A method for preparing a high-rate lithium iron phosphate / carbon composite material

By constructing lithium iron phosphate/carbon composite materials with lithium iron reverse site defect and crystallographic strain, the problem of low rate performance of the positive electrode material of lithium iron phosphate battery is solved, high rate performance and cycle stability are achieved, and the preparation process is simplified. Reduced costs.

CN118281183BActive Publication Date: 2024-12-03TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410162705.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-12-03
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

Due to its structural characteristics, lithium ions can only diffuse in one-dimensional direction, resulting in low electronic conductivity and ionic conductivity, limiting its application in the field of fast charging batteries. The existing improvement methods are complex and costly.

Method used

By constructing the lattice strain in the reverse site defect of lithium iron and the AC direction, using rapid thermal shock and rapid cooling technology, lithium iron phosphate/carbon composite materials are prepared, providing more lithium ion diffusion channels and lattice expansion, and improving the magnification performance.

Benefits of technology

The significant discharge specific capacity improvement and cycle stability of lithium iron phosphate/carbon composite materials at a high current density of 10C are achieved, which simplifies the preparation process and reduces time and energy costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118281183B_ABST
    Figure CN118281183B_ABST
Patent Text Reader

Abstract

The present invention provides a method for ultrafast preparation of high-rate lithium iron phosphate / carbon composite materials. A lithium iron phosphate / carbon composite material with high-rate performance is obtained by directly subjecting a lithium iron phosphate precursor to ultrafast high-temperature thermal shock treatment. The lithium iron phosphate / carbon composite material finally obtained by the present invention has good crystallinity, and has a large number of lithium iron anti-site defects and crystalline lattice strain in the ac direction, which greatly improves the rate performance of the lithium iron phosphate / carbon composite material, and shows a rate performance that is superior to that of lithium iron phosphate prepared by traditional long-term tubular furnace sintering and commercial lithium iron phosphate. At a high current density of 10C, its discharge specific capacity can reach 110mAh / g, and after 2000 cycles, there is still a capacity retention rate of 84.8%, while the discharge specific capacity of commercial lithium iron phosphate can only reach 88mAh / g. The whole process can greatly simplify the preparation process of high-rate lithium iron phosphate / carbon composites, and both time cost and energy cost have been greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery positive electrode material preparation, and in particular to a method for preparing a high-rate lithium iron phosphate / carbon composite material. Background Art

[0002] Olivine-structured lithium iron phosphate battery cathode materials are widely used in electric vehicles and various large-scale energy storage devices due to their stable voltage, low cost, abundant raw materials, and better environmental friendliness. However, due to its own structural characteristics, lithium ions can only diffuse along the one-dimensional channel in the

[010] direction, and other channels are blocked by high energy barriers and cannot cross conduction. Therefore, lithium iron phosphate battery cathode materials have inherently low electronic conductivity and ionic conductivity. This makes lithium iron phosphate battery cathode materials have poor rate performance, limiting their further application in the field of fast-charging batteries.

[0003] At present, people mainly improve the rate performance of lithium iron phosphate battery positive electrode materials by doping, coating, nano-sizing particles and synthesizing particles with specific orientations. However, the above methods require relatively complex process means to achieve.

[0004] Among them, doping and coating mostly require the introduction of secondary sintering after the original primary sintering process to achieve the final effect, but its rate performance is still not ideal. The nano-size particle requires the use of nano-scale precursor particles with higher manufacturing costs or the introduction of other surfactants to obtain nano-scale particles. In addition, the synthesis of particles with specific orientation requires high-temperature and high-pressure hydrothermal reactions, which is a relatively dangerous process. Summary of the invention

[0005] The present invention aims to provide a lithium iron phosphate / carbon composite material with high rate performance, which effectively improves its rate performance by constructing lithium iron anti-site defects and crystalline gra strain in the ac direction. Moreover, the present invention cleverly utilizes the characteristics of rapid thermal shock and rapid temperature rise and fall to achieve ultra-fast preparation of the lithium iron phosphate / carbon composite material with lithium iron anti-site defects and crystalline gra strain in the ac direction.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a high-rate lithium iron phosphate / carbon composite material, which is carried out according to the following steps:

[0007] Step 1: FePO 4 , Li 2 CO 3 and carbon source to prepare lithium iron phosphate / carbon precursor; wherein FePO 4 , Li 2 CO 3 The molar ratio is 2:1.03;

[0008] Step 2, placing the lithium iron phosphate / carbon precursor powder obtained in step 1 on a heated substrate on a heating device in a protective atmosphere. First, rapid high-temperature heating causes the lithium iron phosphate / carbon precursor to decompose rapidly, and ultra-fast diffusion of lithium atoms and iron atoms produces hasty occupation. At this time, the lithium ions occupying the iron site can provide new channels for the lithium ions to diffuse along the

[100] or

[001] direction other than the

[010] direction, so that the lithium ions have more diffusion channels during the charge and discharge process, and lattice expansion is generated at high temperature, followed by extremely short insulation, and finally rapid cooling to obtain the lithium iron phosphate / carbon composite material. Due to the extremely fast heating and cooling rate and extremely short insulation time, a large number of lithium iron anti-site defects and lattice expansion generated at high temperature are retained, and its reasonable lithium iron anti-site defect arrangement mode and quantity can make it show two-dimensional lithium ion diffusion, and if there is crystal lattice strain in the ac plane perpendicular to the lithium ion diffusion direction

[010] , it can also greatly broaden the lithium ion diffusion channel, realize rapid lithium ion diffusion, and have excellent high rate performance.

[0009] The heating and cooling rates are 10 3 -10 5 ℃ / s; the extremely short insulation heating treatment temperature is 600-900℃, and the extremely short insulation heating treatment time is 5-60s.

[0010] Further, the ball milling method for preparing lithium iron phosphate / carbon precursor in step 1 is as follows: first, FePO 4 , Li 2 CO 3 , and pre-grind it in a mortar. Add a carbon source to the powder obtained after the pre-grinding, and then put the obtained mixed powder into a ball mill for wet grinding in a ball milling aid. Finally, put the powder obtained after ball milling into a vacuum oven for drying, and grind the dried powder to obtain lithium iron phosphate / carbon precursor powder.

[0011] Furthermore, the ball milling conditions of the ball milling method described in step 1 are: ball milling speed: 200-2000r / min, ball milling time is 2-12h, and ball milling aids include ethanol, water, acetone, etc. and other solutions that can play a dispersing role.

[0012] Furthermore, the carbon source described in step 1 can be an organic carbon source such as glucose, sucrose, etc., an inorganic carbon source such as carbon nanotubes, acetylene black, Ketjen black, etc., or a combination of the two.

[0013] Furthermore, the protective atmosphere in step 2 is argon, helium or nitrogen.

[0014] Furthermore, the heating substrate in step 2 can be a series of materials with high melting point and good thermal conductivity, such as carbon cloth, carbon paper, carbon felt, graphite sheet, nickel foil, cobalt foil, stainless steel sheet, etc.

[0015] Preferably, the extremely short heat preservation and heating treatment temperature in step 2 is 700° C., and the extremely short heat preservation and heating treatment time is 20 s.

[0016] The beneficial results of the present invention are: the lithium iron phosphate / carbon composite material obtained by the present invention can reach a discharge capacity of 110mAh / g at a high current density of 10C, and still has a capacity retention rate of 84.8% after 2000 cycles, which is a significant improvement over commercial lithium iron phosphate (discharge capacity can only reach 88mAh / g). The present invention also greatly simplifies the preparation process of high-rate lithium iron phosphate / carbon composite, and the time cost and energy cost are greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is the Fourier transform infrared spectrum of the high-rate lithium iron phosphate / carbon composite material prepared in the present invention;

[0018] Figure 2 (a) is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of the high-rate lithium iron phosphate / carbon composite material prepared in the present invention in the

[010] direction; 2(b) is an enlarged view of the area within the rectangular frame in the figure; 2(c) is a geometric phase analysis (GPA) image corresponding to figure (a)

[0019] Figure 3 (a) is a high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of lithium iron phosphate / carbon composite material prepared by conventional calcination process in the

[010] direction; 3(b) is an enlarged view of the area within the rectangular frame in the figure; 3(c) is the geometric phase analysis (GPA) image corresponding to Figure (a)

[0020] Figure 4 This is a comparison chart of the rate performance of the high-rate lithium iron phosphate / carbon composite material prepared in the present invention and commercial lithium iron phosphate / carbon composite materials;

[0021] Figure 5 This is a 10C long cycle performance comparison chart of the high-rate lithium iron phosphate / carbon composite material prepared in the present invention and the commercial lithium iron phosphate / carbon composite material;

[0022] Figure 6 It is the XRD spectrum of the high-rate lithium iron phosphate / carbon composite material prepared in the present invention;

[0023] Figure 7It is a 10C long cycle performance diagram of the high-rate lithium iron phosphate / carbon composite material (sample 3) prepared in the present invention. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below through specific embodiments.

[0025] Example 1

[0026] Step 1: weigh FePO in a molar ratio of 2:1.03 4 , Li 2 CO 3 , and pre-grind it in a mortar. After the pre-grinding, add 1.0 molar ratio of glucose as a carbon source to the powder obtained, and then put the obtained mixed powder into a ball mill in ethanol as a ball milling aid for 6 hours at a speed of 600r / min. Finally, put the powder obtained after ball milling into a vacuum oven at 100℃ and dry it for 12 hours. Grind the dried powder to obtain lithium iron phosphate / carbon precursor powder.

[0027] Step 2: Place the lithium iron phosphate / carbon precursor powder obtained in step 1 on a heated carbon cloth on a heating device in an argon protective atmosphere. 5 The lithium iron phosphate / carbon precursor was heated at a rapid high temperature at a heating rate of 10 °C / s, which caused the atoms in the lithium iron phosphate / carbon precursor to diffuse rapidly and occupy the space hastily, and the lattice expanded at high temperature; then the mixture was kept at 700 °C for 25 s, and finally heated at 10 5 The lithium iron phosphate / carbon composite material can be obtained by rapidly cooling the temperature at a cooling rate of ℃ / s.

[0028] Figure 1 is the Fourier transform infrared spectrum of the high-rate lithium iron phosphate / carbon composite material prepared in this example. -1 The corresponding characteristic peaks indicate the presence of lithium-iron anti-site defects in the material.

[0029] Figure 2 (a) (b) are high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) images of the high-rate lithium iron phosphate / carbon composite material prepared in this embodiment in the

[010] direction. Figure 2 The signal of the lithium site pointed by the green arrow in (b) indicates that the iron atom occupies the site at this time, indicating that there is a lithium-iron anti-site defect in the material. In addition, since lithium ions diffuse one-dimensionally along the

[010] direction in the lithium iron phosphate positive electrode material, the ac plane perpendicular to the lithium ion diffusion direction is seen along this direction. GPA analysis can obtain the strain distribution in the electron microscope image. When there is tensile strain in this area, the image is red and other warm colors, and when there is compressive strain, the image is green and other cold colors. Figure 2(c) Figure 2 (a) The corresponding GPA result, the entire figure appears red, indicating that the high-rate lithium iron phosphate / carbon composite material prepared in this embodiment has obvious tensile strain on the ac plane perpendicular to the lithium ion diffusion direction, and the high-temperature lattice expansion is retained.

[0030] In addition, the lithium iron phosphate / carbon precursor powder obtained in step 1 is placed in a conventional tube furnace in a protective atmosphere of argon, heated to 700°C at a heating rate of 5°C / min, and kept at 700°C for 10 hours to obtain a lithium iron phosphate / carbon composite material prepared by a conventional method for comparison.

[0031] Figure 3 (a) (b) are high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) images of the lithium iron phosphate / carbon composite material prepared according to the conventional method in the

[010] direction in this embodiment, Figure 3 There is no obvious signal at the lithium site pointed by the green arrow in (b), indicating that the site is still occupied by lithium atoms. Due to the slow heating and cooling rate and long-term high-temperature insulation, the atoms of the lithium iron phosphate / carbon composite material prepared by the conventional method have diffused to the equilibrium site, and there is no lithium-iron anti-site defect. Figure 3 (c) Figure 3 (a) The corresponding GPA result, the whole figure is uniformly distributed in red and green, indicating that the tensile and compressive strains in this area are balanced, and the lithium iron phosphate / carbon composite material prepared by the conventional method does not have lattice expansion along the ac plane. It can be seen that the slow heating of the tube furnace can control the nucleation rate to a certain extent. In the slow nucleation process, the atoms in the lattice are conducive to occupying the equilibrium position, and the subsequent long-term annealing process can make some non-equilibrium atoms diffuse to the equilibrium state through a specific crystal plane, so that the lithium iron atoms originally occupying the anti-site return to the equilibrium site, and this process will eliminate the lattice expansion generated at high temperature during the slow cooling process.

[0032] Table 1 is a comparison table of the unit cell volumes of the high-rate lithium iron phosphate / carbon composite material (sample 1) prepared in this embodiment and the commercial lithium iron phosphate / carbon composite material obtained by conventional tube furnace heat treatment method. The larger unit cell parameters of sample 1 in the a and c directions indicate that compared with the commercial sample, it also has lattice expansion in the ac plane.

[0033] Table 1

[0034]

[0035] Figure 4This is a comparison chart of the rate performance of the high-rate lithium iron phosphate / carbon composite material (blue) prepared in this embodiment and the commercial lithium iron phosphate / carbon composite material (green) obtained by a conventional tube furnace heat treatment method. It shows that the lithium iron phosphate / carbon composite material with lithium iron anti-site defects and crystal lattice strain prepared by the present invention has a rate performance far superior to that of the existing commercial lithium iron phosphate / carbon composite material.

[0036] Figure 5 This is a 10C long cycle performance comparison chart of the high-rate lithium iron phosphate / carbon composite material (blue) prepared in this embodiment and the commercial lithium iron phosphate / carbon composite material (green) obtained by the conventional tube furnace heat treatment method. It shows that the lithium iron phosphate / carbon composite material with lithium iron anti-site defects and crystal lattice strain prepared by the present invention has a cycle stability far superior to that of the commercial lithium iron phosphate / carbon composite material at a high rate of 10C, and its structure is stable.

[0037] Example 2

[0038] Step 1: weigh FePO in a molar ratio of 2:1.03 4 , Li 2 CO 3 , and pre-grind it in a mortar. After the pre-grinding, add 0.5 molar ratio of sucrose as a carbon source to the powder obtained, and then put the obtained mixed powder into a ball mill in acetone, a ball milling aid, and wet grind it at a speed of 600r / min for 4h. Finally, put the powder obtained after ball milling into a vacuum oven at 100℃ and dry it for 12h. Grind the dried powder to obtain lithium iron phosphate / carbon precursor powder.

[0039] Step 2: Place the lithium iron phosphate / carbon precursor powder obtained in step 1 on a heated carbon cloth on a heating device in an argon protective atmosphere. 4 The lithium iron phosphate / carbon precursor was heated at a heating rate of 10 °C / s to cause ultrafast diffusion of atoms in the lithium iron phosphate / carbon precursor, resulting in hasty occupation of space and lattice expansion at high temperature. The mixture was then kept at 600 °C for 35 s and then heated at 10 °C / s. 4 The lithium iron phosphate / carbon composite material can be obtained by rapidly cooling the temperature at a cooling rate of ℃ / s.

[0040] In this embodiment, the protective atmosphere may also be helium or nitrogen; the heating substrate may also be a series of materials with high melting point and good thermal conductivity, such as carbon cloth, carbon felt, graphite sheet, nickel foil, cobalt foil, stainless steel sheet, etc.

[0041] Figure 6 The XRD spectrum of the high-rate lithium iron phosphate / carbon composite material obtained in this example is shown in Figure 1. It can be clearly seen that the lithium iron phosphate / carbon composite material prepared by this method is a pure phase.

[0042] Table 2 shows the unit cell volume of the high-rate lithium iron phosphate / carbon composite material obtained in this example and the ratio of lithium iron anti-site defects obtained by XRD refinement. The results show that compared with the lithium iron phosphate / carbon composite material synthesized in a conventional tubular furnace in Example 1, the material has obvious lattice expansion in the ac direction, and a certain amount of lithium iron anti-site defects exists in the material.

[0043] Table 2

[0044]

[0045] Using the same testing method as in Example 1, the lithium iron phosphate / carbon composite material obtained in this example can achieve a discharge specific capacity of 107 mAh / g at a high current density of 10 C, and still has a capacity retention rate of 100% after 500 cycles.

[0046] Example 3

[0047] Step 1: weigh FePO in a molar ratio of 2:1.03 4 , Li 2 CO 3 , and pre-grind it in a mortar. After the pre-grinding, Ketjen black is added to the powder obtained as a carbon source, and then the mixed powder is put into a ball mill in ultrapure water as a ball milling aid for wet grinding at a speed of 1500r / min for 2h. Finally, the powder obtained after ball milling is placed in a vacuum oven at 120℃ and dried for 8h. The dried powder is ground to obtain lithium iron phosphate / carbon precursor powder.

[0048] Step 2: Place the lithium iron phosphate / carbon precursor powder obtained in step 1 on a heated carbon cloth on a heating device in an argon protective atmosphere. 3 The lithium iron phosphate / carbon precursor was heated at a rapid high temperature at a heating rate of 10 °C / s, which caused the atoms in the lithium iron phosphate / carbon precursor to diffuse rapidly and occupy the space hastily, and the lattice expansion occurred at high temperature; then the mixture was kept at 800 °C for 15 s, and finally heated at 10 3 The lithium iron phosphate / carbon composite material can be obtained by rapidly cooling the temperature at a cooling rate of ℃ / s.

[0049] Table 3 shows the unit cell volume of the high-rate lithium iron phosphate / carbon composite material obtained in this example and the ratio of lithium iron anti-site defects obtained by XRD refinement. The results show that compared with the lithium iron phosphate / carbon composite material synthesized in a conventional tubular furnace in Example 1, the material has obvious lattice expansion in the ac direction, and a certain amount of lithium iron anti-site defects exists in the material.

[0050] Table 3

[0051]

[0052] The same test method as in Example 1 was used. Figure 7 As shown, the lithium iron phosphate / carbon composite material obtained in this embodiment can achieve a discharge specific capacity of 100 mAh / g at a high current density of 10C, and still has a capacity retention rate of 91.3% after 1000 cycles.

[0053] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A method for preparing a high-rate lithium iron phosphate / carbon composite material, characterized in that: The composite material has lithium iron anti-site defects and crystal lattice strain in the ac direction, and is prepared by the following method: Step 1, ball milling FePO4, Li2CO3 and a carbon source to prepare a lithium iron phosphate / carbon precursor; wherein the molar ratio of FePO4 to Li2CO3 is 2:1.03; Step 2, placing the lithium iron phosphate / carbon precursor powder obtained in step 1 on a heated substrate on a heating device in a protective atmosphere, and subjecting it to a rapid thermal shock treatment to obtain a lithium iron phosphate / carbon composite material having lithium iron anti-site defects and crystal lattice strain in the ac direction; the rapid thermal shock heating and cooling rates are 10 3 -10 5 ℃ / s; the heat treatment temperature is 600-900℃, and the insulation heating treatment time of rapid thermal shock is 5-60s.

2. The method for preparing a high-rate lithium iron phosphate / carbon composite material according to claim 1, characterized in that: The protective atmosphere is argon, helium or nitrogen.

3. The method for preparing a high-rate lithium iron phosphate / carbon composite material according to claim 1, characterized in that: In step 1, the specific contents of preparing the lithium iron phosphate / carbon precursor include: First, FePO4 and Li2CO3 are weighed in a molar ratio of 2:1.03 and pre-grinded in a mortar; a carbon source is added to the powder obtained after pre-grinding, and the mixed powder is placed in a ball mill for wet grinding in a ball milling aid, and finally the powder obtained after ball milling is placed in a vacuum oven for drying, and the dried powder is ground to obtain lithium iron phosphate / carbon precursor powder.

4. The method for preparing a high-rate lithium iron phosphate / carbon composite material according to claim 3, characterized in that: The carbon source is selected from an organic carbon source and / or an inorganic carbon source. The organic carbon source is one or more of glucose and sucrose, and the inorganic carbon source is one or more of carbon nanotubes, acetylene black, and Ketjen black.

5. The method for preparing the high-rate lithium iron phosphate / carbon composite material according to claim 3, characterized in that: The ball milling conditions are as follows: ball milling speed: 200-2000 r / min, ball milling time is 2-12 h, and a ball milling aid is used to disperse the ball milling material, which is selected from one or more of ethanol, water, and acetone.

6. The method for preparing a high-rate lithium iron phosphate / carbon composite material according to claim 3, characterized in that: The drying conditions in the vacuum oven are as follows: heating temperature is 80-120° C., and heating time is 6-24 hours.

7. The method for preparing a high-rate lithium iron phosphate / carbon composite material according to claim 1, characterized in that: In step 2, the heating substrate is carbon cloth, carbon paper, carbon felt, graphite sheet, nickel foil, cobalt foil or stainless steel sheet.