A production process for environmentally friendly coating material

By mixing polylactic acid with additives such as surface improvers and modified glass powder and preparing it in an extruder, the problems of difficult degradation and poor mechanical strength of traditional coating materials are solved, and an environmentally friendly film suitable for a variety of packaging applications is prepared. The coating material achieves the combination of environmental protection and high performance.

CN118307822BActive Publication Date: 2024-10-18GUANGDONG MEISHIDA MEDICINE PACKAGING MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410584423.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-10-18
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

Traditional coating materials use materials such as polyvinyl chloride that are difficult to degrade, causing environmental pollution, and have poor mechanical strength, affecting performance.

Method used

Using polylactic acid as the main raw material, adding surface improvers, modified glass powder, antioxidants, plasticizers, lubricants and light stabilizers, after drying, mixing and melting and extrusion in the extruder, through the blow molding mechanism Prepare environmentally friendly coating materials.

Benefits of technology

An environmentally friendly coating material with good transparency, toughness, weather resistance, hydrolysis resistance and mechanical strength is prepared, which is suitable for various application scenarios such as food packaging and book covers. The process is simple and low-cost, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of coating technology, and specifically to a production process of an environmentally friendly coating material, which is used to solve the problems that existing coating materials are difficult to degrade, easily cause environmental pollution, and have poor mechanical strength. The production process selects polylactic acid as the main raw material. Polylactic acid is a polymer material with good biocompatibility and complete biodegradability, does not contain toxic and harmful substances, and is environmentally friendly. After adding a surface improver thereto, the hydrophobicity of the polylactic acid can be effectively improved, and certain mechanical properties can also be improved. After that, adding modified glass powder can greatly improve the mechanical properties of the polylactic acid, and the shortcomings of high brittleness and low toughness of the polylactic acid can also be improved. Therefore, the prepared coating material has good transparency, toughness, weather resistance, hydrolysis resistance, stain resistance, mechanical strength and other properties, meets the requirements of the packaging industry for coating materials, and has broad market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of film coating technology, and in particular to a production process of an environmentally friendly film coating material. Background Art

[0002] Lamination is a surface processing technology for printing paper, also known as post-printing lamination, post-printing gluing or post-printing film pasting. It refers to the use of a laminating machine to cover the surface of the printed product with a layer of 0.012-0.020mm thick transparent plastic film to form a paper-plastic integrated product processing technology.

[0003] The laminating process is widely used in the packaging industry. However, in the traditional laminating production process, most of the traditional laminating materials use difficult-to-degrade materials such as polyvinyl chloride. These materials decompose very slowly in the natural environment, causing long-term pollution to the environment. PLA materials have similar physical and chemical properties to traditional plastics, and are also biodegradable, which can effectively improve environmental pollution problems. However, compared with general plastics, PLA is brittle, has low tear strength, and low elongation at break, which greatly affects its performance.

[0004] Therefore, developing an environmentally friendly, degradable coating material with excellent mechanical strength has important social and economic significance. Summary of the invention

[0005] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a production process of an environmentally friendly coating material: by drying polylactic acid, and then adding it together with a surface improver, modified glass powder, an antioxidant, a plasticizer, a lubricant, and a light stabilizer into a mixer for stirring and mixing to obtain a mixture, adding the mixture into an extruder for melt extrusion, and blow-molding it into a film with a blow molding machine to obtain an environmentally friendly coating material, thereby solving the problems that existing coating materials are difficult to degrade, easily cause environmental pollution, and have poor mechanical strength.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A production process of an environmentally friendly coating material comprises the following steps:

[0008] Step 1: Weigh 70-80 parts of polylactic acid, 2-12 parts of surface improver, 6.5-13.5 parts of modified glass powder, 0.8-1.6 parts of antioxidant, 0.5-1.3 parts of plasticizer, 0.3-0.9 parts of lubricant and 0.2-0.6 parts of light stabilizer according to weight parts, and set aside;

[0009] Step 2: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 60-65° C. for 2-3 hours, then adding it into a mixer together with a surface improver, modified glass powder, antioxidant, plasticizer, lubricant, and light stabilizer, stirring and mixing it at a temperature of 45-55° C. and a stirring rate of 400-500 r / min for 40-60 minutes to obtain a mixed material;

[0010] Step 3: Add the mixed material into the extruder for melt extrusion, and blow it into a film through a blow molding machine to obtain an environmentally friendly coating material.

[0011] As a further solution of the present invention: the surface improver is prepared by the following steps:

[0012] Step a1: magnesium chips, iodine particles, bromoethane and anhydrous tetrahydrofuran are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and stirred for reaction for 20-30 minutes at a temperature of 30-35° C. and a stirring rate of 400-500 r / min, then 1-chloro-3,3,3-trifluoropropane is added dropwise while stirring, and the dropping rate is controlled to be 1-2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 20-30 minutes, and then paraformaldehyde is added and the stirring reaction is continued for 5-10 minutes, and then the temperature is raised to 55-60° C. and the stirring reaction is continued for 2-3 hours. After the reaction is completed, the reaction product is cooled to 0-5° C., and then added to a hydrochloric acid solution, and then allowed to stand for stratification, the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;

[0013] Step a2: methyl 2-chloroisonicotinate, 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, anhydrous potassium carbonate, tetrakis(triphenylphosphine)palladium, anhydrous ethanol and toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25-30° C. and a stirring rate of 400-500 r / min for 20-30 min, and then the temperature is raised to reflux and the stirring reaction is continued for 20-25 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to distilled water, and then extracted with dichloromethane for 2-3 times, the extracts are combined, and then the extracts are rotary evaporated to remove the solvent to obtain intermediate 2;

[0014] Step a3: Add intermediate 2, potassium hydroxide solution, anhydrous tetrahydrofuran and anhydrous methanol to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 20-25 hours at a temperature of 40-45° C. and a stirring rate of 400-500 r / min. After the reaction is completed, cool the reaction product to room temperature, then remove the solvent by rotary evaporation, then add it to distilled water, then vacuum filter, adjust the pH of the filtrate to 3-3.5 with hydrochloric acid solution, then vacuum filter, place the filter cake in a vacuum drying oven, and dry it at a temperature of 60-65° C. for 3-4 hours to obtain intermediate 3;

[0015] Step a4: Add intermediate 1, intermediate 3, p-toluenesulfonic acid, toluene and N,N-dimethylacetamide to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir the reaction at a temperature of 25-30°C and a stirring rate of 400-500r / min for 5-15min, then raise the temperature to reflux and continue stirring the reaction for 6-7h. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain a surface improver.

[0016] As a further solution of the present invention: the polylactic acid is PLA4032D.

[0017] As a further solution of the present invention: the antioxidant is one of antioxidant BHT, antioxidant 703 and antioxidant 245.

[0018] As a further solution of the present invention: the plasticizer is one of dimethyl phthalate, di(2-ethylhexyl) phthalate and diisononyl phthalate.

[0019] As a further solution of the present invention: the lubricant is one of butyl stearate, oleamide and ethylene bisstearamide.

[0020] As a further solution of the present invention: the light stabilizer is one of light stabilizer 944, light stabilizer 770 and light stabilizer 622.

[0021] As a further solution of the present invention: the dosage ratio of the magnesium chips, iodine particles, ethyl bromide, anhydrous tetrahydrofuran, 1-chloro-3,3,3-trifluoropropane and formaldehyde in step a1 is 3.5-4.5g: 0.1-0.2g: 1.2-1.6g: 60-65mL: 0.2mol: 6-7g; the mass fraction of the hydrochloric acid solution is 12-15%.

[0022] As a further scheme of the present invention: the usage ratio of the 2-chloroisonicotinate, 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, anhydrous potassium carbonate, tetrakis(triphenylphosphine)palladium, anhydrous ethanol and toluene in step a2 is 10 mmol: 10 mmol: 11-13 mmol: 0.5-0.7 g: 15-20 mL: 40-45 mL.

[0023] As a further scheme of the present invention: the usage ratio of the intermediate 2, potassium hydroxide solution, anhydrous tetrahydrofuran and anhydrous methanol in step a3 is 5g:20-30mL:18-24mL:18-24mL; the molar concentration of the potassium hydroxide solution is 5-5.5mol / L; the mass fraction of the hydrochloric acid solution is 20-22%.

[0024] As a further scheme of the present invention: the usage ratio of the intermediate 1, intermediate 3, p-toluenesulfonic acid, toluene and N,N-dimethylacetamide in step a4 is 30-35 mmol: 10 mmol: 0.5-1.5 g: 20-25 mL: 50-60 mL.

[0025] As a further solution of the present invention: the modified glass powder is prepared by the following steps:

[0026] Step b1: Add the silane coupling agent and the ethanol solution to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 30-50 minutes at a temperature of 25-30°C and a stirring rate of 400-500 r / min, then add the glass powder and continue stirring and reacting for 5-6 hours at a temperature of 80-85°C. After the reaction is completed, cool the reaction product to room temperature, centrifuge it, place the precipitate in a vacuum drying oven, and dry it at a temperature of 100-110°C for 1-2 hours to obtain pretreated glass powder;

[0027] Step b2: Add the pretreated glass powder and deionized water into a three-necked flask equipped with an agitator and a thermometer, stir and react for 5-10 minutes at a temperature of 25-30°C and a stirring rate of 400-500r / min, then add oleic acid and continue stirring and reacting for 8-10 hours at a temperature of 80-85°C. After the reaction, cool the reaction product to room temperature, centrifuge it, place the precipitate in a vacuum drying oven, and dry it at a temperature of 70-75°C for 2-3 hours to obtain modified glass powder.

[0028] As a further solution of the present invention: the usage ratio of the silane coupling agent, ethanol solution and glass powder in step b1 is 0.7-1.1 g: 60-70 mL: 5 g.

[0029] As a further solution of the present invention: the silane coupling agent in step b1 is silane coupling agent KH-550, the volume fraction of the ethanol solution is 80-85%, and the particle size of the glass powder is 10000 mesh.

[0030] As a further solution of the present invention: the usage ratio of the pretreated glass powder, deionized water and oleic acid in step b2 is 5g:50-55mL:2-5mL.

[0031] Beneficial effects of the present invention:

[0032] The environmentally friendly film material production process of the present invention comprises the following steps: drying polylactic acid, adding the polylactic acid together with a surface improver, modified glass powder, an antioxidant, a plasticizer, a lubricant and a light stabilizer into a mixer, stirring and mixing to obtain a mixed material; adding the mixed material into an extruder for melt extrusion, and blowing the mixed material into a film by a blow molding machine to obtain the environmentally friendly film material; the production process selects polylactic acid as the main raw material, and polylactic acid is a polymer material with good biocompatibility and complete biodegradability, does not contain toxic and harmful substances, is environmentally friendly, and can effectively improve the quality of the film after adding a surface improver. It can not only improve the hydrophobic properties of polylactic acid, but also improve certain mechanical properties. After adding modified glass powder, the mechanical properties of polylactic acid can be greatly improved, and the high brittleness and low toughness of polylactic acid can be improved. Therefore, the prepared coating material has good transparency, toughness, weather resistance, hydrolysis resistance, stain resistance and mechanical strength, etc., which meets the requirements of the packaging industry for coating materials, has broad market application prospects, and is suitable for food packaging, book covers, billboards and other application scenarios. Moreover, the production process is simple, low-cost, and suitable for large-scale industrial production.

[0033] In the process of preparing the environmentally friendly coating material, a surface improver is first prepared. First, magnesium chips and 1-chloro-3,3,3-trifluoropropane are used as raw materials to prepare a Grignard reagent, which is then reacted with paraformaldehyde and finally hydrolyzed to form an alcohol group to obtain an intermediate 1. Then, 2-chloroisonicotinic acid methyl ester and 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester are reacted. The chlorine atom on the 2-chloroisonicotinic acid methyl ester reacts with the boric acid pinacol ester group on the 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, thereby replacing the boric acid pinacol ester group with the isonicotinoic acid methyl ester structure and then introducing it into the benzene ring to obtain an intermediate 2. Then, the intermediate 2 is reacted under alkaline conditions. The reaction is carried out under the following conditions, and after acidification, the ester group is hydrolyzed to form a carboxyl group, and an intermediate 3 containing three carboxyl groups is obtained. Then, the intermediate 1 and the intermediate 3 are reacted, and the hydroxyl group on the intermediate 1 and the carboxyl group on the intermediate 3 undergo an esterification reaction, and a large number of CF bonds are introduced to obtain a surface improver; the molecular structure of the surface improver contains a benzene ring and a pyridine ring, which gives it excellent mechanical properties, and a large number of CF bonds can give it excellent hydrophobicity. Therefore, adding the surface improver to the environmentally friendly coating material can give the environmentally friendly coating material excellent mechanical properties, hydrolysis resistance and stain resistance, so that the environmentally friendly coating material can remain clean for a long time and is easy to clean;

[0034] In the process of preparing the environmentally friendly coating material, a modified glass powder is also prepared. First, the glass powder is treated with a silane coupling agent. After hydrolysis, the silane coupling agent can be grafted onto the particle surface of the glass powder to introduce amino groups to obtain pretreated glass powder. Then, the pretreated glass powder is secondary treated with oleic acid. After the carboxyl group on the oleic acid reacts with the amino group, a long alkane chain can be introduced to obtain modified glass powder. The glass powder has clear transparency and can provide good scratch resistance. After adding it to the environmentally friendly coating material, the hardness, wear resistance and scratch resistance of the environmentally friendly coating material can be improved. Moreover, the long alkane chain on the surface of the modified glass powder produces a steric hindrance effect, which prevents the glass powder from precipitating and agglomerating, and increases the distance between molecular chains, reduces the intermolecular force, and improves the mobility of the molecular chains, achieving a plasticizing effect. Therefore, the environmentally friendly coating material containing the modified glass powder has excellent mechanical properties and high toughness. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Embodiment 1:

[0037] This embodiment is a production process of an environmentally friendly coating material, comprising the following steps:

[0038] Step S1: 3.5 g of magnesium chips, 0.1 g of iodine particles, 1.2 g of bromoethane and 60 mL of anhydrous tetrahydrofuran are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and stirred for reaction for 20 min at a temperature of 30° C. and a stirring rate of 400 r / min, then 0.2 mol of 1-chloro-3,3,3-trifluoropropane is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the stirring reaction is continued for 20 min, and then 6 g of paraformaldehyde is added and the stirring reaction is continued for 5 min, and then the stirring reaction is continued for 2 h under the condition of heating to 55° C. After the reaction is completed, the reaction product is cooled to 0° C., and then added to a hydrochloric acid solution with a mass fraction of 12%, and then allowed to stand for stratification, the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;

[0039] Step S2: 10 mmol 2-chloroisonicotinate methyl ester, 10 mmol 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, 11 mmol anhydrous potassium carbonate, 0.5 g tetrakis(triphenylphosphine)palladium, 15 mL anhydrous ethanol and 40 mL toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred and reacted for 20 min at a temperature of 25° C. and a stirring rate of 400 r / min, and then the temperature is raised to reflux and the stirring reaction is continued for 20 h. After the reaction is completed, the reaction product is cooled to room temperature and then added to distilled water, and then extracted twice with dichloromethane, the extracts are combined, and then the extracts are rotary evaporated to remove the solvent to obtain intermediate 2;

[0040] Step S3: 5 g of intermediate 2, 20 mL of potassium hydroxide solution with a molar concentration of 5 mol / L, 18 mL of anhydrous tetrahydrofuran and 18 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 40°C and a stirring rate of 400 r / min for 20 h. After the reaction, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then added to distilled water, and then vacuum filtered. The filtrate was adjusted to pH 3 with hydrochloric acid solution, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at a temperature of 60°C for 3 h to obtain intermediate 3;

[0041] Step S4: 30 mmol of intermediate 1, 10 mmol of intermediate 3, 0.5 g of p-toluenesulfonic acid, 20 mL of toluene and 50 mL of N, N-dimethylacetamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stirred for reaction at a temperature of 25 ° C. and a stirring rate of 400 r / min for 5 min, then the temperature was raised to reflux and the stirring reaction was continued for 6 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a surface improver;

[0042] Step S5: adding 0.7 g of silane coupling agent KH-550 and 60 mL of 80% ethanol solution by volume to a three-necked flask equipped with a stirrer and a thermometer, stirring and reacting for 30 min at a temperature of 25° C. and a stirring rate of 400 r / min, then adding glass powder with a particle size of 10000 mesh and heating to 80° C. and continuing to stir and react for 5 h. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 100° C. for 1 h to obtain a pretreated glass powder;

[0043] Step S6: 5 g of pretreated glass powder and 50 mL of deionized water were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 5 min, and then 2 mL of oleic acid was added and the temperature was raised to 80° C. and the stirring reaction was continued for 8 h. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at a temperature of 70° C. for 2 h to obtain a modified glass powder;

[0044] Step S7: weigh 70 parts of polylactic acid, 2 parts of surface improver, 6.5 parts of modified glass powder, 0.8 parts of antioxidant, 0.5 parts of plasticizer, 0.3 parts of lubricant and 0.2 parts of light stabilizer according to weight parts, and set aside; the polylactic acid is PLA4032D; the antioxidant is antioxidant BHT; the plasticizer is dimethyl phthalate; the lubricant is butyl stearate;

[0045] Step S8: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 60° C. for 2 h, then adding it into a mixer together with a surface improver, modified glass powder, an antioxidant, a plasticizer, a lubricant, and a light stabilizer, stirring and mixing them at a temperature of 45° C. and a stirring rate of 400 r / min for 40 min to obtain a mixed material;

[0046] Step S9: adding the mixed material into an extruder for melt extrusion, and blowing it into a film through a blow molding machine to obtain an environmentally friendly film material.

[0047] Embodiment 2:

[0048] This embodiment is a production process of an environmentally friendly coating material, comprising the following steps:

[0049] Step S1: 4.0 g of magnesium chips, 0.15 g of iodine particles, 1.4 g of bromoethane and 62 mL of anhydrous tetrahydrofuran are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and stirred for reaction for 25 min at a temperature of 32 ° C and a stirring rate of 450 r / min, then 0.2 mol 1-chloro-3,3,3-trifluoropropane is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the stirring reaction is continued for 25 min, and then 6.5 g of paraformaldehyde is added and the stirring reaction is continued for 8 min, and then the temperature is raised to 58 ° C and the stirring reaction is continued for 2.5 h. After the reaction is completed, the reaction product is cooled to 3 ° C, and then added to a hydrochloric acid solution with a mass fraction of 14%, and then allowed to stand for stratification, the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;

[0050] Step S2: 10 mmol 2-chloroisonicotinate methyl ester, 10 mmol 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, 12 mmol anhydrous potassium carbonate, 0.6 g tetrakis(triphenylphosphine)palladium, 18 mL anhydrous ethanol and 42 mL toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 28° C. and a stirring rate of 450 r / min for 25 min, and then the temperature is raised to reflux and the stirring reaction is continued for 22 h. After the reaction is completed, the reaction product is cooled to room temperature and then added to distilled water, and then extracted twice with dichloromethane, the extracts are combined, and then the extracts are rotary evaporated to remove the solvent to obtain intermediate 2;

[0051] Step S3: 5 g of intermediate 2, 25 mL of potassium hydroxide solution with a molar concentration of 5.2 mol / L, 21 mL of anhydrous tetrahydrofuran and 21 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 42° C. and a stirring rate of 450 r / min for 22 h. After the reaction, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then added to distilled water, and then vacuum filtered. The filtrate was adjusted to pH 3.2 with hydrochloric acid solution, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at a temperature of 62° C. for 3.5 h to obtain intermediate 3;

[0052] Step S4: 32 mmol of intermediate 1, 10 mmol of intermediate 3, 1.0 g of p-toluenesulfonic acid, 22 mL of toluene and 55 mL of N,N-dimethylacetamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was stirred for reaction at 28 ° C. and a stirring rate of 450 r / min for 10 min, and then the mixture was heated to reflux and continued to stir for 6.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a surface improver;

[0053] Step S5: adding 0.9 g of silane coupling agent KH-550 and 65 mL of ethanol solution with a volume fraction of 82% to a three-necked flask equipped with a stirrer and a thermometer, stirring and reacting for 40 min at a temperature of 28° C. and a stirring rate of 450 r / min, then adding glass powder with a particle size of 10000 mesh and heating to 82° C. and continuing to stir and react for 5.5 h. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 105° C. for 1.5 h to obtain a pretreated glass powder;

[0054] Step S6: 5 g of pretreated glass powder and 52 mL of deionized water were added to a three-necked flask equipped with a stirrer and a thermometer, and the mixture was stirred at 28° C. and 450 r / min for 7 min. Then, 3.5 mL of oleic acid was added and the mixture was heated to 82° C. and stirred for 9 h. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 72° C. for 2.5 h to obtain a modified glass powder.

[0055] Step S7: weigh 75 parts of polylactic acid, 7 parts of surface improver, 10 parts of modified glass powder, 1.2 parts of antioxidant, 0.9 parts of plasticizer, 0.6 parts of lubricant and 0.4 parts of light stabilizer according to weight parts, and set aside; the polylactic acid is PLA4032D; the antioxidant is antioxidant 703; the plasticizer is di(2-ethylhexyl) phthalate; the lubricant is oleamide;

[0056] Step S8: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 62° C. for 2.5 hours, then adding it into a mixer together with a surface improver, modified glass powder, an antioxidant, a plasticizer, a lubricant, and a light stabilizer, stirring and mixing it at a temperature of 50° C. and a stirring rate of 450 r / min for 50 minutes to obtain a mixed material;

[0057] Step S9: adding the mixed material into an extruder for melt extrusion, and blowing it into a film through a blow molding machine to obtain an environmentally friendly film material.

[0058] Embodiment 3:

[0059] This embodiment is a production process of an environmentally friendly coating material, comprising the following steps:

[0060] Step S1: 4.5 g of magnesium chips, 0.2 g of iodine particles, 1.6 g of bromoethane and 65 mL of anhydrous tetrahydrofuran are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and stirred for 30 min at a temperature of 35 ° C and a stirring rate of 500 r / min, then 0.2 mol 1-chloro-3,3,3-trifluoropropane is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 30 min, and then 7 g of paraformaldehyde is added and the stirring reaction is continued for 10 min, and then the temperature is raised to 60 ° C and the stirring reaction is continued for 3 h. After the reaction is completed, the reaction product is cooled to 5 ° C, and then added to a hydrochloric acid solution with a mass fraction of 15%, and then allowed to stand for stratification, the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;

[0061] Step S2: 10 mmol 2-chloroisonicotinate methyl ester, 10 mmol 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, 13 mmol anhydrous potassium carbonate, 0.7 g tetrakis(triphenylphosphine)palladium, 20 mL anhydrous ethanol and 45 mL toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 500 r / min for 30 min, and then the temperature is raised to reflux and the stirring reaction is continued for 25 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to distilled water, and then extracted with dichloromethane for 3 times, the extracts are combined, and then the extracts are rotary evaporated to remove the solvent to obtain intermediate 2;

[0062] Step S3: 5 g of intermediate 2, 30 mL of potassium hydroxide solution with a molar concentration of 5.5 mol / L, 24 mL of anhydrous tetrahydrofuran and 24 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 45° C. and a stirring rate of 500 r / min for 25 h. After the reaction, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then added to distilled water, and then vacuum filtered. The filtrate was adjusted to pH 3.5 with hydrochloric acid solution, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at a temperature of 65° C. for 4 h to obtain intermediate 3;

[0063] Step S4: 35 mmol of intermediate 1, 10 mmol of intermediate 3, 1.5 g of p-toluenesulfonic acid, 25 mL of toluene and 60 mL of N,N-dimethylacetamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stirred for reaction at a temperature of 30°C and a stirring rate of 500 r / min for 15 min, then the temperature was raised to reflux and the stirring reaction was continued for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a surface improver;

[0064] Step S5: 1.1 g of silane coupling agent KH-550 and 70 mL of ethanol solution with a volume fraction of 85% are added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 30° C. and a stirring rate of 500 r / min for 50 min, then glass powder with a particle size of 10000 mesh is added and the temperature is raised to 85° C. and the stirring reaction is continued for 6 h. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 110° C. for 2 h to obtain a pretreated glass powder;

[0065] Step S6: 5 g of pretreated glass powder and 55 mL of deionized water were added to a three-necked flask equipped with a stirrer and a thermometer, and the mixture was stirred at 30° C. and 500 r / min for 10 min. Then, 5 mL of oleic acid was added and the mixture was heated to 85° C. and stirred for 10 h. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 75° C. for 3 h to obtain a modified glass powder.

[0066] Step S7: 80 parts of polylactic acid, 12 parts of surface improver, 13.5 parts of modified glass powder, 1.6 parts of antioxidant, 1.3 parts of plasticizer, 0.9 parts of lubricant and 0.6 parts of light stabilizer are weighed according to weight parts for use; the polylactic acid is PLA4032D; the antioxidant is antioxidant 245; the plasticizer is diisononyl phthalate; the lubricant is ethylene bisstearamide;

[0067] Step S8: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 65° C. for 3 hours, then adding it into a mixer together with a surface improver, modified glass powder, an antioxidant, a plasticizer, a lubricant, and a light stabilizer, stirring and mixing them at a temperature of 55° C. and a stirring rate of 500 r / min for 60 minutes to obtain a mixed material;

[0068] Step S9: adding the mixed material into an extruder for melt extrusion, and blowing it into a film through a blow molding machine to obtain an environmentally friendly film material.

[0069] Comparative Example 1:

[0070] This comparative example is a production process of an environmentally friendly coating material, comprising the following steps:

[0071] Step S1: 80 parts of polylactic acid, 1.6 parts of antioxidant, 1.3 parts of plasticizer, 0.9 parts of lubricant and 0.6 parts of light stabilizer are weighed according to weight parts for use; the polylactic acid is PLA4032D; the antioxidant is antioxidant 245; the plasticizer is diisononyl phthalate; the lubricant is ethylene bisstearamide;

[0072] Step S2: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 65° C. for 3 hours, then adding it into a mixer together with an antioxidant, a plasticizer, a lubricant, and a light stabilizer, stirring and mixing them at a temperature of 55° C. and a stirring rate of 500 r / min for 60 minutes to obtain a mixed material;

[0073] Step S3: adding the mixed material into an extruder for melt extrusion, and blowing it into a film through a blow molding machine to obtain an environmentally friendly film material.

[0074] Comparative Example 2:

[0075] This comparative example is a production process of an environmentally friendly coating material, comprising the following steps:

[0076] Step S1: 4.5 g of magnesium chips, 0.2 g of iodine particles, 1.6 g of bromoethane and 65 mL of anhydrous tetrahydrofuran are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 30 min at a temperature of 35° C. and a stirring rate of 500 r / min, and then 0.2 mol of 1-chloro-3,3,3-trifluoropropane is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the addition is completed, the stirring reaction is continued for 30 min, and then 7 g of paraformaldehyde is added and the stirring reaction is continued for 10 min, and then the temperature is raised to 60° C. and the stirring reaction is continued for 3 h. After the reaction is completed, the reaction product is cooled to 5° C. and then added to a hydrochloric acid solution with a mass fraction of 15%, and then allowed to stand for stratification, and the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;

[0077] Step S2: 10 mmol 2-chloroisonicotinate methyl ester, 10 mmol 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, 13 mmol anhydrous potassium carbonate, 0.7 g tetrakis(triphenylphosphine)palladium, 20 mL anhydrous ethanol and 45 mL toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 500 r / min for 30 min, and then the temperature is raised to reflux and the stirring reaction is continued for 25 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to distilled water, and then extracted with dichloromethane for 3 times, the extracts are combined, and then the extracts are rotary evaporated to remove the solvent to obtain intermediate 2;

[0078] Step S3: 5 g of intermediate 2, 30 mL of potassium hydroxide solution with a molar concentration of 5.5 mol / L, 24 mL of anhydrous tetrahydrofuran and 24 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 45° C. and a stirring rate of 500 r / min for 25 h. After the reaction, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then added to distilled water, and then vacuum filtered. The filtrate was adjusted to pH 3.5 with hydrochloric acid solution, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at a temperature of 65° C. for 4 h to obtain intermediate 3;

[0079] Step S4: 35 mmol of intermediate 1, 10 mmol of intermediate 3, 1.5 g of p-toluenesulfonic acid, 25 mL of toluene and 60 mL of N,N-dimethylacetamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stirred for reaction at a temperature of 30°C and a stirring rate of 500 r / min for 15 min, then the temperature was raised to reflux and the stirring reaction was continued for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a surface improver;

[0080] Step S5: 80 parts of polylactic acid, 12 parts of surface improver, 1.6 parts of antioxidant, 1.3 parts of plasticizer, 0.9 parts of lubricant and 0.6 parts of light stabilizer are weighed according to weight parts for use; the polylactic acid is PLA4032D; the antioxidant is antioxidant 245; the plasticizer is diisononyl phthalate; the lubricant is ethylene bisstearamide;

[0081] Step S6: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 65° C. for 3 hours, then adding it into a mixer together with a surface improver, an antioxidant, a plasticizer, a lubricant, and a light stabilizer, stirring and mixing them at a temperature of 55° C. and a stirring rate of 500 r / min for 60 minutes to obtain a mixed material;

[0082] Step S7: adding the mixed material into an extruder for melt extrusion, and blowing it into a film through a blow molding machine to obtain an environmentally friendly film material.

[0083] Comparative Example 3:

[0084] This comparative example is a production process of an environmentally friendly coating material, comprising the following steps:

[0085] Step S1: 1.1 g of silane coupling agent KH-550 and 70 mL of ethanol solution with a volume fraction of 85% are added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction for 50 min at a temperature of 30° C. and a stirring rate of 500 r / min, then glass powder with a particle size of 10000 mesh is added and the temperature is raised to 85° C. and the stirring reaction is continued for 6 h. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 110° C. for 2 h to obtain a pretreated glass powder;

[0086] Step S2: 5 g of pretreated glass powder and 55 mL of deionized water were added to a three-necked flask equipped with a stirrer and a thermometer, and the mixture was stirred at 30° C. and 500 r / min for 10 min. Then, 5 mL of oleic acid was added and the mixture was heated to 85° C. and stirred for 10 h. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 75° C. for 3 h to obtain a modified glass powder.

[0087] Step S3: 80 parts of polylactic acid, 13.5 parts of modified glass powder, 1.6 parts of antioxidant, 1.3 parts of plasticizer, 0.9 parts of lubricant and 0.6 parts of light stabilizer are weighed according to weight parts for use; the polylactic acid is PLA4032D; the antioxidant is antioxidant 245; the plasticizer is diisononyl phthalate; the lubricant is ethylene bisstearamide;

[0088] Step S4: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 65° C. for 3 hours, then adding it into a mixer together with the modified glass powder, antioxidant, plasticizer, lubricant, and light stabilizer, stirring and mixing them at a temperature of 55° C. and a stirring rate of 500 r / min for 60 minutes to obtain a mixed material;

[0089] Step S5: adding the mixed material into an extruder for melt extrusion, and blowing it into a film through a blow molding machine to obtain an environmentally friendly film material.

[0090] The environmentally friendly coating materials of Examples 1-3 and Comparative Examples 1-3 were tested for performance, and the test results are shown in the following table:

[0091] sample Tensile strength, MPa Elongation at break, % Water drop contact angle, % Example 1 43.8 376 131 Example 2 45.3 391 136 Example 3 47.1 413 142 Comparative Example 1 28.4 239 96 Comparative Example 2 37.7 318 137 Comparative Example 3 39.0 325 118

[0092] Referring to the data in the above table, based on the comparison between Examples 1-3 and Comparative Examples 1-3, it can be seen that adding surface improvers and modified glass powder can effectively enhance the mechanical properties and hydrophobic properties of the environmentally friendly coating material, thereby preparing an environmentally friendly coating material with high strength, good toughness and excellent stain resistance.

[0093] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0094] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A production process for environmentally friendly coating materials, characterized in that: The following steps are involved: Step 1: Weigh 70-80 parts of polylactic acid, 2-12 parts of surface improver, 6.5-13.5 parts of modified glass powder, 0.8-1.6 parts of antioxidant, 0.5-1.3 parts of plasticizer, 0.3-0.9 parts of lubricant and 0.2-0.6 parts of light stabilizer according to weight parts, and set aside; Step 2: placing the polylactic acid in a vacuum drying oven, drying it at a temperature of 60-65° C. for 2-3 hours, then adding it into a mixer together with a surface improver, modified glass powder, antioxidant, plasticizer, lubricant, and light stabilizer, stirring and mixing it at a temperature of 45-55° C. and a stirring rate of 400-500 r / min for 40-60 minutes to obtain a mixed material; Step 3: adding the mixed material into an extruder for melt extrusion, and blowing it into a film through a blow molding machine to obtain an environmentally friendly film material; Wherein, the surface improver is prepared by the following steps: Step a1: Stir and react magnesium chips, iodine particles, ethyl bromide and anhydrous tetrahydrofuran, then add 1-chloro-3,3,3-trifluoropropane dropwise while stirring, continue to stir and react after the addition is complete, then add paraformaldehyde and continue to stir and react, after the reaction is completed, cool the reaction product, then add it to a hydrochloric acid solution, then stand and separate, dry the organic phase, then vacuum filter, and rotary evaporate the filtrate to obtain an intermediate 1; Step a2: stirring methyl 2-chloroisonicotinate, 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, anhydrous potassium carbonate, tetrakis(triphenylphosphine)palladium, anhydrous ethanol and toluene for reaction, cooling the reaction product after the reaction, then adding it to distilled water, then extracting it, and then rotary evaporating the extract to obtain intermediate 2; Step a3: stirring the intermediate 2, potassium hydroxide solution, anhydrous tetrahydrofuran and anhydrous methanol for reaction, cooling the reaction product after the reaction, then rotary evaporating, then adding it to distilled water, then vacuum filtering, adjusting the pH of the filtrate with hydrochloric acid solution, then vacuum filtering, and drying the filter cake to obtain the intermediate 3; Step a4: stirring the intermediate 1, the intermediate 3, p-toluenesulfonic acid, toluene and N,N-dimethylacetamide for reaction, cooling the reaction product after the reaction is completed, and then rotary evaporating to obtain a surface improver.

2. The production process of an environmentally friendly coating material according to claim 1, characterized in that: The polylactic acid is PLA4032D; The antioxidant is one of antioxidant BHT, antioxidant 703 and antioxidant 245; The plasticizer is one of dimethyl phthalate, di(2-ethylhexyl) phthalate and diisononyl phthalate; The lubricant is one of butyl stearate, oleamide and ethylene bis stearamide; The light stabilizer is one of the light stabilizer 944 , the light stabilizer 770 and the light stabilizer 622 .

3. The production process of an environmentally friendly coating material according to claim 1, characterized in that: The magnesium chips, iodine particles, ethyl bromide, anhydrous tetrahydrofuran, 1-chloro-3,3,3-trifluoropropane and formaldehyde in step a1 are used in a ratio of 3.5-4.5 g: 0.1-0.2 g: 1.2-1.6 g: 60-65 mL: 0.2 mol: 6-7 g; the mass fraction of the hydrochloric acid solution is 12-15%.

4. The production process of an environmentally friendly coating material according to claim 1, characterized in that: The amount ratio of the 2-chloroisonicotinate, 3,5-bis(methoxycarbonyl)phenylboronic acid pinacol ester, anhydrous potassium carbonate, tetrakis(triphenylphosphine)palladium, anhydrous ethanol and toluene in step a2 is 10mmol:10mmol:11-13mmol:0.5-0.7g:15-20mL:40-45mL.

5. The production process of an environmentally friendly coating material according to claim 1, characterized in that: The usage ratio of the intermediate 2, potassium hydroxide solution, anhydrous tetrahydrofuran and anhydrous methanol in step a3 is 5g:20-30mL:18-24mL:18-24mL; the molar concentration of the potassium hydroxide solution is 5-5.5mol / L; and the mass fraction of the hydrochloric acid solution is 20-22%.

6. The process for producing an environmentally friendly coating material according to claim 1, characterized in that: The usage ratio of the intermediate 1, intermediate 3, p-toluenesulfonic acid, toluene and N,N-dimethylacetamide in step a4 is 30-35 mmol: 10 mmol: 0.5-1.5 g: 20-25 mL: 50-60 mL.

7. The process for producing an environmentally friendly coating material according to claim 1, characterized in that: The modified glass powder is prepared by the following steps: Step b1: stirring the silane coupling agent and the ethanol solution for reaction, then adding the glass powder and continuing the stirring reaction, cooling the reaction product after the reaction is completed, then centrifuging, and drying the precipitate to obtain the pretreated glass powder; Step b2: Stir the pretreated glass powder and deionized water for reaction, then add oleic acid and continue stirring the reaction. After the reaction is completed, cool the reaction product, then centrifuge it, and dry the precipitate to obtain modified glass powder.

8. The process for producing an environmentally friendly coating material according to claim 7, characterized in that: The usage ratio of the silane coupling agent, ethanol solution and glass powder in step b1 is 0.7-1.1 g: 60-70 mL: 5 g.

9. The process for producing an environmentally friendly coating material according to claim 7, characterized in that: The silane coupling agent in step b1 is silane coupling agent KH-550, the volume fraction of the ethanol solution is 80-85%, and the particle size of the glass powder is 10000 mesh.

10. The process for producing an environmentally friendly coating material according to claim 7, characterized in that: The dosage ratio of the pretreated glass powder, deionized water and oleic acid in step b2 is 5g:50-55mL:2-5mL.

Citation Information

Patent Citations

  • Polylactic acid modified material with high flexibility and heat resistance and preparation method of polylactic acid modified material

    CN106700450A

  • Degradable plastic film and preparation method thereof

    CN113999506A