Multilayer polyimide film and its preparation method

By adjusting the ratio of dianhydride and diamine, a multilayer polyimide film was prepared, which solved the problems of dimensional instability and insufficient adhesion of polyimide film during high-temperature lamination. This resulted in low dielectric loss and high adhesion at high frequencies, making it suitable for high-frequency and high-speed communication.

CN118284513BActive Publication Date: 2026-11-10PI ADVANCED MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280077278.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-11-23
Publication Date
2026-11-10
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing polyimide films are dimensionally unstable and have insufficient adhesion during high-temperature lamination, and their dielectric constant and dielectric loss rate cannot meet the requirements of high-frequency and high-speed communication at high frequencies.

Method used

By adjusting the ratio of dianhydride and diamine components, a multilayer polyimide film structure, including a core layer and a surface layer, is formed. The dielectric loss rate and adhesion are optimized. The multilayer polyimide film is prepared by co-extrusion and imidization processes.

Benefits of technology

A multilayer polyimide film with low dielectric loss and high adhesion at high frequencies was achieved, making it suitable for high-frequency and high-speed communication and ensuring circuit stability and electrical insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004850172390000121
    Figure BDA0004850172390000121
  • Figure BDA0004850172390000122
    Figure BDA0004850172390000122
  • Figure BDA0004850172390000131
    Figure BDA0004850172390000131
Patent Text Reader

Abstract

The present invention provides a multilayer polyimide film and a method for preparing the same. The multilayer polyimide film includes at least one surface layer formed on at least one outer side of the core layer, and has a dielectric loss rate of less than 0.003 and an adhesion of more than 1000 gf / cm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a multilayer polyimide film with low dielectric properties and excellent adhesion, and a method for preparing the same. Background Technology

[0002] Polyimide (PI) is a polymer material based on a rigid aromatic backbone and an imide ring with excellent chemical stability. It also has the highest level of heat resistance, chemical resistance, electrical insulation, chemical resistance and weather resistance among organic materials.

[0003] Moreover, due to its excellent electrical properties such as insulation and low dielectric constant, it has attracted much attention as a high-functionality polymer material in fields such as microelectronics and optics.

[0004] In the field of microelectronics, for example, due to the trend towards lightweight and miniaturized electronic products, there is a strong demand for highly integrated and flexible thin circuit boards. These thin circuit boards increasingly utilize structures where circuitry, including metal foil, is formed on polyimide films that possess excellent heat resistance, low-temperature resistance, and insulation properties, and are easily bendable. Broadly speaking, this type of thin circuit board is also called a flexible metal-clad laminate. As an example, when a thin copper plate is used as the metal foil, it is narrowly referred to as a flexible copper-clad laminate (FCCL). Furthermore, polyimide can also be used as a protective film, insulating film, etc., for thin circuit boards.

[0005] Methods for preparing flexible metal-coated laminates include, for example: (i) casting or coating polyamic acid, a polyimide precursor, onto a metal foil followed by imidization; (ii) metallization, in which a metal layer is directly deposited on a polyimide film by sputtering or gold plating; and (iii) lamination, in which a polyimide film is bonded to a metal foil using heat and pressure with a thermoplastic polyimide.

[0006] Among these methods, lamination offers advantages such as a wider range of applicable foil thicknesses compared to casting and lower equipment costs compared to metallization. Lamination equipment includes roller laminators or dual-belt presses that continuously laminate while the rolled material is being fed in. From a productivity standpoint, hot roller lamination, based on hot roller lamination equipment, is the most efficient.

[0007] However, for lamination, as mentioned earlier, the bonding of the polyimide film to the metal foil utilizes a thermoplastic resin. Therefore, in order to express the thermal fusion properties of this thermoplastic resin, it is necessary to apply heat of 300°C or higher to the polyimide film, or even heat of 400°C or higher, depending on the situation, close to or higher than the glass transition temperature (Tg) of the polyimide film.

[0008] Generally, the storage modulus of viscoelastic materials such as polyimide films is believed to decrease significantly in the temperature range above the glass transition temperature compared to the value at room temperature.

[0009] That is, when lamination is performed at high temperatures, the storage modulus of the polyimide film decreases significantly at high temperatures. At low storage modulus, the polyimide film becomes loose and may not exist in a flat shape after lamination. In other words, under lamination, the dimensional changes of the polyimide film can be said to be relatively unstable.

[0010] Another point to note is that the glass transition temperature of the polyimide film is significantly lower than the lamination temperature. Specifically, at the lamination temperature, the polyimide film has relatively high viscosity, resulting in relatively large dimensional changes. Therefore, there is a risk of a decrease in the appearance quality of the polyimide film after lamination.

[0011] Therefore, there is an urgent need for a technology that can solve the above problems and greatly improve processability.

[0012] On the other hand, with the recent integration of various functions into electronic devices, these devices require high computing and communication speeds. To meet these requirements, thin circuit boards with low dielectric loss at frequencies above 10 GHz are being developed to enable high-speed communication transmission.

[0013] To achieve high-frequency, high-speed communication, insulators with high impedance are needed that can maintain electrical insulation even at high frequencies.

[0014] Impedance is inversely proportional to the frequency at which it forms in an insulator and to the dielectric constant (Dk). Therefore, even at high frequencies, the dielectric constant should be reduced as much as possible to maintain insulation.

[0015] However, typical polyimide has a dielectric constant of around 3.4 to 3.6, which is not high enough to maintain adequate insulation in high-frequency communications. For example, in thin circuit boards used for high-frequency communications above 10 GHz, there is a possibility of partial or complete loss of insulation.

[0016] In addition, it is well known that the lower the dielectric constant of an insulator, the less harmful stray capacitance and noise will occur in thin circuit boards, which can largely eliminate the cause of communication delay. Therefore, minimizing the dielectric constant of polyimide is considered to be the most important factor for the performance of thin circuit boards.

[0017] It should also be noted that dielectric dissipation is inevitably generated through polyimide during high-frequency communication above 10 GHz.

[0018] The dielectric dissipation factor (Df) refers to the degree of energy wastage on a thin circuit board and is closely related to the signal transmission delay that determines communication speed. Therefore, minimizing the dielectric dissipation factor of polyimide is considered an important factor in the performance of thin circuit boards.

[0019] Therefore, there is an urgent need to develop a polyimide film with relatively low dielectric loss rate and high adhesion, which can achieve stable circuits, and an effective preparation method thereof.

[0020] The matters described in the prior art above are used to help understand the background of the invention and may include matters that are not known to a person skilled in the art.

[0021] [Existing Technical Documents]

[0022] [Patent Literature]

[0023] Patent document 1: Korean Patent Publication No. 10-2012-0133807. Summary of the Invention

[0024] One objective of this invention is to provide a multilayer polyimide film with excellent adhesion and relatively low dielectric loss rate, and an effective preparation method thereof. Specifically, a polyimide film is provided in which the types of dianhydrides, diamines and their proportions are determined, and polyimide resins with different components are formed into a multilayer, thus exhibiting both excellent adhesion and low dielectric loss at high frequencies.

[0025] Another objective of this invention is to provide a flexible copper-clad laminate comprising a multilayer polyimide film with excellent adhesion and relatively low dielectric loss rate, which is effective for high-frequency high-speed transmission and high-speed communication.

[0026] Therefore, the essential objective of this invention is to provide specific embodiments thereof.

[0027] However, the technical problems to be solved by the present invention are not limited to those mentioned above. Other technical problems not mentioned can be clearly understood by those skilled in the art from the following description.

[0028] To achieve the objectives described above, one aspect of the present invention provides a multilayer polyimide film comprising at least one surface layer formed on at least one outer surface of a core layer, wherein the dielectric loss rate is less than 0.003 and the adhesion is greater than 1000 gf / cm.

[0029] Another aspect of the present invention provides a flexible metal-coated laminate comprising the above-described multilayer polyimide film and conductive metal foil.

[0030] Another aspect of the present invention provides an electronic component comprising the above-described flexible metal foil laminate.

[0031] This invention provides a polyimide film with excellent low dielectric and adhesion properties by providing a polyimide film with adjusted ratios and reaction ratios of dianhydride and diamine components.

[0032] Another objective of this invention is to provide a flexible copper-clad laminate comprising a multilayer polyimide film with excellent adhesion and relatively low dielectric loss rate, which is effective for high-frequency high-speed transmission and high-speed communication. Detailed Implementation

[0033] The terms or words used in this specification and the scope of the patent application shall not be limited to their ordinary or dictionary meanings, but shall be interpreted only in accordance with the principle that “the inventor may appropriately define the concepts of terms in order to best explain his or her invention”, and shall be interpreted only in the meaning and concept that conforms to the technical idea of ​​the present invention.

[0034] Therefore, the embodiments described in this specification are merely one preferred embodiment of the present invention and do not represent all of the technical ideas of the present invention. It should be understood that at the time of this application, there may be various equivalents and variations that can be substituted for them.

[0035] Unless the context clearly indicates otherwise, singular expressions in this specification include plural expressions. In this specification, terms such as “comprising,” “possessing,” or “having” are used to specify the presence of a feature, number, step, constituent element, or combination thereof as an embodiment, and should be understood as not precluding the presence or additional possibility of one or more other features or numbers, steps, constituent elements, or combinations thereof.

[0036] In this specification, "dianhydride" means including its precursors or derivatives, which may not technically be dianhydrides, but nonetheless, reacting with diamines to form polyamic acid, which can be converted back into polyimide.

[0037] In this specification, "diamine" means including its precursors or derivatives, which may not technically be diamines, but nonetheless, reacting with dianhydrides to form polyamic acid, which can be converted back into polyimide.

[0038] In this specification, when a quantity, concentration, or other value or parameter is given by listing ranges, preferred ranges, or preferred upper and lower limits, it should be understood, regardless of whether the range is otherwise disclosed, that all ranges formed by any pair of any upper or preferred range values ​​and any lower or preferred range values ​​are specifically disclosed.

[0039] When a range of numerical values ​​is mentioned in this specification, unless otherwise stated, the range means all integers and fractions including their endpoints and within their range. This means that the scope of the invention is not limited to the specific values ​​mentioned in the definition of the range.

[0040] One embodiment of the present invention provides a multilayer polyimide film that may include at least one surface layer formed on at least one outer side of the core layer, having a dielectric loss rate of less than 0.003 and an adhesion strength of more than 1000 gf / cm.

[0041] In one embodiment, the multilayer polyimide film may include the surface layer formed on one outer side of the core layer and the opposite side of the outer side, respectively, and is composed of a three-layer structure.

[0042] The dianhydride and diamine components and their ratios formed on one outer side and the opposite side of the core layer may be the same or different.

[0043] Furthermore, the thickness of the surface layer formed on one outer side of the core layer and the opposite side of the outer side may be the same or different.

[0044] In one embodiment, the total thickness of the polyimide film with the above-mentioned three-layer structure can be more than 10 μm and less than 100 μm, the thickness of the core layer can be more than 70% and less than 95% of the total thickness of the multilayer polyimide film, and the sum of the thicknesses of the surface layers formed on one outer side of the core layer and the opposite side of the outer side can be more than 5% and less than 30% of the total thickness of the multilayer polyimide film.

[0045] For example, the thickness of the core layer can be 35 μm or more and 45 μm or less, and the thickness of the surface layer can be 2.5 μm or more and 7.5 μm or less.

[0046] If the thickness of the core layer and / or surface layer exceeds or falls below the aforementioned range, the dielectric loss rate of the multilayer polyimide film will increase, and its low dielectric properties or adhesion will decrease.

[0047] In one embodiment, the core layer can be obtained by imidizing a polyamic acid solution containing dianhydride and diamine components, wherein the dianhydride components include biphenyl dianhydride (BPDA) and pyromellitic dianhydride (PMDA), and the diamine components include p-phenylenediamine (PPD) and m-tolidine.

[0048] Alternatively, the aforementioned surface layer can be obtained by imidizing a polyamic acid solution containing dianhydride and diamine components. The dianhydride components include biphenyltetracarboxylic dianhydride and pyromellitic dianhydride, and the diamine components include p-phenylenediamine, meta-toluidine, and diaminodiphenyl ether (ODA).

[0049] In one embodiment, in the core layer, based on a total content of 100 mol% of the dianhydride components, the content of the biphenyltetracarboxylic dianhydride can be 50 mol% or more and 70 mol% or less, the content of the pyromellitictetracarboxylic dianhydride can be 30 mol% or more and 50 mol% or less, based on a total content of 100 mol% of the diamine components, the content of the p-phenylenediamine can be 60 mol% or more and 80 mol% or less, and the content of the meta-toluidine can be 20 mol% or more and 40 mol% or less.

[0050] In one implementation, the core layer may comprise a block copolymer comprising two or more blocks.

[0051] The block copolymer of the core layer may include a first block and a second block. Based on a total dianhydride content of 100 mol% in the polyimide film, the first block contains 50 mol% to 60 mol% of the biphenyl dianhydride. Based on a total diamine content of 100 mol% in the polyimide film, the second block contains 30 mol% to 40 mol% of meta-toluidine.

[0052] The first block can be obtained by imidizing biphenyltetracarboxylic dianhydride and p-phenylenediamine, and the second block can be obtained by imidizing meta-toluidine and pyromellitic dianhydride.

[0053] In addition, the biphenyltetracarboxylic dianhydride in the first block can be completely imidized with p-phenylenediamine, and the meta-toluidine in the second block can be completely imidized with pyromellitic dianhydride.

[0054] In one embodiment, in the aforementioned surface layer, based on a total content of 100 mol% for the aforementioned dianhydride components, the content of the aforementioned biphenyltetracarboxylic dianhydride may be 30 mol% or more and 50 mol% or less, the content of the aforementioned pyromellitictetracarboxylic dianhydride may be 50 mol% or more and 70 mol% or less, based on a total content of 100 mol% for the aforementioned diamine components, the content of the aforementioned p-phenylenediamine may be 5 mol% or more and 25 mol% or less, the content of the aforementioned meta-toluidine may be 60 mol% or more and 80 mol% or less, and the content of the aforementioned diaminodiphenyl ether may be 5 mol% or more and 25 mol% or less.

[0055] The p-phenylenediamine of this invention is a rigid monomer. As the p-phenylenediamine content increases, the synthesized polyimide has a more linear structure, which helps to improve the mechanical properties of the polyimide.

[0056] In addition, meta-toluidine, in particular, has a hydrophobic methyl group, which contributes to the low moisture absorption properties of polyimide films, and low moisture absorption properties are related to the dimensional stability of moisture.

[0057] The polyimide chain derived from biphenyl dianhydride of the present invention has a structure named charge transfer complex (CTC), that is, a regular linear structure in which the electron donor and electron acceptor are arranged close to each other, which enhances the intermolecular interaction.

[0058] This structure prevents the formation of hydrogen bonds with moisture, thus maximizing the reduction of the hygroscopicity of the polyimide film. The hygroscopicity of the polyimide film affects the reduction of moisture absorption rate, thereby affecting the dimensional stability against moisture.

[0059] In addition, pyromellitic dianhydride is a dianhydride component with a relatively rigid structure, which can impart appropriate elasticity to the polyimide film, and is therefore preferred.

[0060] For polyimide films to exhibit excellent dimensional stability, the dianhydride content ratio is crucial. For example, the lower the biphenyltetracarboxylic dianhydride content ratio, the less likely it is to be expected to achieve the low moisture absorption rate caused by the aforementioned CTC structure, and the lower the dimensional stability against moisture.

[0061] In addition, biphenyl dianhydride contains two benzene rings corresponding to the aromatic moiety, while pyromellitic dianhydride contains one benzene ring corresponding to the aromatic moiety.

[0062] In the dianhydride component, the increase in the content of pyromellitic dianhydride, based on the same molecular weight, can be understood as an increase in intramolecular imide groups. This can be understood as the ratio of imide groups derived from the aforementioned pyromellitic dianhydride on the polyimide polymer chain being relatively higher than that derived from biphenyltetracarboxylic dianhydride.

[0063] That is, the increase in the content of pyromellitic dianhydride can be regarded as a relative increase of imide groups, even relative to the entire polyimide film. Therefore, it is difficult to expect high dimensional stability against moisture caused by low moisture absorption.

[0064] Conversely, if the content of pyromellitic dianhydride is reduced, the rigid structure will be reduced relatively, and the elasticity of the polyimide film will drop below the desired level.

[0065] For this reason, when the content of biphenyl dianhydride exceeds the above range or the content of pyromellitic dianhydride is below the above range, the dimensional stability of the polyimide film will be low.

[0066] Conversely, if the content of biphenyl dianhydride is below the above range or the content of pyromellitic dianhydride exceeds the above range, it will also have an adverse effect on the dimensional stability of the polyimide film.

[0067] In this invention, the preparation of polyamic acid can be carried out by, for example, the following methods: (1) a method in which the diamine component is added in full to a solvent, and then a dianhydride component is added to make the diamine component substantially equimolar and polymerize; (2) a method in which the dianhydride component is added in full to a solvent, and then a diamine component is added to make the dianhydride component substantially equimolar and polymerize; (3) a method in which a portion of the diamine component is added to a solvent, and then a portion of the dianhydride component is mixed relative to the reactants at a ratio of about 95 to 105 mol%, the remaining diamine component is added, and then the remaining dianhydride component is added to make the diamine component and the dianhydride component substantially equimolar and polymerize; (4) a method in which a portion of the diamine compound is added to a solvent, and then a portion of the diamine compound is mixed relative to the reactants at a ratio of about 95 to 105 mol%, and then the remaining diamine component is added, and then the remaining dianhydride component is added to make the diamine component and the dianhydride component substantially equimolar and polymerize; After mixing at a ratio of 10%, other dianhydride components are added, followed by the remaining diamine components, so that the diamine components and dianhydride components are substantially equimolar and polymerized; (5) Method: In a solvent, a portion of the diamine component reacts with a portion of the dianhydride component to make one of them excess, forming a first composition; in another solvent, a portion of the diamine component reacts with a portion of the dianhydride component to make one of them excess, forming a second composition; then, the first and second compositions are mixed to complete the polymerization. At this time, when the first composition is formed, if the diamine component is in excess, the dianhydride component is in excess in the second composition; if the dianhydride component is in excess in the first composition, the diamine component is in excess in the second composition. The first and second compositions are mixed so that all the diamine components and dianhydride components used in the reaction are substantially equimolar and polymerized.

[0068] In this invention, the polymerization method of polyamic acid as described above can be defined as a random polymerization method. The polyimide film prepared from polyamic acid by the process described above is preferably applicable in order to maximize the effect of the present invention in improving dimensional stability and chemical resistance.

[0069] However, the polymerization method described above limits the utilization of the various excellent properties of the polyimide chain derived from the dianhydride component because the repeating units within the polymer chain described above are relatively short. Therefore, the polymerization method of polyamic acid that is particularly preferred in this invention is block polymerization.

[0070] On the other hand, the solvent used to synthesize polyamic acid is not particularly limited. Any solvent that can dissolve polyamic acid can be used, but amide solvents are preferred.

[0071] Specifically, the solvents mentioned above can be organic polar solvents, more specifically, they can be aprotic polar solvents, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methylpyrrolidone (NMP), γ-butyrolactone (GBL), and diethylene glycol dimethyl ether (Diglyme), but are not limited thereto, and can be used alone or in combination of two or more as needed.

[0072] In one example, N,N-dimethylformamide and N,N-dimethylacetamide are particularly preferred solvents.

[0073] In addition, fillers can be added during the preparation process of polyamic acid to improve various film properties such as lubricity, thermal conductivity, corona resistance, and ring hardness. The added fillers are not particularly limited; preferred examples include silica, titanium dioxide, alumina, silicon nitride, boron nitride, dicalcium phosphate, calcium phosphate, and mica.

[0074] The particle size of the filler is not particularly limited and can be determined according to the characteristics of the film to be modified and the type of filler added. Generally, the average particle size is 0.05 μm to 100 μm, preferably 0.1 μm to 75 μm, more preferably 0.1 μm to 50 μm, and especially preferably 0.1 μm to 25 μm.

[0075] If the particle size is below this range, it is difficult to show a modification effect; if it exceeds this range, there is a situation where the surface properties are greatly damaged or the mechanical properties are significantly reduced.

[0076] Furthermore, the amount of filler added is not particularly limited and can be determined according to the characteristics of the film to be modified or the particle size of the filler. Generally speaking, the amount of filler added relative to 100 parts by weight of polyimide is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight.

[0077] If the amount of filler added is below this range, it will be difficult to demonstrate the modifying effect of the filler; if it exceeds this range, there is a possibility that the mechanical properties of the film will be severely damaged. The method of adding the filler is not particularly limited, and any known method may be used.

[0078] In the preparation method of the present invention, the polyimide film can be prepared by thermal imidization and chemical imidization.

[0079] Alternatively, it can be prepared by a composite imidization method that combines thermal imidization and chemical imidization.

[0080] The aforementioned thermal imidization method is a method that uses heat sources such as hot air or infrared dryers to induce the imidization reaction without the use of chemical catalysts.

[0081] The above-mentioned thermal imidization method can heat-treat the gel film at a variable temperature ranging from 100°C to 600°C to imidize the amide groups present in the gel film. More specifically, the heat treatment can be carried out at 200°C to 500°C, and more specifically, at 300°C to 500°C, to imidize the amide groups present in the gel film.

[0082] However, during the formation of the gel film, a portion of the amic acid (approximately 0.1 mol% to 10 mol%) will be imidized. For this purpose, the polyamic acid composition can be dried at a variable temperature ranging from 50°C to 200°C, which can also be included in the scope of the above-mentioned thermal imidization method.

[0083] In the case of chemical imidization, polyimide films can be prepared using dehydrating agents and imidizing agents in accordance with methods known in the industry.

[0084] As an example of the composite imidization method, a polyimide film can be prepared by adding a dehydrating agent and an imidizing agent to a polyamic acid solution, heating it at 80°C to 200°C, preferably at 100°C to 180°C, and after partial curing and drying, heating it at 200°C to 400°C for 5 to 400 seconds.

[0085] On the other hand, the multilayer polyimide film of the present invention, as described to date, can be prepared by any one or more of co-extrusion or coating.

[0086] Co-extrusion is a method of preparing a multi-layered polyimide film by filling a storage tank with a polyamic acid solution or polyimide resin prepared by imidization, extruding multiple layers on a casting tape using a co-extrusion die, and then curing them. It has high productivity, and different types of polyimide resins can be miscible at the interface, which can ensure high interfacial adhesion reliability.

[0087] For example, the method for preparing a multilayer polyimide film according to the present invention includes: a first filling step, in which a first polyamic acid solution or a first polyimide resin (i.e., a first solution) prepared by imidizing the first polyamic acid solution is filled into a first storage tank; a second filling step, in which a second polyamic acid solution or a second polyimide resin (i.e., a second solution) prepared by imidizing the second polyamic acid solution is filled into a second storage tank; a co-extrusion step, in which a first flow path connected to the first storage tank, a second flow path and a third flow path respectively connected to the second storage tank are co-extruded through co-extrusion molds formed inside the first and second solutions; and a curing step, in which the co-extruded first and second solutions are cured.

[0088] The first polyamic acid solution is used to form the core layer, preferably prepared by polymerizing a dianhydride component containing biphenyl dianhydride (BPDA) and pyromellitic dianhydride (PMDA) with a diamine component containing p-phenylenediamine (PPD) and m-tolidine.

[0089] The second polyamic acid solution is used to form the surface layer, preferably prepared by polymerizing a dianhydride component containing biphenyltetracarboxylic dianhydride and pyromellitic dianhydride with a diamine component containing p-phenylenediamine, meta-toluidine and diaminodiphenyl ether (ODA).

[0090] On the other hand, when the first polyamic acid solution is used as the first solution and the second polyamic acid solution is used as the second solution, it is preferable to further include an imidization step of imidizing the co-extruded first solution and the second solution before the curing step.

[0091] The present invention provides a flexible metal foil laminate comprising the above-mentioned multilayer polyimide film and conductive metal foil.

[0092] The metal foil used is not particularly limited, but when the flexible metal foil laminate of the present invention is used for electronic or electrical equipment applications, it may be, for example, a metal foil including copper or copper alloys, stainless steel or alloys thereof, nickel or nickel alloys (including 42 alloy), aluminum or aluminum alloys.

[0093] In conventional flexible metal-coated laminates, copper foil, also known as rolled copper foil or electrolytic copper foil, is widely used and is preferably used in this invention. Additionally, rust-preventive layers, heat-resistant layers, or adhesive layers may be applied to the surface of these metal foils.

[0094] In this invention, the thickness of the metal foil is not particularly limited, as long as it is thick enough to fully perform its function according to its application.

[0095] The flexible metal foil laminate of the present invention may be a structure in which a metal foil is laminated on at least one side of the above-mentioned multilayer polyimide film.

[0096] The following detailed description of the invention's function and effects is provided through specific preparation examples and embodiments. However, these preparation examples and embodiments are merely illustrative and do not limit the scope of the invention.

[0097] Preparation example: Preparation of multilayer polyimide films

[0098] A first polyamic acid solution for preparing the core layer was prepared by block copolymerization of biphenyl dianhydride (BPDA), pyromellitic dianhydride (PMDA), p-phenylenediamine (PPD), and m-tolidine (MTD).

[0099] A second polyamic acid solution for preparing the surface layer was prepared by polymerizing biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, p-phenylenediamine, meta-toluidine, and diaminodiphenyl ether (ODA).

[0100] The composition and ratio of the core layer and the surface layer are shown in Table 1 below.

[0101] [Table 1]

[0102]

[0103] The first and second polyamic acid solutions prepared earlier were co-extruded and then cured after imidization, thereby preparing a three-layer polyimide film with the core layer as the center and the outer side of the core layer and the opposite side of the outer side formed respectively.

[0104] However, the core layer is prepared by co-extrusion of a first polyamic acid solution, and the surface layer is prepared by co-extrusion of a second polyamic acid solution.

[0105] When preparing the above-mentioned polyamic acid, the solvent is generally an amide solvent, and an aprotic solvent can be used, such as N,N'-dimethylformamide, N,N'-dimethylacetamide, N-methylpyrrolidone or a combination thereof.

[0106] The dianhydride and diamine components mentioned above can be added in powder, agglomerate, or solution form. Initially, they are added in powder form for the initial reaction, but to adjust the polymerization viscosity, they are preferably added in solution form.

[0107] The obtained polyamic acid solution can be mixed with an imidization catalyst and a dehydrating agent and coated onto a support.

[0108] Examples of catalysts used include tertiary amines (e.g., isoquinoline, β-methylpyridine, pyridine, etc.), and examples of dehydrating agents include acid anhydrides, but are not limited to these.

[0109] Examples and Comparative Examples

[0110] According to the preparation examples, while preparing a three-layer polyimide film, the thicknesses of the core layer and the surface layer were adjusted as shown in Table 2 below, and multilayer polyimide films of Examples 1 to 3 and Comparative Examples 1 to 8 were prepared.

[0111] However, Comparative Example 1 and Comparative Example 8 are equivalent to single-layer polyimide films.

[0112] [Table 2]

[0113]

[0114]

[0115] *The thickness of the surface layer in Table 2 above corresponds to the total thickness of the surface layers formed on one outer side of the core layer and the opposite side of the aforementioned outer side. That is, it corresponds to the total thickness of the two surface layers. The two surface layers are formed with the same thickness. Therefore, for example, the thickness of one surface layer of the multilayer (3-layer) polyimide film in Example 2 is 5 μm.

[0116] The dielectric loss rate (Df) and adhesion of the prepared polyimide film were measured and are shown in Table 3 below.

[0117] The methods for measuring dielectric loss rate (Df) and adhesion are as follows.

[0118] (1) Measurement of dielectric loss rate (Df)

[0119] The dielectric loss rate (Df) was measured by drying the sample in an oven at 130°C for 30 minutes and then placing it in an environment at 23°C and 50% relative humidity for 24 hours. The dielectric loss rate at 10 GHz was measured using a network analyzer from Keysight Technologies and an SPDR harmonic analyzer from QWED.

[0120] (2) Adhesion measurement

[0121] The adhesion test involved placing Innoflex (1 mil, epoxy resin type, Innox product) on both sides of a polyimide film, with a 1 oz copper foil on each side, followed by a protective PI film. The film was then heated to 180°C and subjected to a 30 MPa pressure for 1 hour for hot-pressing. The film was then cut into 15 mm widths and subjected to a 180° peel test.

[0122] [Table 3]

[0123]

[0124]

[0125] Measurement results show that the dielectric loss rate of the multilayer (3-layer) polyimide films in Examples 1 to 3 is less than 0.003 and the adhesion is more than 1000 gf / cm.

[0126] In contrast, the single-layer Comparative Example 1 is equivalent to the core layer of the multilayer polyimide film of Examples 1 to 3, with a thickness of 50 μm and very low adhesion.

[0127] In addition, the core layer and / or surface layer of Comparative Examples 2 to 7 are thicker or thinner than the multilayer polyimide films of Examples 1 to 3, resulting in increased dielectric loss rate and decreased low dielectric properties.

[0128] On the other hand, Comparative Example 8 is equivalent to the surface layer of the multilayer polyimide film of Examples 1 to 3. It is a single layer with a thickness of 50 μm, and its dielectric loss rate is increased while its low dielectric properties are decreased.

[0129] Therefore, it can be confirmed that the multilayer polyimide films of Examples 1 to 3 prepared within the suitable range of this invention have excellent low dielectric and adhesive properties, but when they exceed the suitable range of this invention, it is difficult to fully meet the low dielectric and adhesive properties of the multilayer polyimide films of this invention.

[0130] That is, it can be confirmed that the multilayer polyimide film with excellent low dielectric and adhesion properties and fully meets the diverse conditions applicable to various application fields is the multilayer polyimide film prepared within the suitable scope of this case.

[0131] The embodiments of the multilayer polyimide film and the method for preparing the multilayer polyimide film of the present invention are merely preferred embodiments that enable those skilled in the art to readily implement the present invention, and are not limited to the above embodiments. Therefore, the scope of the present invention is not limited thereto. Thus, the true scope of protection of the present invention should be determined based on the technical concept of the appended patent claims. Furthermore, various substitutions, modifications, and alterations can be implemented without departing from the technical concept of the present invention; this is self-evident to those skilled in the art, and the parts that can be easily modified by those skilled in the art are naturally included within the scope of the present invention.

[0132] Industrial applicability

[0133] This invention provides a polyimide film with excellent low dielectric and adhesion properties by providing a polyimide film with adjusted ratios and reaction ratios of dianhydride and diamine components.

[0134] Another objective of this invention is to provide a flexible copper-clad laminate comprising a multilayer polyimide film with excellent adhesion and relatively low dielectric loss rate, which is effective for high-frequency high-speed transmission and high-speed communication.

Claims

1. A multilayer polyimide film, wherein, The multilayer polyimide film includes at least one surface layer formed on at least one outer side of the core layer. The core layer comprises polyimide obtained by reacting a polyamic acid solution through an imidization reaction, wherein the polyamic acid solution contains dianhydride and diamine components. The dianhydride component comprises biphenyltetracarboxylic dianhydride and pyromellitic dianhydride, and the diamine component comprises p-phenylenediamine and meta-toluidine. Specifically, in the core layer, based on a total dianhydride content of 100 mol%, the content of biphenyltetracarboxylic dianhydride is 50 mol% to 70 mol%, and the content of pyromellitic dianhydride is 30 mol% to 50 mol%. In the core layer, based on a total diamine content of 100 mol%, the content of p-phenylenediamine is 60 mol% to 80 mol%, and the content of meta-toluidine is 20 mol% to 40 mol%. The resin forming the core layer and the surface layer is a polyimide resin. The polyamic acid in the core layer comprises a block copolymer consisting of two or more blocks. The block copolymer comprises a first block and a second block. Based on a total dianhydride content of 100 mol% in the polyimide film, the first block comprises 50 mol% to 60 mol% of biphenyl dianhydride. Based on a total diamine content of 100 mol% in the polyimide film, the second block comprises 30 mol% to 40 mol% of meta-toluidine. The dielectric loss rate of the multilayer polyimide film is below 0.003, and the adhesion is above 1000 gf / cm.

2. The multilayer polyimide film according to claim 1, wherein, The multilayer polyimide film includes a surface layer formed on one outer side of the core layer and the opposite side of the outer side, thus constituting a three-layer structure.

3. The multilayer polyimide film according to claim 2, wherein, The total thickness of the multilayer polyimide film is 10 μm or more and 100 μm or less, and the thickness of the core layer is 70% or more and 95% or less of the total thickness of the multilayer polyimide film. The sum of the thicknesses of the surface layers formed on one outer side and the opposite side of the core layer is more than 5% and less than 30% of the total thickness of the multilayer polyimide film.

4. The multilayer polyimide film according to claim 1, wherein, The surface layer is obtained by imidizing a polyamic acid solution containing dianhydride and diamine components. The dianhydride components include biphenyltetracarboxylic dianhydride and pyromellitic dianhydride, and the diamine components include p-phenylenediamine, meta-toluidine, and diaminodiphenyl ether.

5. The multilayer polyimide film according to claim 4, wherein, In the surface layer, based on a total dianhydride content of 100 mol%, the content of biphenyltetracarboxylic dianhydride is 30 mol% or more and 50 mol% or less, and the content of pyromellitic dianhydride is 50 mol% or more and 70 mol% or less. In the surface layer, based on a total diamine content of 100 mol%, the content of p-phenylenediamine is 5 mol% or more and 25 mol% or less, the content of meta-toluidine is 60 mol% or more and 80 mol% or less, and the content of diaminodiphenyl ether is 5 mol% or more and 25 mol% or less.

6. The multilayer polyimide film according to any one of claims 1 to 5, wherein, The multilayer polyimide film is prepared by any one or more methods selected from the group consisting of co-extrusion and coating.

7. A flexible metal foil-coated laminate comprising a multilayer polyimide film according to any one of claims 1 to 5; and a conductive metal foil.

8. An electronic component comprising the flexible metal foil-coated laminate according to claim 7.

Citation Information

Patent Citations

  • Method for Preparing Multilayered Polyimide Film and Multilayered Polyimide Film by the Method

    KR1020120133807A

  • Low-dielectric loss multi-layer polyimide film having excellent adhesive strength and manufacturing method therefor

    CN113677531A

  • Method for producing a polyimide film, the polyimide film manufactured by the method, and multilayer film, flexible metal foil laminate and electronic component containing the same

    TW202120606A