A welding process for solar cells
By applying adhesive film and solder paste to both sides of copper-based plates or copper foils, the problem of varying solder strip lengths and cumbersome manual operation in Sunpower battery cells has been solved, achieving efficient and controllable automated welding, and improving production efficiency and quality.
Patent Information
- Application Number
- CN202410117002.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-27
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-27
AI Technical Summary
The existing Sunpower battery cell manufacturing process suffers from issues such as varying solder strip lengths, cumbersome manual operation, low welding efficiency, and difficulty in quality control, making it unsuitable for the needs of continuous production lines for mass production.
Using whole copper-based plates or copper foils as raw materials, adhesive films are applied to both sides, and then the adhesive films at the solder joints are removed by stamping. The plates are then cleaned and coated with solder paste. Finally, they are cut into shape and adjacent battery cells are simultaneously welded together using a solder strip. The equipment enables automated welding.
It reduces the types of raw materials and management workload, improves welding quality and efficiency, adapts to mass production, and allows for controllable welding temperature and time, reducing potential quality risks and improving production efficiency.
Smart Images

Figure CN118268668B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solar cell equipment manufacturing technology in the photovoltaic new energy industry, and specifically relates to a welding process method for solar cell wafers. Background Technology
[0002] The specifications of Sunpower solar cells (i.e., solar cells) in the photovoltaic new energy industry include 125×125mm, 125×62.5mm, 125×41.6mm, 166×166mm, 166×83mm, and 166×41.5mm, etc. The existing Sunpower solar cell manufacturing process has the following defects: 1. Different specifications and models of Sunpower solar cells have different widths, and the required solder strip lengths are also different. When stocking raw materials, it is necessary to prepare materials to match solder strips of different lengths. There are many types of raw materials, and the workload of procurement, warehousing, material management and material handling is large. 2. Existing Sunpower solar cells typically consist of a three-layer structure: the first layer is the solar cell, the second layer is the adhesive film, and the third layer is the welding ribbon. During production, the solar cells need to be manually positioned and fixed, and then the adhesive film needs to be manually applied to each cell one by one. After multiple solar cells are formed into a single string, they are transferred to the next process for welding. Manually applying the adhesive film is inconvenient, the accuracy of the application position is poor, and impurities are easily left on the film surface, causing potential quality problems. Furthermore, the welding dwell time and welding force cannot be controlled. 3. The existing Sunpower battery cell production process can only be carried out by sporadic manual welding. After the battery cell is positioned and fixed by a fixture, the adhesive film is first pasted, then the welding ribbon is placed on the adhesive film, and finally welding is carried out. The welding efficiency and welding quality are low and cannot meet the needs of continuous production lines for mass production. 4. During the production process, depending on the different specifications and models of Sunpower battery cells, it is necessary to select and match the appropriate length of welding strips for welding. This operation is cumbersome, time-consuming, has a large amount of ineffective work, and results in low production efficiency. Summary of the Invention
[0003] To address the aforementioned problems in the existing technology, the present invention aims to provide a welding process method for solar cells that uses fewer types of raw materials, eliminates the need for manual application of adhesive film to each cell, ensures high accuracy in adhesive film application, guarantees welding quality, is easy to operate, can adapt to the needs of continuous production lines for mass production, and has high production efficiency.
[0004] The technical solution adopted in this invention is as follows: The first technical solution provides a welding process method for solar cells. The following steps are included: Select metal sheets or metal foils as raw materials; Apply adhesive film to both sides of the metal sheet or metal foil. The adhesive film at the solder joint is removed by stamping. Apply solder paste to the solder joints; The welding strip is formed by punching and shearing. All solar cells located within the area of two adjacent solar cells are simultaneously welded together using a single welding strip.
[0005] The second technical solution provides another welding process for solar cells, which includes the following steps: Select copper-based plates or rolled copper foil as raw materials; Slitting and punching positioning holes in one go; Apply adhesive film to both sides of the copper-based plate or copper foil. bake; The adhesive film at the solder joint is removed by stamping. Cleaning; Apply solder paste to the solder joints; The strip is formed by punching and shearing, and then slit again to obtain the finished welding strip. All solar cells located within the area of two adjacent solar cells are simultaneously welded together using a single welding strip.
[0006] The third technical solution also provides another welding process for solar cells, which includes the following steps: S01, copper-based sheet material preparation; S02, Arrange the layout of the solder strips on the copper-based plate according to the production order design plan; S03, machining fixture positioning holes on copper-based plates; S04, First Slicing; S05, apply adhesive film to both sides of the copper-based plate. S06, the copper-based substrate is baked at high temperature for a period of time; S07, stamping removes the adhesive film from each solder joint of each solder strip, exposing the copper-based substrate at all solder joint locations; S08, Clean the solder joint area; S09, Place the cleaned copper-based board into a stencil container, and apply solder paste to all solder joints to obtain a semi-finished board with solder strips. S10: Place the semi-finished welding strip into the stamping fixture for stamping to achieve the second slitting; at the same time, stamping and blanking are performed to obtain the finished welding strip; then proceed to S11 or S12. S11, Pack according to packaging requirements; S12, transfer to the battery cell welding platform loading area; S13 uses a gripping and suction device to pick up the battery cells and welding strips onto the welding platform respectively; S14, Positioning and fixing the welding strip; S15, pick up the battery cell and place it on the solder ribbon; S16, the welding ribbon and the battery cell are simultaneously adsorbed and fixed onto the conveyor belt by a negative pressure device; S17, the conveyor belt runs in a cycle, continuously transporting the welding strip and the battery cells forward at the same time; S18, the welding station uses a welding head to fix and weld each welding point of the welding strip to the corresponding battery cell, thereby enabling the simultaneous welding and connection of all battery cells located in the area of two adjacent whole battery cells through a single welding strip.
[0007] Furthermore, the Vickers hardness of the copper-based plate is less than 55 kg / mm². The thickness of the copper-based plate is 0.1mm to 0.2mm.
[0008] Furthermore, the thickness of the copper-based plate is 0.15 mm.
[0009] Furthermore, the material of the adhesive film is polyimide. The thickness of the adhesive film is 0.06mm to 0.15mm.
[0010] Furthermore, the thickness of the adhesive film is 0.06 mm.
[0011] Furthermore, the baking temperature is 230℃~280℃; the baking time is 2~5 minutes; Preferably, the baking temperature is 250°C and the baking time is 3 minutes.
[0012] Furthermore, step S05 also includes the following operations: The areas on the adhesive film corresponding to the solder joints that need to be exposed on the copper-based substrate are pre-engraved with lines using a laser engraving machine to form knockout hole structures.
[0013] Furthermore, the thickness of the solder paste applied to the solder joint is 50–70 μm; preferably, the thickness of the solder paste applied to the solder joint is 60 μm.
[0014] Finally, the welding strip includes a long strip-shaped welding strip body, on which multiple pairs of welding points extending and protruding to both sides are provided; The copper-based plate of the welding strip body has one or more break points in the middle, and the adhesive film on both sides of each break point is continuous.
[0015] The beneficial effects of this invention are as follows: A welding process for solar cells uses a whole copper-based plate or copper foil as raw material. First, adhesive film is applied to both sides of the copper-based plate or copper foil. Then, the adhesive film at the solder joints is removed by punching, the area is cleaned, and solder paste is applied to the solder joints. Finally, the strips are cut and slit to obtain finished solder ribbons. The solder ribbons require only one type of raw material: the whole copper-based plate. Different sizes and specifications of solder ribbons can be arranged and laid out on the whole copper-based plate. The fewer types of raw materials reduce the workload in procurement, warehousing, material management, and material handling. It eliminates the need for manual application of adhesive film to each sheet, ensuring high accuracy in adhesive film application and guaranteeing welding quality. The process is convenient and adaptable to the needs of continuous production lines for mass production, resulting in high production efficiency.
[0016] 1. The welding process of the solar cell of the present invention greatly improves production efficiency. Compared with the hourly output of conventional manual welding, the welding efficiency of the welding strip bonding equipment produced by this process can be increased by 40% per hour. 2: The welding process of the solar cell of the present invention produces welding strips that can be precisely welded on equipment. The welding temperature and welding time of the equipment welding can be precisely controlled. Compared with the previous manual welding method, the welding temperature and welding dwell time could not be precisely controlled. The quality stability and controllability of the products using this process are greatly improved. 3: A copper strip substrate with more suitable hardness was used, which reduced the problem of microcracks in the welded cells caused by the stress of the solder strip; 4: The process of applying tin to the solder joints is adopted, which increases the thickness of the tin layer, improves solderability, and reduces the surface tin cost problem caused by applying tin to all conventional solder ribbons. 5. The welding process of the solar cell of the present invention reduces the step of immersing the welding strip in flux during welding, thereby reducing the quality risks of flux residue on the surface of the cell. Attached Figure Description
[0017] Figure 1 This is a schematic diagram of the solder ribbon structure used for the entire SunPower solar cell in the welding process method of the solar cell according to Embodiment 1 of the present invention. Figure 2 yes Figure 1 A schematic diagram of the rear view structure; Figure 3 yes Figure 1 Enlarged schematic diagram of the left-side view structure; Figure 4 This is a schematic diagram of the solder strip structure used for a 1 / 2 SunPower solar cell in the welding process method of the solar cell according to Embodiment 1 of the present invention; Figure 5 yes Figure 4 A schematic diagram of the rear view structure; Figure 6 yes Figure 4 Enlarged schematic diagram of the left-side view structure; Figure 7 This is a schematic diagram of the solder strip structure used for a 1 / 3 SunPower solar cell in the welding process method of the solar cell according to Embodiment 1 of the present invention; Figure 8 yes Figure 7 A schematic diagram of the rear view structure; Figure 9 yes Figure 7 Enlarged schematic diagram of the left-side view structure; Figure 10 This is a schematic diagram of the structure of multiple whole sunpower cells connected by welding ribbons for fixing and welding a whole sunpower cell in the welding process method of the solar cell of Embodiment 1 of the present invention. Figure 11 This is a schematic diagram of the layout scheme of the welding strips on the copper-based substrate in the welding process method of the solar cell according to Embodiment 1 of the present invention. Figure 12 This is a schematic diagram of the solder ribbon break point structure for a 1 / 2 SunPower solar cell in the welding process method of the solar cell according to Embodiment 1 of the present invention; Figure 13 This is a schematic diagram of the solder ribbon break point structure for a 1 / 3 SunPower solar cell in the welding process method of the solar cell according to Embodiment 1 of the present invention. Detailed Implementation
[0018] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0019] like Figures 1-13 As shown, in order to solve the technical problems in the prior art, the present invention provides a welding process method for solar cells. The overall planning scheme first conceives of a novel welding strip structure and a high-efficiency, time-saving and labor-saving welding process method for solar cells to solve the technical problems existing in the prior art.
[0020] First, we examine the technical problems in existing technologies. The first issue is the wide variety of specifications for SunPower battery cells used in lithium-ion batteries, primarily including the following specifications: Available in sizes such as 125×125mm, 125×62.5mm, 125×41.6mm, 166×166mm, 166×83mm and 166×41.5mm.
[0021] 1. Different specifications and models of Sunpower solar cells have different widths, and the required solder strip lengths are also different. When stocking raw materials, it is necessary to prepare materials to match solder strips of different lengths. There are many types of raw materials, and the workload of procurement, warehousing, material management and material handling is large. 2. Existing Sunpower solar cells typically consist of a three-layer structure: the first layer is the solar cell, the second layer is the adhesive film, and the third layer is the welding ribbon. During production, the solar cells need to be manually positioned and fixed, and then the adhesive film needs to be manually applied to each cell one by one. After multiple solar cells are formed into a single string, they are transferred to the next process for welding. Manually applying the adhesive film is inconvenient, the accuracy of the application position is poor, and impurities are easily left on the film surface, causing potential quality problems. Furthermore, the welding dwell time and welding force cannot be controlled. 3. The existing Sunpower battery cell production process can only be carried out by sporadic manual welding. After the battery cell is positioned and fixed by a fixture, the adhesive film is first pasted, then the welding ribbon is placed on the adhesive film, and finally welding is carried out. The welding efficiency and welding quality are low and cannot meet the needs of continuous production lines for mass production. 4. During the production process, depending on the different specifications and models of Sunpower battery cells, it is necessary to select and match the appropriate length of welding strips for welding. This operation is cumbersome, time-consuming, has a large amount of ineffective work, and results in low production efficiency.
[0022] The overall planning scheme is as follows: The first technical solution provides a welding process method for solar cells. The following steps are included: Select metal sheets or metal foils as raw materials; Apply adhesive film to both sides of the metal sheet or metal foil. The adhesive film at the solder joint is removed by stamping. Apply solder paste to the solder joints; The strip is punched and sheared to produce the finished welding strip; all the battery cells located in the area of two adjacent whole battery cells are simultaneously welded together by a single welding strip.
[0023] The second technical solution provides another welding process for solar cells, including the following steps: Select copper-based plates or rolled copper foil as raw materials; Slitting and punching positioning holes in one go; Apply adhesive film to both sides of the copper-based plate or copper foil. bake; The adhesive film at the solder joint is removed by stamping. Cleaning; Apply solder paste to the solder joints; The strip is formed by punching and shearing, and then slit again to obtain the finished welding strip. All solar cells located within the area of two adjacent solar cells are simultaneously welded together using a single welding strip.
[0024] The third technical solution also provides another welding process for solar cells, which is carried out according to the following steps: S01, Prepare copper-based sheet material; the Vickers hardness of the copper-based sheet material is required to be less than 55 kg / mm2; the thickness of the copper-based sheet material is 0.1 mm to 0.2 mm.
[0025] The preferred thickness of the copper-based plate is 0.15 mm.
[0026] Specifically, rolled copper foil with a thickness of 0.15mm can be used; Because the copper foil raw material has a large area, it needs to be cut into three parts according to the specifications and dimensions of the jigs in the production equipment, that is, the whole working board is divided into 3PNLs. S02, According to the production order design plan, the layout plan of the welding strip 10 on the copper base plate 100; S03, machining fixture positioning holes on the copper-based plate, through which the copper-based plate can be positioned on the fixture; S04, First slitting; According to the layout plan of the original welding strips, punch the break point of each welding strip; The welding process method for solar cells of the present invention is applicable to a strip core structure of a long strip body 1, on which multiple pairs of protruding welding points 2 extending to both sides are provided. In order to meet the requirements of the Sunpower battery cells to be welded and connected separately and to be mutually insulated, one or more break points 3 need to be set in the middle of the copper base plate of the welding strip body, and the adhesive film 4 on both sides of each break point is continuous.
[0027] The specific break point structure of the solder strip is as follows: Figures 12-13 As shown.
[0028] The length, width, solder joint position, number of solder joint pairs, and the position and number of break points of the main body of the welding strip can all be adaptively set according to the specifications and dimensions of the solar cells. For example, based on different specifications of Sunpower solar cells such as 125×125mm, 125×62.5mm, 125×41.6mm, 166×166mm, 166×83mm, and 166×41.5mm, the length, width, solder joint position, number of solder joint pairs, and the position and number of break points of the main body of the welding strip can be set accordingly. For example, 125×125mm and 166×166mm Sunpower solar cells are whole Sunpower solar cells, and correspondingly, a whole-piece solder ribbon structure can be set for whole Sunpower solar cells; 125×62.5mm and 166×83mm Sunpower solar cells are 1 / 2 Sunpower solar cells, and correspondingly, a 1 / 2 Sunpower solar cell solder ribbon structure can be set for 1 / 2 Sunpower solar cells; 125×41.6mm Sunpower solar cells are 1 / 3 Sunpower solar cells, and correspondingly, a 1 / 3 Sunpower solar cell solder ribbon structure can be set for 1 / 3 Sunpower solar cells; 166×41.5mm Sunpower solar cells are 1 / 4 Sunpower solar cells, and correspondingly, a 1 / 4 Sunpower solar cell solder ribbon structure can be set for 1 / 4 Sunpower solar cells.
[0029] S05, apply adhesive film to both sides of the copper-based plate. The preferred material for the adhesive film is polyimide. The thickness of the adhesive film is 0.06mm to 0.15mm; The preferred thickness of the adhesive film is 0.06 mm or 0.135 mm.
[0030] Before applying the adhesive film, the shape of the part of the copper substrate that needs to be exposed during the use of the solder ribbon is pre-engraved on the adhesive film. Specifically, the adhesive film is pre-carved with lines using a laser engraving machine at the locations of the solder joints that need to be exposed on the copper-based plate, forming a knockout hole structure; S06, the copper-based substrate is baked at high temperature for a period of time; The baking temperature range is 230℃~280℃; The specific baking time is 2 to 5 minutes, but in special circumstances it can be baked for one hour.
[0031] Preferably, the baking temperature is set to 250°C and the baking time is set to 3 minutes.
[0032] S07, the adhesive film on each solder joint of each solder strip is removed by die stamping, exposing the copper base plate at all solder joints; the specific stamping die can be a conventional film-removing device in the existing technology; S08, Clean the solder joint area; specifically, the conventional degreasing and micro-etching cleaning production line in the existing technology can be used to clean the solder joint area; S09, the cleaned copper-based plate is placed into a stencil container, and solder paste is applied to all solder joints to obtain a semi-finished solder strip board; specifically, the conventional stencil printing process in the existing technology can be used to apply solder paste to all solder joints. The thickness of the solder paste applied to the solder joint is 50–70 μm; preferably, the thickness of the solder paste applied to the solder joint is 60 μm.
[0033] S10: Place the semi-finished welding strip plate into the stamping fixture for stamping to achieve the second slitting; at the same time, punch and shear to remove the copper base plate and adhesive film from each of the four stress relief holes, stamp and form, and blank; A finished solder strip integral structure with double-sided film coating of 300 was obtained; The subsequent steps are either S11 or S12. S11, Pack and store according to packaging requirements; Specific packaging and storage requirements are as follows: Store in a cool, dry, and well-ventilated environment at a temperature of <25℃ and a humidity of <70%, away from light. Storage environment: Temperature: 18-24℃, Humidity: 40-70%; Note: FPC shelf life: 12 months for chemical gold process, 6 months for antioxidant process (vacuum packaged). S12, transfer to the battery cell welding platform loading area; specifically, it can be directly transferred to the welding platform loading area of a conventional conductor automatic welding production line equipment with equipment such as gripper, conveyor belt, negative pressure, and welding head in the existing technology; S13 uses a gripping and suction device to pick up the battery cells and welding strips onto the welding platform respectively; S14, Positioning and fixing the welding strip; S15, pick up the battery cell and place it on the solder ribbon; S16, the welding ribbon and the battery cell are simultaneously adsorbed and fixed onto the conveyor belt by a negative pressure device; S17, the conveyor belt runs in a cycle, continuously transporting the welding strip and the battery cells forward at the same time; S18, the welding station uses a welding head to fix and weld each welding point of the welding strip to the corresponding battery cell, thereby enabling the simultaneous welding and connection of all battery cells located within the area 200 of two adjacent whole battery cells using a single welding strip.
[0034] The welding connection method and structure are designed for solar cells of different sizes. All solar cells located within the area 200 of two adjacent solar cells are simultaneously welded together using welding strips 10 with corresponding different structures. The specific method is as follows: I. The specific structure of the welding strip for a 1 / 2 Sunpower battery cell with a specification of 125×62.5mm is as follows: A pair of outwardly extending welding ears are set on the main body of the welding strip near both ends, a break point is set in the middle of the main body of the welding strip, and multiple stress relief holes are set in the middle and ends of the main body of the welding strip. The solder pads on each pair of welding ears are respectively welded to two adjacent 125×62.5mm half-cell solar cells. Through the solder ribbons of the 125×62.5mm half-cell Sunpower solar cells, four adjacent half-cell solar cells located above, below, left, and right in the area of two adjacent 125×125mm solar cells in a row of full solar cells can be welded together, thereby forming two adjacent 125×125mm full solar cells.
[0035] II. The specific structure of the welding strip used for 1 / 3 Sunpower battery cells with a specification of 125×41.6mm is as follows: A pair of outwardly extending welding ears are set on the main body of the welding strip near both ends, and a pair of outwardly extending welding ears are also set in the middle of the main body of the welding strip, that is, three pairs of welding ears are evenly distributed on the main body of the welding strip, and a break point is set between each pair of adjacent welding ears; multiple stress relief holes are set in the middle and ends of the main body of the welding strip.
[0036] The pads on each pair of welding ears are welded to two adjacent 1 / 3-cell solar cells of 125×41.6mm size; the three welding ears on one side edge of each welding strip can be welded to three 1 / 3-cell solar cells arranged side by side to form a whole solar cell.
[0037] By using the solder ribbon of a 1 / 3 Sunpower solar cell with a specification of 125×41.6mm, six 1 / 3 solar cells located vertically or horizontally adjacent to two full 125×125mm solar cells in a row of solar cells can be soldered together, thereby forming two full 125×125mm solar cells that are vertically adjacent to each other.
[0038] III. The specific structure of the welding strip used for a whole Sunpower battery cell with a specification of 125×125mm is as follows: A pair of outwardly extending welding ears are respectively set on the welding strip body near both ends, a pair of outwardly extending welding ears 2 are set in the middle of the welding strip body, and multiple stress relief holes are set in the middle and ends of the welding strip body. Two adjacent 125×125mm SunPower solar cells in a row can be soldered together using a solder strip made of a single 125×125mm SunPower solar cell.
[0039] IV. The specific structure of the welding strip for a 1 / 2 Sunpower battery cell with a specification of 166×83mm is as follows: A pair of outwardly extending welding ears are set on the welding strip body near both ends, and two pairs of welding ears are evenly distributed in the middle section of the welding strip body, that is, four pairs of welding ears are evenly distributed on the welding strip body. Multiple stress relief holes are set in the middle and ends of the welding strip body. A break point is set between the two pairs of welding ears in the middle section of the welding strip body.
[0040] The pads on each pair of welding ears are welded to two adjacent 166×83mm half-cell solar cells; the four welding ears on one side edge of each welding strip can be welded to two 166×83mm half-cell solar cells arranged side by side to form a whole solar cell.
[0041] Using the solder ribbons for 166×83mm Sunpower solar cells, four 166×83mm 1 / 2 solar cells located vertically or horizontally adjacent to two adjacent full solar cells in a row of full solar cells can be soldered together to form two vertically adjacent full 166×166mm solar cells.
[0042] V. The specific structure of the welding strip used for 1 / 4 Sunpower battery cells with a specification of 166×41.5mm is as follows: A pair of outwardly extending welding ears are respectively set on the welding strip body near both ends, and two pairs of welding ears are evenly distributed in the middle section of the welding strip body, that is, four pairs of welding ears are evenly distributed on the welding strip body. A break point is set between each pair of adjacent welding ears; multiple stress relief holes are set in the middle and ends of the welding strip body.
[0043] The pads on each pair of welding ears are welded to two adjacent 166×41.5mm quarter-cell solar cells; the four welding ears on one side edge of each welding strip can be welded to four 166×41.5mm quarter-cell solar cells arranged side by side to form a whole solar cell.
[0044] Using the solder ribbons for 1 / 4-cell Sunpower solar cells of 166×41.5mm size, eight 1 / 4-cell solar cells of 166×41.5mm size located vertically or horizontally within two adjacent full-cell areas in a row of full-cell solar cells can be soldered together to form two adjacent full-cell solar cells of 166×166mm size.
[0045] VI. The specific structure of the welding strip used for the 166×166mm full-size Sunpower battery cell is as follows: A pair of outwardly extending welding ears are respectively set on the welding strip body near both ends, and two pairs of welding ears are evenly distributed in the middle section of the welding strip body, that is, four pairs of welding ears are evenly distributed on the welding strip body. Multiple stress relief holes are set in the middle and ends of the welding strip body.
[0046] The pads on each pair of welding ears are welded to two adjacent 166×166mm solar cells, meaning that the four welding ears on the same side edge of each welding strip can be welded to the same 166×166mm solar cell; two adjacent 166×166mm solar cells in a row can be welded together through a single welding strip.
[0047] The welding process for solar cells of this invention uses a whole copper-based plate or copper foil as raw material. First, adhesive film is applied to both sides of the copper-based plate or copper foil. Then, the adhesive film at the solder joints is removed by punching, followed by cleaning and application of solder paste. Finally, the strips are cut and slit to obtain finished solder ribbons. The solder ribbons require only one type of raw material: the whole copper-based plate. Different sizes and specifications of solder ribbons can be arranged on the whole copper-based plate. This reduces the number of raw material types, decreasing workload in procurement, warehousing, material management, and material handling. It eliminates the need for manual application of adhesive film to each cell, ensuring high accuracy in adhesive film application, guaranteeing welding quality. The process is convenient and adaptable to the needs of continuous production lines for mass production, resulting in high production efficiency. Applicable to Sunpower 125 solar cells. 125mm125 62.5mm125 41.6mm, 166 166mm166 83mm, 166 The 41.5mm weld fills the technological gap in this field where centralized equipment welding cannot be used.
[0048] Example 1: The actual operation process of Example 1 is as follows: 1: Use a 0.15mm copper substrate panel with a hardness (HV) of less than 55. First, drill positioning holes in the copper foil, and then perform one slitting. 2: After the copper foil is slit once, a 0.06mm thick polyimide film is then applied to both sides of the copper foil; 3: Place the coated copper foil into an oven and bake at 250 degrees Celsius for 3 minutes to ensure the film and copper foil are completely bonded together. 4. Place the baked material into a custom mold, and use a stamping method to remove the surface film at the solder joint location, leaving the solder joint area exposed. Then, place the solder joint area into a specific box for cleaning to maintain its cleanliness and prepare for the soldering process. 5: Place the cleaned raw materials under a specific stencil container and apply solder paste to the solder joints. The solder paste thickness should be 60µm. 6: Then, the finished product is placed into the stamping fixture with the mold opened for stamping and slitting, and stamping into strips that meet the requirements of the drawings; 7: Then package the welding strips according to the packaging requirements; 8: When producing welded Sunpower battery cells, simply place the processed welding strip in the loading area, and the equipment will pick up the welding strip and battery cells respectively according to the program and place them onto the welding platform; 9: The first step is to pick up the welding strip and fix it in position on the platform. Then, pick up the battery cell and place it on the welding strip. At the same time, the negative pressure equipment will adsorb and fix the welding strip and the battery cell. The conveyor belt will transport them forward. The special welding head of the equipment will weld the welding strip and the battery cell together directly, completing the entire welding process.
[0049] Example 1 transforms the traditional method of separating the solder strip and film into an integrated component using a single process, particularly for 125. 62.5mm, 125 41.6mm 166 83mm, 166 The welding of 41.5mm products completely overturns the traditional welding process. It directly adopts a double-sided film coating process, which realizes the protection of the insulation layer between welds and reflects the overall process of the weld strip. It can also carry out the same process on the same set of equipment, and it is very convenient to switch between different specifications of products.
[0050] Example 1 addresses the drawbacks of conventional Sunpower solder ribbon production, which requires manual film application and cannot be mass-produced using equipment, by unifying the process into a single step and allowing for direct welding using equipment. The process directly combines the film and solder ribbon together, replacing the traditional separate film application method, to form a single, integrated component that can be produced directly by equipment. This simplifies the manual operation process, reducing time and inefficiency. The equipment-based film application, using a high-temperature coating technology, ensures greater stability, eliminates air bubbles between the film and solder ribbon, and provides stronger adhesion, reducing the quality risks associated with impurities left on the film surface due to manual application.
[0051] 1. The welding process of the solar cell of the present invention greatly improves production efficiency. Compared with the hourly output of conventional manual welding, the welding efficiency of the welding strip bonding equipment produced by this process can be increased by 40% per hour. 2: The welding process of the solar cell of the present invention produces welding strips that can be precisely welded on equipment. The welding temperature and welding time of the equipment welding can be precisely controlled. Compared with the previous manual welding method, the welding temperature and welding dwell time could not be precisely controlled. The quality stability and controllability of the products using this process are greatly improved. 3: A copper strip substrate with more suitable hardness was used, which reduced the problem of microcracks in the welded cells caused by the stress of the solder strip; 4: The process of applying tin to the solder joints is adopted, which increases the thickness of the tin layer, improves solderability, and reduces the surface tin cost problem caused by applying tin to all conventional solder ribbons. 5. The welding process of the solar cell of the present invention reduces the step of immersing the welding strip in flux during welding, thereby reducing the quality risks of flux residue on the surface of the cell.
[0052] Example 2: The actual operation process of Example 2 is based on the technical solution of Example 1 above. The thickness of the copper base plate is 0.1 mm; the thickness of the adhesive film is 0.1 mm; the baking temperature is 230℃; the baking time is 2 minutes; and the thickness of the solder paste applied at the solder joint is 50 μm.
[0053] Compared to Example 1, Example 2 achieves the following technical effects: due to the shorter baking time and slightly lower baking temperature, the adhesion between the film and the copper foil may slightly separate during strong scratching or peeling, but this does not affect the normal use of the solar cell electrode. Other performance characteristics and effects are the same as in Example 1.
[0054] Example 3: The actual operation process of Example 3 is based on the technical solution of Example 1 above. The thickness of the copper base plate is 0.2 mm; the thickness of the adhesive film is 0.15 mm; the baking temperature is 280℃; the baking time is 5 minutes; and the thickness of the solder paste applied at the solder joint is 70 μm.
[0055] Compared to Example 1, Example 3 achieves slightly different overall appearances of the film material due to a longer baking time and a slightly higher baking temperature. However, the overall appearance is essentially the same and does not affect the normal use of the solar cell electrode. Other properties and effects are the same as in Example 1.
[0056] In summary, the parameter technical solution of Embodiment 1 is the best implementation method, and Embodiments 2 and 3 can also be adopted with relaxed conditions.
[0057] This invention is not limited to the above-described optional embodiments. Anyone can derive other various forms of products under the guidance of this invention. However, regardless of any changes made in their shape or structure, any technical solution that falls within the scope of the claims of this invention shall be protected by this invention.
Claims
1. A welding process for solar cells, characterized in that: The following steps are included: S01, copper-based sheet material preparation; S02, According to the production order design plan, arrange the layout of the welding strips on the copper-based plate; S03, machining fixture positioning holes on copper-based plates; S04, First slitting: According to the layout plan of the original welding strips, punch the break point of each welding strip. S05, apply adhesive film to both sides of the copper-based plate. S06, the copper-based substrate is baked at high temperature for a period of time; S07, stamping removes the adhesive film from each solder joint of each solder strip, exposing the copper-based substrate at all solder joint locations; S08, Clean the solder joint area; S09, Place the cleaned copper-based board into a stencil container, and apply solder paste to all solder joints to obtain a semi-finished board with solder strips; S10: Place the semi-finished welding strip into the stamping fixture for stamping to achieve the second slitting; at the same time, stamping and blanking are performed to obtain the finished welding strip; then proceed to S11 or S12. S11, Pack according to packaging requirements; S12, transfer to the battery cell welding platform loading area; S13 uses a gripping and suction device to pick up the battery cells and welding strips onto the welding platform respectively; S14, Positioning and fixing the welding strip; S15, pick up the battery cell and place it on the solder ribbon; S16, the welding ribbon and the battery cell are simultaneously adsorbed and fixed onto the conveyor belt by a negative pressure device; S17, the conveyor belt runs in a cycle, continuously conveying the welding strip and the battery cells forward at the same time; S18, the welding station uses a welding head to fix and weld each welding point of the welding strip to the corresponding battery cell, thereby achieving simultaneous welding and connection of all battery cells located in the area of two adjacent whole battery cells through a single welding strip; The welding strip includes a long strip-shaped welding strip body, on which multiple pairs of welding points extending and protruding to both sides are provided; The copper-based plate of the welding strip body has one or more break points in the middle, and the adhesive film on both sides of each break point is continuous.
2. The welding process method for solar cells according to claim 1, characterized in that: The Vickers hardness of the copper-based plate is less than 55 kg / mm2; The thickness of the copper-based plate is 0.15 mm.
3. The welding process method for solar cells according to claim 1, characterized in that: The adhesive film is made of polyimide. The thickness of the adhesive film is 0.06mm to 0.15mm.
4. The welding process method for solar cells according to claim 1, characterized in that: The thickness of the adhesive film is 0.06 mm.
5. The welding process method for solar cells according to claim 1, characterized in that: Baking temperature is 230℃~280℃; baking time is 2~5 minutes.
6. The welding process method for solar cells according to claim 1, characterized in that: Step S05 also includes the following operations: The areas on the adhesive film corresponding to the solder joints that need to be exposed on the copper-based substrate are pre-engraved with lines using a laser engraving machine to form knockout hole structures.
7. The welding process method for solar cells according to claim 1, characterized in that: The thickness of the solder paste applied to the solder joint should be 50–70 μm.
Citation Information
Patent Citations
Solder strip for back-contact solar cell
CN102983195A
Method for manufacturing back contact type crystalline silicon solar cell component
CN103456843A
Special assembly strip for battery protective plate connecting piece
CN105633329A