A high conductive silver paste for HJT battery and preparation method thereof
By using materials such as doped silver powder and 2,6-diaminopurine in the conductive silver paste of HJT batteries, the problem of balancing conductive performance and printing performance is solved, and the combination of high conductive performance and excellent printing performance is achieved, which is suitable for HJT batteries. .
Patent Information
- Application Number
- CN202410698388.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-05-31
AI Technical Summary
The existing conductive silver paste for HJT batteries is difficult to balance between improving conductivity and printing performance. High silver powder content leads to a decrease in conductivity and an increase in viscosity, which affects printing adaptability.
Doped silver powder is used to prepare graphene oxide and silver nitrate blended by Hummer's method. Electrostatic interaction is used to increase the contact between silver particles and fill the gaps to improve conductivity. The tertiary amine functional group is introduced through 2,6-diaminopurine to shorten the curing time and improve Cure efficiency and dispersion.
It achieves high conductivity and excellent printing performance, reduces contact resistivity, improves fine grid width and printing uniformity, and is suitable for HJT batteries.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the field of HJT batteries, and in particular to a high-conductivity silver paste for HJT batteries and a preparation method thereof. Background Art
[0002] With the continuous advancement of photovoltaic cell technology, the trend of iteration from P-type to N-type will begin in 2021, moving towards a higher efficiency level. N-type technology routes represented by TOPCon (Tunnel Oxide Passivating Contacts) tunnel oxide passivation contact cells and HJT (Heterojunction with Intrinsic Thinfilm) heterojunction cells have made breakthroughs one after another, and the industrialization process is expected to accelerate. Compared with TOPCon, HJT has better contact resistance and passivation effects, is more suitable for thin filming, has higher photoelectric conversion efficiency, and can meet the requirements of the next generation of stacked cells. At present, the electrodes of HJT batteries mainly adopt the screen printing process, using low-temperature curing conductive silver paste. The low-temperature silver paste used for fine grid printing needs to have lower body resistance and contact resistance, high adhesion, high aspect ratio and excellent weather resistance, as well as excellent printability.
[0003] In the existing conductive silver paste, the silver powders are in surface or line contact with each other, which can improve the conductive properties of the conductive silver paste. The silver powder content of the conductive silver paste prepared by flaky silver powder can be appropriately reduced, that is, a conductive silver paste with low silver content and high conductivity is obtained. However, the printing performance and bending resistance of the conductive silver paste prepared by flaky silver powder will decrease accordingly. The spherical silver powders are in point contact with each other, which can improve the rheological properties of the silver paste and is suitable for solar panels with high requirements for mechanical properties such as printing characteristics and bending resistance. The disadvantage is that the conductive properties will decrease accordingly, so a higher silver powder content is required. At the same time, a high silver powder content will also increase the viscosity of the conductive silver paste, thereby affecting the printing adaptability of the conductive silver paste. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a high conductive silver paste for HJT battery and a preparation method thereof.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A high-conductivity silver paste for HJT batteries, comprising the following raw materials in parts by weight: 80-85 parts of doped silver powder, 5-8 parts of solvent, 3.2-5.5 parts of bisphenol A epoxy resin, 0.5-1.2 parts of curing agent, 1.5-3 parts of thixotropic agent, and 1.5-2.5 parts of dispersant;
[0007] The doped silver powder is prepared by the following steps:
[0008] The graphene oxide prepared by the Hummer's method is added to deionized water, and silver nitrate is added after stirring. After stirring for 2 hours, deionized water is added and stirred evenly to prepare solution a. The amount ratio of graphene oxide, silver nitrate and deionized water is controlled to be 0.1-0.2g:0.5g:20mL; under a 55°C water bath, a 35% mass fraction silver nitrate solution is slowly added dropwise to the mixed solution b, stirred at a uniform speed and reacted for 1 hour, then centrifuged, washed three times with deionized water, deionized water was added again, mixed evenly, solution a was added dropwise, the reaction was continued for 1 hour, centrifuged, washed, dried, and calcined at 450°C for 2 hours to prepare doped silver powder, and the volume ratio of solution a, silver nitrate solution and mixed solution b was 2:2.5-3:3.
[0009] Silver particles are prepared by a liquid phase reduction method using silver nitrate as a raw material, and graphene oxide is added during the synthesis of the silver particles. The graphene oxide is introduced onto the surface of the silver particles through the electrostatic interaction between the graphene oxide and the silver particles, which can solve the problem of weak mutual interaction caused by a single blend. The introduction of graphene oxide can increase the contact between the silver particles on the one hand, and the strong interaction caused by the close contact with the silver particles can improve the transfer efficiency of electrons at the interface of the silver particles. In addition, the introduced graphene oxide can fill the gaps between the silver powders, further improving the conductive properties.
[0010] Furthermore, the mixed solution b is prepared by mixing gum arabic, ascorbic acid and deionized water in a dosage ratio of 0.12-0.15 g: 9-10 mmol: 30 mL.
[0011] Furthermore, the solvent is a mixture of terpineol, diethylene glycol dimethyl ether and diethylene glycol butyl ether acetate in a volume ratio of 1:1:1.
[0012] Furthermore, the thixotropic agent is a mixture of one or more of hydrogenated castor oil, fumed silica and polyethylene wax in any proportion, the dispersant is an aliphatic amide dispersant (Dumeen TDO), and the bisphenol A epoxy resin is E44.
[0013] The curing agent comprises the following steps:
[0014] Step S1, adding 2,6-diaminopurine to anhydrous methanol, and slowly adding epichlorohydrin and sodium hydroxide while stirring after ultrasonic treatment for 30 minutes, heating to 85°C, and reflux reaction for 72 hours. After the reaction is completed, cooling to room temperature to obtain an intermediate, wherein the amount ratio of 2,6-diaminopurine, epichlorohydrin and anhydrous methanol is controlled to be 1-1.2 mmol: 5-8 mmol: 30 mL, and the amount of sodium hydroxide is 10-15% of the weight of 2,6-diaminopurine;
[0015] In step S1, the amino group on 2,6-diaminopurine reacts with epichlorohydrin to introduce an epoxy group into the structure of 2,6-diaminopurine to generate an intermediate.
[0016] Step S2, adding the obtained intermediate and ethylenediamine into anhydrous methanol, raising the temperature to 85°C, and keeping the temperature to react for 24 hours to obtain a curing agent, and controlling the usage ratio of the intermediate, ethylenediamine and anhydrous methanol to be 0.8-1mmol:4-5mmol:30mL.
[0017] In step S2, the epoxy group on the intermediate reacts with the amino group on ethylenediamine to prepare a curing agent. The curing agent uses 2,6-diaminopurine as a matrix and introduces multiple tertiary amine functional groups, which can promote the curing of epoxy resin according to the anionic polymerization mechanism, greatly shorten the curing time, and the hydroxyl groups in the structure can also participate in the curing process of the bisphenol A epoxy resin, further improving the curing efficiency. In addition, the large conjugated plane of the 2,6-diaminopurine molecule itself is tightly combined with the π-π interaction between graphene, which solves the problem of strong π-π interaction between carbon materials and easy agglomeration and sedimentation, thereby improving the dispersibility of graphene, preventing aggregation, and improving the uniformity of printing.
[0018] A method for preparing a highly conductive silver paste for a HJT battery comprises the following steps:
[0019] The first step is to add bisphenol A epoxy resin, thixotropic agent and dispersant into the solvent, stir evenly to prepare a mixed solution;
[0020] The second step is to add the doped silver powder and curing agent into the mixed solution and stir for 2 hours, then put it into a three-roll mill and roll it for 6 times. When the scraper fineness is less than 10μm, filter it to obtain a highly conductive silver paste.
[0021] Beneficial effects of the present invention:
[0022] The invention prepares a conductive silver paste, which uses doped silver powder as a raw material and can improve the conductive performance. In the preparation process of the doped silver powder, silver nitrate is used as a raw material, and silver particles are prepared by a liquid phase reduction method. In the synthesis process of the silver particles, graphene oxide is added, and the graphene oxide is introduced into the surface of the silver particles through the electrostatic interaction between the graphene oxide and the silver particles, so that the problem of weak mutual interaction caused by single blending can be solved. On the one hand, the contact between the silver particles can be increased by introducing the graphene oxide, and the strong interaction caused by the close contact with the silver particles can improve the transfer efficiency of electrons at the interface of the silver particles. In addition, the introduced graphene oxide can fill the gaps between the silver powders, so as to further improve the conductive performance.
[0023] The present invention also prepares a curing agent, which uses 2,6-diaminopurine as a matrix and introduces multiple tertiary amine functional groups, can promote the curing of epoxy resin according to the anionic polymerization mechanism, greatly shorten the curing time, and the hydroxyl groups in the structure can also participate in the curing process of the bisphenol A type epoxy resin, further improving the curing efficiency, and the large conjugated plane of the 2,6-diaminopurine molecule itself is tightly combined with the π-π interaction between graphene, solving the problem of strong π-π interaction between graphene and easy agglomeration and sedimentation, thereby improving the dispersibility of the doped silver powder, preventing aggregation, and improving the printing performance. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1: A highly conductive silver paste for HJT batteries, comprising the following raw materials in parts by weight: 80 parts of doped silver powder, 5 parts of solvent, 3.2 parts of bisphenol A epoxy resin, 0.5 parts of curing agent, 1.5 parts of thixotropic agent, and 1.5 parts of dispersant;
[0026] The method for preparing a highly conductive silver paste for a HJT battery comprises the following steps:
[0027] The first step is to add bisphenol A epoxy resin, thixotropic agent and dispersant into the solvent, stir evenly to prepare a mixed solution;
[0028] The second step is to add the doped silver powder and curing agent into the mixed solution and stir for 2 hours, then put it into a three-roll mill and roll it for 6 times. When the scraper fineness is less than 10μm, filter it to obtain a highly conductive silver paste.
[0029] The doped silver powder is prepared by the following steps:
[0030] The graphene oxide prepared by the Hummer's method was added to deionized water, and silver nitrate was added after stirring. After stirring for 2 hours, deionized water was added and stirred evenly to prepare solution a. The amount ratio of graphene oxide, silver nitrate and deionized water was controlled to be 0.1g:0.5g:20mL; under a 55°C water bath, a 35% mass fraction silver nitrate solution was slowly added dropwise to the mixed solution b, stirred at a uniform speed and reacted for 1 hour, then centrifuged, washed three times with deionized water, deionized water was added again, mixed evenly, solution a was added dropwise, the reaction was continued for 1 hour, centrifuged, washed, dried, and calcined at 450°C for 2 hours to prepare doped silver powder. The volume ratio of solution a, silver nitrate solution and mixed solution b was 2:2.5:3.
[0031] The mixed solution b is prepared by mixing gum arabic, ascorbic acid and deionized water in a dosage ratio of 0.12 g: 9 mmol: 30 mL.
[0032] The solvent is a mixture of terpineol, diethylene glycol dimethyl ether and diethylene glycol butyl ether acetate in a volume ratio of 1:1:1, the dispersant is an aliphatic amide dispersant Dumeen TDO, the thixotropic agent is hydrogenated castor oil, and the bisphenol A epoxy resin is E44.
[0033] The curing agent comprises the following steps:
[0034] Step S1, adding 2,6-diaminopurine to anhydrous methanol, and slowly adding epichlorohydrin and sodium hydroxide while stirring after ultrasonic treatment for 30 minutes, heating to 85°C, and reflux reaction for 72 hours. After the reaction is completed, cooling to room temperature to obtain an intermediate, wherein the amount ratio of 2,6-diaminopurine, epichlorohydrin and anhydrous methanol is controlled to be 1mmol:5mmol:30mL, and the amount of sodium hydroxide is 10-15% of the weight of 2,6-diaminopurine;
[0035] Step S2, adding the obtained intermediate and ethylenediamine into anhydrous methanol, raising the temperature to 85°C, and keeping the temperature to react for 24 hours to obtain a curing agent, and controlling the usage ratio of the intermediate, ethylenediamine and anhydrous methanol to be 0.8mmol:4mmol:30mL.
[0036] Example 2: A highly conductive silver paste for HJT batteries, comprising the following raw materials in parts by weight: 82 parts of doped silver powder, 6 parts of solvent, 4 parts of bisphenol A epoxy resin, 0.8 parts of curing agent, 2 parts of thixotropic agent, and 2 parts of dispersant;
[0037] The method for preparing a highly conductive silver paste for a HJT battery comprises the following steps:
[0038] The first step is to add bisphenol A epoxy resin, thixotropic agent and dispersant into the solvent, stir evenly to prepare a mixed solution;
[0039] The second step is to add the doped silver powder and curing agent into the mixed solution and stir for 2 hours, then put it into a three-roll mill and roll it for 6 times. When the scraper fineness is less than 10μm, filter it to obtain a highly conductive silver paste.
[0040] The doped silver powder is prepared by the following steps:
[0041] The graphene oxide prepared by the Hummer's method was added to deionized water, and silver nitrate was added after stirring. After stirring for 2 hours, deionized water was added and stirred evenly to prepare solution a. The amount ratio of graphene oxide, silver nitrate and deionized water was controlled to be 00.2g:0.5g:20mL; under a 55°C water bath, a 35% mass fraction silver nitrate solution was slowly added dropwise to the mixed solution b, stirred at a uniform speed and reacted for 1 hour, then centrifuged, washed three times with deionized water, deionized water was added again, mixed evenly, solution a was added dropwise, the reaction was continued for 1 hour, centrifuged, washed, dried, and calcined at 450°C for 2 hours to prepare doped silver powder. The volume ratio of solution a, silver nitrate solution and mixed solution b was 2:2.8:3.
[0042] The mixed solution b is prepared by mixing gum arabic, ascorbic acid and deionized water in a dosage ratio of 0.12 g: 9 mmol: 30 mL.
[0043] The solvent is a mixture of terpineol, diethylene glycol dimethyl ether and diethylene glycol butyl ether acetate in a volume ratio of 1:1:1, the dispersant is an aliphatic amide dispersant Dumeen TDO, the thixotropic agent is hydrogenated castor oil, and the bisphenol A epoxy resin is E44.
[0044] The curing agent comprises the following steps:
[0045] Step S1, adding 2,6-diaminopurine to anhydrous methanol, and slowly adding epichlorohydrin and sodium hydroxide while stirring after ultrasonic treatment for 30 minutes, heating to 85°C, and reflux reaction for 72 hours. After the reaction is completed, cooling to room temperature to obtain an intermediate, wherein the amount ratio of 2,6-diaminopurine, epichlorohydrin and anhydrous methanol is controlled to be 1.1mmol:6mmol:30mL, and the amount of sodium hydroxide is 10-15% of the weight of 2,6-diaminopurine;
[0046] Step S2, adding the obtained intermediate and ethylenediamine into anhydrous methanol, raising the temperature to 85°C, and keeping the temperature to react for 24 hours to obtain a curing agent, wherein the amount ratio of the intermediate, ethylenediamine and anhydrous methanol is controlled to be 0.9mmol:4.5mmol:30mL.
[0047] Example 3: A highly conductive silver paste for HJT batteries, comprising the following raw materials in parts by weight: 85 parts of doped silver powder, 8 parts of solvent, 5.5 parts of bisphenol A epoxy resin, 1.2 parts of curing agent, 3 parts of thixotropic agent, and 2.5 parts of dispersant;
[0048] The method for preparing a highly conductive silver paste for a HJT battery comprises the following steps:
[0049] The first step is to add bisphenol A epoxy resin, thixotropic agent and dispersant into the solvent, stir evenly to prepare a mixed solution;
[0050] The second step is to add the doped silver powder and curing agent into the mixed solution and stir for 2 hours, then put it into a three-roll mill and roll it for 6 times. When the scraper fineness is less than 10μm, filter it to obtain a highly conductive silver paste.
[0051] The doped silver powder is prepared by the following steps:
[0052] The graphene oxide prepared by the Hummer's method was added to deionized water, and silver nitrate was added after stirring. After stirring for 2 hours, deionized water was added and stirred evenly to prepare solution a. The amount ratio of graphene oxide, silver nitrate and deionized water was controlled to be 0.2g:0.5g:20mL; under a 55°C water bath, a 35% mass fraction silver nitrate solution was slowly added dropwise to the mixed solution b, stirred at a uniform speed and reacted for 1 hour, then centrifuged, washed three times with deionized water, deionized water was added again, mixed evenly, solution a was added dropwise, the reaction was continued for 1 hour, centrifuged, washed, dried, and calcined at 450°C for 2 hours to prepare doped silver powder, and the volume ratio of solution a, silver nitrate solution and mixed solution b was 2:3:3.
[0053] The mixed solution b is prepared by mixing gum arabic, ascorbic acid and deionized water in a dosage ratio of 0.12 g: 9 mmol: 30 mL.
[0054] The solvent is a mixture of terpineol, diethylene glycol dimethyl ether and diethylene glycol butyl ether acetate in a volume ratio of 1:1:1, the dispersant is an aliphatic amide dispersant Dumeen TDO, the thixotropic agent is hydrogenated castor oil, and the bisphenol A epoxy resin is E44.
[0055] The curing agent comprises the following steps:
[0056] Step S1, adding 2,6-diaminopurine to anhydrous methanol, and slowly adding epichlorohydrin and sodium hydroxide while stirring after ultrasonic treatment for 30 minutes, heating to 85°C, and reflux reaction for 72 hours. After the reaction is completed, cooling to room temperature to obtain an intermediate, wherein the amount ratio of 2,6-diaminopurine, epichlorohydrin and anhydrous methanol is controlled to be 1.2mmol:8mmol:30mL, and the amount of sodium hydroxide is 15% of the weight of 2,6-diaminopurine;
[0057] Step S2, adding the obtained intermediate and ethylenediamine into anhydrous methanol, raising the temperature to 85°C, and keeping the temperature to react for 24 hours to obtain a curing agent, wherein the amount ratio of the intermediate, ethylenediamine and anhydrous methanol is controlled to be 1mmol:5mmol:30mL.
[0058] Comparative Example 1: Compared with Example 3, this comparative example uses commercially available silver powder instead of the doped silver powder of the present invention, and the rest is the same as Example 3.
[0059] Comparative Example 2: Compared with Example 3, this comparative example uses silver powder and graphene mixed in a weight ratio of 10:1 to replace the doped silver powder, and the rest is the same as Example 3.
[0060] Comparative Example 3: In this comparative example, the epoxy resin T-31 curing agent produced by a certain company on the market is used instead of the curing agent of the present invention, and the rest is the same as in Example 3.
[0061] The conductive pastes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were screen printed onto the TCO surface of the HJT battery and baked at 180° C. for 30 min. The silver paste was cured on the TCO surface to form an electrode. The contact resistivity was tested using the TLM method and the line width was measured using a 3D microscope. The results are shown in Table 1:
[0062] Table 1
[0063]
[0064] It can be seen from Table 1 above that the conductive silver pastes prepared in Examples 1 to 3 of the present invention have lower contact resistivity, finer grid width, better printing performance, and less light blocking.
[0065] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A highly conductive silver paste for HJT batteries, characterized in that: The method comprises the following raw materials in parts by weight: 80-85 parts of doped silver powder, 5-8 parts of solvent, 3.2-5.5 parts of bisphenol A epoxy resin, 0.5-1.2 parts of curing agent, 1.5-3 parts of thixotropic agent, and 1.5-2.5 parts of dispersant; The doped silver powder is prepared by the following steps: The graphene oxide prepared by Hummer's method was added to deionized water, and silver nitrate was added after stirring. After stirring for 2 hours, deionized water was added and stirred evenly to obtain solution a; in a 55°C water bath, a 35% silver nitrate solution was slowly added dropwise to the mixed solution b, stirred at a uniform speed and reacted for 1 hour, and then centrifuged. After washing with deionized water three times, deionized water was added again, mixed evenly, solution a was added dropwise, and the reaction was continued for 1 hour. The mixture was centrifuged, washed, dried, and calcined at 450°C for 2 hours to obtain doped silver powder; The mixed solution b is prepared by mixing gum arabic, ascorbic acid and deionized water in a dosage ratio of 0.12-0.15 g: 9-10 mmol: 30 mL; The curing agent is prepared by the following steps: Step S1, adding 2,6-diaminopurine to anhydrous methanol, and slowly adding epichlorohydrin and sodium hydroxide while stirring after ultrasonic treatment for 30 minutes, heating to 85° C., and reflux reaction for 72 hours. After the reaction is completed, cooling to room temperature to obtain an intermediate; Step S2, adding the obtained intermediate and ethylenediamine into anhydrous methanol, heating to 85° C., and keeping the temperature to react for 24 hours to obtain a curing agent; The amount ratio of graphene oxide, silver nitrate and deionized water in solution a is controlled to be 0.1-0.2 g: 0.5 g: 20 mL, and the volume ratio of solution a, silver nitrate solution and mixed solution b is 2: 2.5-3: 3; The solvent is a mixture of terpineol, diethylene glycol dimethyl ether and diethylene glycol butyl ether acetate in a volume ratio of 1:1:1; The thixotropic agent is a mixture of one or more of hydrogenated castor oil, fumed silica and polyethylene wax in any proportion, the dispersant is an aliphatic amide dispersant, and the bisphenol A epoxy resin is E44; In step S1, the dosage ratio of 2,6-diaminopurine, epichlorohydrin and anhydrous methanol is controlled to be 1-1.2mmol: 5-8mmol: 30mL, the dosage of sodium hydroxide is 10-15% of the weight of 2,6-diaminopurine, and in step S2, the dosage ratio of the intermediate, ethylenediamine and anhydrous methanol is controlled to be 0.8-1mmol: 4-5mmol: 30mL.
2. A method for preparing a highly conductive silver paste for HJT batteries as claimed in claim 1, characterized in that: The steps include: The first step is to add bisphenol A epoxy resin, thixotropic agent and dispersant into the solvent, stir evenly to prepare a mixed solution; The second step is to add the doped silver powder and curing agent into the mixed solution and stir for 2 hours, then put it into a three-roll mill and roll it for 6 times. When the scraper fineness is less than 10μm, filter it to obtain a highly conductive silver paste.