to high-temperature superconducting magnets is achieved while reducing conductive heat to the magnets, meeting transmission current requirements and controlling temperature gradients.
Smart Images

Figure CN118262966B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-temperature superconducting leads, and in particular relates to a composite current lead structure based on high-temperature superconducting materials. Background Art
[0002] The current lead of a superconducting magnet needs to meet two requirements: one is to transmit current, and the other is to reduce the heat leakage from room temperature to low temperature. Therefore, the current lead structure must consider the use of low-resistivity conductive materials and low-thermal conductivity material structures. However, the existing superconducting magnet current leads do not meet the above conditions. Summary of the invention
[0003] In view of the above problems, the present invention provides a composite current lead structure based on high temperature superconducting materials.
[0004] The composite current lead structure based on high temperature superconducting material provided by the present invention comprises: a first section, a second section and a third section.
[0005] The first section includes a superconducting tape encapsulated by a substrate of a high thermal conductivity material;
[0006] The second section comprises a substrate made of a low thermal conductivity material, on which the superconducting tape is fixed;
[0007] The third section adopts a conventional conductor with high thermal conductivity;
[0008] One end of the first section is a low-temperature end, which is used to connect to a high-temperature superconducting magnet, and the other end of the first section is a high-temperature end, which is mechanically connected to one end of the second section;
[0009] The superconducting tape at the other end of the second section is led out and welded to one end of the third section.
[0010] further,
[0011] The substrate of the first section is a thin and long strip structure with a width of 15-25 mm and a height of 5-15 mm;
[0012] A first shallow groove is provided on one surface of the substrate along the length direction of the substrate, the first shallow groove extends from one end of the substrate to the other end, the depth of the first shallow groove is 1-3 mm, the width is 10-20 mm, and the superconducting tape is welded in the first shallow groove along the length direction of the substrate.
[0013] further,
[0014] The base material of the first section is copper or copper alloy;
[0015] The substrate has a width of 20 mm and a height of 10 mm;
[0016] The shallow groove has a depth of 2 mm and a width of 16 mm.
[0017] further,
[0018] The first section of the substrate is provided with a heat exchanger, the heat exchanger is provided with an air inlet and an air outlet, and cold helium gas with a temperature of 20K flows inside the heat exchanger.
[0019] further,
[0020] The base of the second section is an elongated strip structure;
[0021] A second shallow groove is provided on one surface of the substrate of the second section along the length direction of the substrate, the second shallow groove extends from one end of the substrate to the other end, the depth and width of the second shallow groove are the same as those of the first shallow groove, and the superconducting tape is welded in the second shallow groove along the length direction of the substrate;
[0022] The superconducting tape has a width of 5-15 mm, a thickness of 50-100 μm, and a length covering the first section and the second section to one end of the third section;
[0023] The length of the base of the second section does not exceed 700 mm;
[0024] In the mechanical connection between the high temperature end of the first section and one end of the second section, the substrate of the first section and the base of the second section overlap and the contact area is 30×30-70×70 mm 2 .
[0025] further,
[0026] The base material of the second section is stainless steel;
[0027] The superconducting tape is a copper-plated superconducting tape with a width of 10 mm and a thickness of 75 μm, and is also a stacked superconducting tape;
[0028] The length of the base of the second section does not exceed 500 mm;
[0029] The contact area between the first section substrate and the second section substrate is 50×50 mm 2 .
[0030] further,
[0031] The surface of the substrate of the second section is plated with nickel, and the copper-plated superconducting tape is brazed on the surface using 6337 solder.
[0032] further,
[0033] The contact between the substrate of the first section and the base of the second section is fastened with M6 bolts, and the contact is padded with indium sheets.
[0034] further,
[0035] One end of the third section is a square heat exchanger, the width of the square heat exchanger is 50-100 mm, the length is 90-150 mm, and the thickness is 20-40 mm. A flow channel is arranged inside the square heat exchanger, a joint groove is arranged at one end of the square heat exchanger, and the other end of the square heat exchanger is connected to a copper tube, and the copper tube is connected to the flow channel inside the square heat exchanger;
[0036] The end of the superconducting tape led out from the other end of the second section is in a stepped shape, wherein the stacked superconducting tapes are shortened by 15-35 mm from the top layer to the bottom layer, and the end is welded in the joint groove with 6337 solder, and the solder length is 15-35 mm. The superconducting surface of the bottom layer of the stacked superconducting tapes is welded to the bottom of the joint groove, and the top of the top layer of the stacked superconducting tapes is welded to the end wall of the joint groove.
[0037] further,
[0038] The square heat exchanger has a width of 80 mm, a length of 120 mm and a thickness of 30 mm;
[0039] The other end of the square heat exchanger is connected to the copper tube by brazing;
[0040] The stacked superconducting tapes are successively shortened by 25 mm from the top layer to the bottom layer, and the length of the solder is 25 mm;
[0041] The base at the other end of the second section is fixed to one end of the third section by mechanical connection;
[0042] The high temperature superconducting magnet is connected to one end of the first section by a superconducting joint.
[0043] The composite current lead structure based on high-temperature superconducting materials provided by the present invention divides the current lead into section A, section B and section C. Section A, section B and section C respectively work in different temperature zones and are connected in sequence, thereby satisfying the transmission current demand of the magnet and reducing the conducted heat to the magnet.
[0044] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0046] Figure 1 A schematic structural diagram of a composite current lead structure based on high temperature superconducting material according to an embodiment of the present invention is shown;
[0047] Figure 2 It shows a schematic structural diagram of a section A substrate in a composite current lead structure based on a high temperature superconducting material according to an embodiment of the present invention;
[0048] Figure 3 The structure of the high-temperature superconducting cross joint used in the composite current lead structure based on high-temperature superconducting materials according to an embodiment of the present invention is shown. Figure 1 ;
[0049] Figure 4 The structure of the high-temperature superconducting cross joint used in the composite current lead structure based on high-temperature superconducting materials according to an embodiment of the present invention is shown. Figure 2 ;
[0050] Figure 5 A schematic structural diagram of a B-section-C-section joint in a composite current lead structure based on high-temperature superconducting materials according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of the present application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit the present application; the terms "including" and "having" in the specification and claims of the present application and the above-mentioned drawings and any variations thereof are intended to cover non-exclusive inclusions. The terms "first", "second", "third", etc. in the specification and claims of the present application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order or a primary and secondary relationship. "Multiple" appearing in this application refers to more than two (including two).
[0053] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0054] Figure 1 The schematic diagram of the structure of the composite current lead structure based on high temperature superconducting material provided by the present invention is shown. Figure 1 The composite current lead structure includes: section A (i.e., the first section), section B (i.e., the second section) and section C (i.e., the third section). Section A, section B and section C respectively operate in different temperature zones and adopt different lead structures, which can meet the transmission current requirements of magnets such as high-temperature superconducting magnets and reduce the conduction heat to the magnets.
[0055] Figure 2 The structure of the substrate of section A in the composite current lead structure based on high temperature superconducting material provided by the present invention is shown in FIG. The structure of section A is formed by encapsulating a superconducting tape using a substrate of a high thermal conductivity material such as copper or copper alloy. The structure of the substrate of section A is shown in FIG. Figure 2. The substrate of section A is a long and thin strip structure, and its two ends are connected to the magnet and section B respectively. The width of the substrate of section A is 15-25mm, preferably 20mm, and the height is 5-15mm, preferably 10mm. A first shallow groove is provided on one surface of the substrate of section A along the length direction of the substrate. The first shallow groove extends from one end of the substrate of section A to the other end, and has a depth of 1-3mm, preferably 2mm, and a width of 10-20mm, preferably 16mm. Stacked superconducting tapes are welded in the first shallow groove along the length direction of the substrate, and the stacked superconducting tapes are also copper-plated superconducting tapes. The structural dimensions of section A can be obtained through simulation. When simulating, the docking strength between the two ends of section A and the high-temperature superconducting magnet and section B should be considered respectively. Under the condition of meeting the flow and heat conduction requirements, the cross-section of section A is minimized to reduce the overall weight of section A. Section A uses zero-resistance superconducting tape to transmit current and high thermal conductivity materials to transfer heat, so the magnet temperature can be controlled to be no higher than the magnet operating temperature (<=50K), and the heat exchanger can be used to control the temperature difference between the low-temperature end and the high-temperature end of Section A to be as small as possible.
[0056] The high-temperature superconducting magnet is connected to one end of section A, i.e., the low-temperature end, by a superconducting joint. The superconducting joint may be a high-temperature superconducting cross joint formed by welding the superconducting tape led out of the high-temperature superconducting magnet and the copper-plated superconducting tape led out of the low-temperature end of section A. The other end of section A, i.e., the high-temperature end, is fixed to one end of section B, i.e., the low-temperature end, by a mechanical connection. The same copper-plated superconducting tape runs through sections A and B for conduction. A heat exchanger is attached closely to the substrate of section A. The heat exchanger is used to absorb the heat generated during the operation of section A. The heat exchanger is provided with an air inlet and an air outlet. Cold helium with a temperature of 20K (Kelvin) flows inside the heat exchanger. In the mechanical connection, the substrate of section A and the base of section B overlap, and the contact area is 30×30 (length×width)-70×70mm. 2 , preferably 50×50mm 2 , 6 M6 bolts are used to tighten the overlap, and the 6 M6 bolts are arranged in two rows (3 bolts on each side), and indium sheets are placed at the contact points. The strip orientation is adjusted according to the actual space layout, which is a more flexible choice.
[0057] The base of the B segment is an elongated strip structure, which is made of a low thermal conductivity material such as stainless steel. A second shallow groove is provided on one surface of the B segment base along its length direction, and the copper-plated superconducting tape is welded in the second shallow groove along its length direction, and the second shallow groove extends from one end of the B segment base to the other end. The second shallow groove is connected to the first shallow groove, and the width and depth of the second shallow groove are the same as those of the first shallow groove. The length and cross-sectional area of the base of the B segment need to be optimized and designed through simulation according to the heat leakage and mechanical strength of the B segment. The present invention is based on the allowable heat leakage of 2W (watt) at the connection between the B segment base and the A segment base material, and the space distance between the A segment and the C segment, and determines that the length of the B segment base cannot exceed 700mm, preferably cannot exceed 500mm. Based on the above principles, the cross-section and length of the B segment can be further optimized through simulation. The width of the copper-plated superconducting tape is 5-15mm, preferably 10mm, and the thickness is 50-100μm, preferably 75μm. The length of the copper-plated superconducting tape needs to cover the A segment and the B segment until one end of the C segment, i.e., the low-temperature end. There may be more than one first shallow groove and second shallow groove, but the number of the first shallow groove and the second shallow groove is the same and the first shallow groove and the second shallow groove are connected one by one. There may be more than one copper-plated superconducting tape welded and fixed in a correspondingly connected first shallow groove and a second shallow groove. For example, the first shallow groove and the second shallow groove are both parallel, and the two first shallow grooves and the two second shallow grooves are connected one by one to form two parallel copper-plated superconducting tape shallow grooves, and two copper-plated superconducting tapes are welded and fixed in each copper-plated superconducting tape shallow groove. At this time, the connection structure between the high-temperature superconducting magnet and one end of section A, i.e., the low-temperature end, is as follows: Figure 3 and Figure 4 The structure of the high temperature superconducting cross joint shown in FIG. Figure 3 and Figure 4 , the copper-plated superconducting tape is led out from one end of section A, i.e., the low-temperature end, and 4 packaged superconducting tapes are led out from the wire lead-out guide groove separately arranged on the magnet. The copper-plated superconducting tape and the packaged superconducting tape are evenly arranged in two parallel rows, with 2 superconducting tapes stacked in each row, and the spacing between the two rows is 0.5-1.5mm (millimeter), preferably 1mm; the length of the copper-plated superconducting tape and the packaged superconducting tape is determined by the specific working conditions; the width of the copper-plated superconducting tape is 5-15mm, preferably 10mm, and the thickness is 50-100μm (micrometer), preferably 75μm; the width of the packaged superconducting tape is 6-18mm, preferably 12mm, and the thickness is 100-300μm, preferably 200μm; the joints of the copper-plated superconducting tape and the packaged superconducting tape are fixed by welding with 6337 solder; the copper-plated superconducting tape is loaded between the packaged superconducting tapes, and the copper-plated superconducting tape is loaded and welded to the ends of the packaged superconducting tape and fixed perpendicularly to each other. The resistance value of the high-temperature superconducting cross joint at 77K is less than 40nΩ (nanoohm).
[0058] The surface of the base of section B is nickel-plated, and the copper-plated superconducting tape is brazed on the surface with 6337 solder to achieve reliable mechanical fixation and good thermal conductivity. Section B uses zero-resistance superconducting tape to transmit current and uses low-conductivity materials for thermal insulation, thereby establishing a temperature gradient at both ends of section B, so that the temperature of the low-temperature end of section B is the operating temperature of the high-temperature end of section A (<=50K), and the temperature of the high-temperature end of section B is the operating temperature of the low-temperature end of section C (<=80K).
[0059] Figure 5 This is a schematic diagram of the structure of the B-C segment joint in the composite current lead structure based on high-temperature superconducting materials provided by the present invention. The other end of the base of the B segment, i.e., the high-temperature end, and one end of the C segment, i.e., the low-temperature end, are also fixed by the aforementioned mechanical connection: the base of the high-temperature end of the B segment overlaps the low-temperature end of the C segment, and the contact area is 30×30 (length×width)-70×70mm 2 , preferably 50×50mm 2 The high temperature end of section B is 3-7mm thick, preferably 5mm, and the overlap is tightened with 6 M6 bolts, which are arranged in two rows (3 bolts on each side), and the contact is padded with indium sheets. Figure 5 , the copper-plated superconducting tape at the high-temperature end of section B is led out and welded to section C for conduction. The end of the copper-plated superconducting tape at the high-temperature end of section B is stepped, wherein the stacked superconducting tapes are successively shortened by 15-35mm, preferably 25mm, from the top layer to the bottom layer. A joint groove is provided on one end of section C. The end of the copper-plated superconducting tape led out from the high-temperature end of section B is soldered in the joint groove of section C with 6337 solder. The solder length is 15-35mm, preferably 25mm. The superconducting surface of the bottom layer of the stacked superconducting tape is welded to the bottom of the joint groove, and the top layer of the superconducting tape of the stacked superconducting tape is welded to the end wall of the joint groove. The joint formed by the welding of the copper-plated superconducting tape at the high-temperature end of section B and the low-temperature end of section C has a resistance value not exceeding 300nΩ. For details of the welding distribution diagram, see Figure 5 The number of joint slots is determined according to specific working conditions.
[0060] One end of the C section is a square heat exchanger, the width of the square heat exchanger is 50-100 mm, preferably 80 mm, the length is 90-150 mm, preferably 120 mm, and the thickness is 20-40 mm, preferably 30 mm. The square heat exchanger is provided with a flow channel to fully exchange heat. One end of the square heat exchanger is provided with the joint groove, and the other end of the square heat exchanger is brazed and connected with a copper tube, and the copper tube is connected with the internal flow channel of the square heat exchanger. The square heat exchanger and the copper tube constitute the entire C section.
[0061] The material of section C uses a high thermal conductivity conventional conductor (non-superconductor, for example, copper or copper alloy), which uses the material itself to transmit current and transition the temperature of the high temperature end of section B to room temperature. Specifically, the copper tube of section C can be selected in different lengths according to the height of the device used for the magnet. The low temperature end and the high temperature end of section C are connected to 50K and 300K temperature sources respectively, and the cooling medium circulates in section C to absorb heat and cool down section C. After comprehensively considering the manufacturing cost and the convenience of actual installation, the copper tube of section C can be selected with an inner diameter of 15-25mm, preferably 20mm, and a wall thickness of 5-10mm, preferably 7mm.
[0062] The composite current lead structure based on high-temperature superconducting materials provided by the present invention divides the current lead into section A, section B and section C. Section A, section B and section C respectively work in different temperature zones and are connected in sequence, thereby satisfying the transmission current demand of the magnet and reducing the conducted heat to the magnet.
[0063] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite current lead structure based on high temperature superconducting material, characterized in that: include: The first, second and third paragraphs, The first section includes a superconducting tape encapsulated by a substrate of a high thermal conductivity material; The second section comprises a substrate made of a low thermal conductivity material, on which the superconducting tape is fixed; The third section adopts a conventional conductor with high thermal conductivity; One end of the first section is a low-temperature end, which is used to connect to a high-temperature superconducting magnet, and the other end of the first section is a high-temperature end, which is mechanically connected to one end of the second section; The superconducting tape at the other end of the second section is led out and welded to one end of the third section; The substrate of the first section is a thin and long strip structure with a width of 15-25 mm and a height of 5-15 mm; A first shallow groove is provided on one surface of the substrate along the length direction of the substrate, the first shallow groove extends from one end of the substrate to the other end, the depth of the first shallow groove is 1-3 mm, the width is 10-20 mm, and the superconducting tape is welded in the first shallow groove along the length direction of the substrate.
2. The composite current lead structure based on high temperature superconducting material according to claim 1, characterized in that: The base material of the first section is copper or copper alloy; The substrate has a width of 20 mm and a height of 10 mm; The shallow groove has a depth of 2 mm and a width of 16 mm.
3. The composite current lead structure based on high temperature superconducting material according to any one of claims 1 to 2, characterized in that: The first section of the substrate is provided with a heat exchanger, the heat exchanger is provided with an air inlet and an air outlet, and cold helium gas with a temperature of 20 degrees Kelvin flows inside the heat exchanger.
4. The composite current lead structure based on high temperature superconducting material according to any one of claims 1 to 2, characterized in that: The base of the second section is an elongated strip structure; A second shallow groove is provided on one surface of the substrate of the second section along the length direction of the substrate, the second shallow groove extends from one end of the substrate to the other end, the depth and width of the second shallow groove are the same as those of the first shallow groove, and the superconducting tape is welded in the second shallow groove along the length direction of the substrate; The superconducting tape has a width of 5-15 mm, a thickness of 50-100 μm, and a length covering the first section and the second section to one end of the third section; the length of the base of the second section does not exceed 700 mm; In the mechanical connection between the high temperature end of the first section and one end of the second section, the substrate of the first section and the base of the second section overlap and the contact area is 30×30-70×70 mm 2 .
5. The composite current lead structure based on high temperature superconducting material according to claim 4, characterized in that: The base material of the second section is stainless steel; The superconducting tape is a copper-plated superconducting tape with a width of 10 mm and a thickness of 75 μm, and is also a stacked superconducting tape; The length of the base of the second section does not exceed 500 mm; The contact area between the first section substrate and the second section substrate is 50×50 mm 2 .
6. The composite current lead structure based on high temperature superconducting material according to claim 5, characterized in that: The surface of the substrate of the second section is plated with nickel, and the copper-plated superconducting tape is brazed on the surface using 6337 solder.
7. The composite current lead structure based on high temperature superconducting material according to claim 5, characterized in that: The contact between the substrate of the first section and the base of the second section is fastened with M6 bolts, and the contact is padded with indium sheets.
8. The composite current lead structure based on high temperature superconducting material according to claim 5, characterized in that: One end of the third section is a square heat exchanger, the width of the square heat exchanger is 50-100 mm, the length is 90-150 mm, and the thickness is 20-40 mm. A flow channel is provided inside the square heat exchanger, and a joint groove is provided at one end of the square heat exchanger. The other end of the square heat exchanger is connected to a copper tube, and the copper tube is connected to the flow channel inside the square heat exchanger; The end of the superconducting tape led out from the other end of the second section is in a stepped shape, wherein the stacked superconducting tapes are shortened by 15-35 mm from the top layer to the bottom layer, and the end is welded in the joint groove with 6337 solder, and the solder length is 15-35 mm. The superconducting surface of the bottom layer of the stacked superconducting tapes is welded to the bottom of the joint groove, and the top of the top layer of the stacked superconducting tapes is welded to the end wall of the joint groove.
9. The composite current lead structure based on high temperature superconducting material according to claim 8, characterized in that: The square heat exchanger has a width of 80 mm, a length of 120 mm and a thickness of 30 mm; The other end of the square heat exchanger is connected to the copper tube by brazing; The stacked superconducting tapes are successively shortened by 25 mm from the top layer to the bottom layer, and the length of the solder is 25 mm; The base at the other end of the second section is fixed to one end of the third section by mechanical connection; The high temperature superconducting magnet is connected to one end of the first section by a superconducting joint.
Citation Information
Patent Citations
W-band high-temperature superconducting plane filter and bandwidth and external Q value adjustment method therefor
CN105932375A
6 kA high temperature superconducting (HTS) current lead
CN107068324A