A quantitative identification method and system for local corrosion defects of equipment
By combining ultrasonic waveguide and instantaneous electromagnetic scanning, using linear regression and least squares model, the problem of difficulty in identifying local corrosion by fixed-point monitoring of a single physical signal is solved, and accurate quantitative identification and positioning of local corrosion defects of pipelines is achieved, and detection is improved Accuracy meets the security risk monitoring needs.
Patent Information
- Application Number
- CN202410524470.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-04-29
AI Technical Summary
In the prior art, the fixed-point monitoring method of a single physical signal is difficult to meet the accuracy requirements of local corrosion defect detection of equipment, especially when local corrosion locations are highly random and concealed, it is difficult to effectively identify and locate corrosion abnormalities.
Using a combination of ultrasonic waveguide and instantaneous electromagnetic scanning, the corrosion thinning rate and predict the waveguide amplitude are calculated through linear regression model, local corrosion anomalies are judged, and the equivalent diameter and depth of corrosion defects are calculated by fitting the least squares method to achieve Quantitative identification and positioning of local corrosion defects in pipelines.
It improves the accuracy of corrosion defect detection, meets the safety risk monitoring needs of local corrosion defects in coated pipelines, and ensures the safe operation of equipment and reduces economic losses.
Smart Images

Figure CN118311149B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of corrosion anomaly detection, and in particular to a quantitative identification method and system for local corrosion defects of equipment. Background Art
[0002] In the process industry, corrosion anomalies in medium-risk units often directly threaten their safe operation, among which local corrosion poses a more serious safety threat. Local corrosion has the characteristics of large randomness and strong concealment of corrosion locations, which often leads to corrosion leakage incidents that are difficult to prevent. In the absence of corresponding monitoring methods, high-frequency leakage incidents are likely to cause fires and explosions or huge economic losses, posing a threat to safe production.
[0003] For the purpose of safety management, in the process of monitoring data sampling, in order to reduce the additional risks such as high temperature burns and corrosion under the insulation layer caused by the damage of the coating, it is necessary to ensure the integrity of the pipeline coating. At present, the identification of local corrosion anomalies is mainly based on fixed-point monitoring, including ultrasonic thickness measurement and field fingerprinting that rely on a single physical signal.
[0004] Since the defect location of local corrosion has a certain randomness, in order to accurately identify the abnormal local corrosion situation of a certain pipe section, it is necessary to have regional monitoring capabilities to cope with the randomness of the local corrosion location.
[0005] With respect to the above technical solution, the fixed-point monitoring method of a single physical signal in the prior art is not easy to use for regional monitoring and is difficult to meet the accuracy requirements for local corrosion defect detection of equipment. Summary of the invention
[0006] In order to improve the accuracy of corrosion defect detection, the present invention provides a method and system for quantitatively identifying local corrosion defects of equipment.
[0007] In a first aspect, the present invention provides a method for quantitatively identifying local corrosion defects of equipment, which adopts the following technical solution:
[0008] A quantitative identification method for local corrosion defects of equipment includes the following steps:
[0009] Acquisition of data I: Ultrasonic guided wave monitoring of the pipe section for N sampling cycles, the monitoring cycle is , get the amplitude of the waveguide signal of the nth sampling period ;
[0010] Calculate corrosion rate: Calculate the historical corrosion thinning rate of the monitored pipe section , The calculation model is:
[0011] ;
[0012] Calculate the regression intercept: Calculate the linear regression intercept b of the waveguide signal amplitude in the first N sampling periods GW , b GW The calculation model is:
[0013] ;
[0014] Obtain prediction error: Calculate the prediction error of the guided wave amplitude based on the historical guided wave signal amplitude data of the monitored pipeline , The calculation model is:
[0015] ;
[0016] Guided wave amplitude prediction: Calculate the predicted guided wave amplitude of the monitored pipe section in the N+1th sampling period based on historical data , The calculation model is:
[0017] ;
[0018] Determine corrosion anomaly: obtain the amplitude of the guided wave signal in the N+1th sampling period , if satisfied , it is judged that the pipe section has local corrosion abnormality and recorded as a corrosion defective pipe section. Otherwise, it is judged that no local corrosion abnormality has occurred;
[0019] Data acquisition II: Perform instantaneous electromagnetic scanning of the corrosion defective pipe section for N sampling cycles, with a monitoring period of , obtain the instantaneous electromagnetic signal amplitude of the nth sampling period , phase angle ;
[0020] Calculate defect diameter: Calculate the equivalent diameter of localized corrosion defects , The calculation model is:
[0021] ;
[0022] Among them, η is the instantaneous electromagnetic linear fitting coefficient, ε is the instantaneous electromagnetic linear fitting constant, λ is the waveguide linear fitting coefficient, κ is the waveguide linear fitting constant, η and ε are obtained by fitting the historical instantaneous electromagnetic signal amplitude through the least squares linear regression algorithm, λ and κ are obtained by fitting the historical waveguide signal amplitude through the least squares linear regression algorithm, is the instantaneous electromagnetic signal amplitude of the Nth sampling period, is the amplitude of the waveguide signal in the Nth sampling period.
[0023] By adopting the above technical solution, for a certain section of the coated pipeline, the local corrosion of the section is monitored online periodically using ultrasonic guided waves without destroying the integrity of the coating layer. The historical corrosion thinning rate of the monitored section within the first N sampling periods is calculated based on the linear regression time factor expression. ,according to Calculate the prediction error of guided wave amplitude and the predicted guided wave amplitude of the N+1th sampling period , and then determine whether local corrosion abnormalities occur in the pipe section, and realize the identification and location of local corrosion defects; perform instantaneous electromagnetic scanning on the corrosion defect pipe section. After the scanning is completed, the equivalent diameter of the local corrosion defect is calculated based on η, ε, λ, and κ obtained by fitting the least squares linear regression algorithm, using the mathematical relationship that the ultrasonic guided wave echo amplitude is proportional to the cross-sectional area of the local corrosion defect, and the low-frequency electromagnetic signal amplitude is proportional to the volume of the local corrosion defect. ,Such setting improves the accuracy of corrosion defect detection and meets the ,needs of safety risk monitoring of local corrosion defects of ,coated pipelines in practical applications.
[0024] Optionally, in the step of calculating the defect diameter, The calculation model is updated as follows:
[0025] ;
[0026] in, is the diameter correction factor, The calculation model is:
[0027] ;
[0028] in, is the inner diameter of the monitored pipe section, is the electromagnetic footprint diameter of the instantaneous electromagnetic sensor of the monitored pipe section, is the length of a single sensor in the waveguide array group of the monitored pipe section.
[0029] By adopting the above technical solution, the equivalent diameter of the local corrosion defect is calculated , and according to , , Calculate the diameter correction factor ,use right Corrections are made to reduce the impact of differences in sensor length and diameter on detection accuracy, improve the accuracy of defect diameter calculation, and thus improve the accuracy of corrosion defect detection.
[0030] Optionally, a judgment step is further provided between the step of obtaining data II and the step of calculating the defect diameter;
[0031] Judgment: If the nth sampling period satisfies and , then judge is the effective instantaneous electromagnetic signal amplitude of the nth sampling period, otherwise, repeatedly execute the step of acquiring data II until the effective instantaneous electromagnetic signal amplitude is obtained.
[0032] By adopting the above technical solution, the corrosion defective pipe section is subjected to instantaneous electromagnetic scanning to obtain the instantaneous electromagnetic signal amplitude. and phase angle , if satisfied and , then judge is the effective electromagnetic signal amplitude, otherwise the scan is repeated until the effective value is obtained; since the local corrosion defect is a concave geometric shape, the corresponding initial phase angle of the electromagnetic signal is 90°±30°, while that of the weld is 270°±30°. Considering the possible non-ideal measurement state of the pipeline, the interval is enlarged to 45°. Because the weld is the interference source in the actual measurement, the interference of the weld can be eliminated. Further narrowing the range limit has no obvious beneficial effect.
[0033] Optionally, a defect depth calculation step is further provided after the defect diameter calculation step;
[0034] Calculate defect depth: Calculate the equivalent depth of localized corrosion defects , The calculation model is:
[0035] .
[0036] By adopting the above technical solution, the equivalent depth of the local corrosion defect is calculated according to the fitting coefficient and the fitting constant. , which is conducive to further determining the corrosion state of the local corrosion defects in the pipe section, thereby improving the accuracy of corrosion defect detection and meeting the needs of safety risk monitoring of local corrosion defects in coated pipelines in practical applications.
[0037] Optionally, in the defect depth calculation step, The calculation model is updated as follows:
[0038] ;
[0039] in is the depth correction factor, The calculation model is:
[0040] ;
[0041] Where t is the designed wall thickness of the monitored pipe section, is the inner diameter of the monitored pipe section, is the electromagnetic footprint diameter of the instantaneous electromagnetic sensor of the monitored pipe section, is the length of a single sensor in the waveguide array group of the monitored pipe section.
[0042] By adopting the above technical solution, according to Different values calculate different depth correction factors ,use right Correction is made based on the statistics of actual measurement data, due to the diameter of local corrosion defects When the cross section of the local corrosion defect is ≤10mm, it can be approximated as a circle, and the equivalent depth can be calculated according to the circular cross section. On the contrary, the cross section of a local corrosion defect is closer to an oblong or rectangular cross section, so it is advisable to use a rectangular cross section to calculate the equivalent depth. , thereby improving the accuracy of defect depth calculation.
[0043] In a second aspect, the present invention provides a quantitative identification system for local corrosion defects of equipment, which adopts the following technical solution:
[0044] A quantitative identification system for local corrosion defects of equipment, including the following modules:
[0045] Acquisition module I: The output end is connected to the input end of the calculation module I, and is used to perform ultrasonic guided wave monitoring on the pipe section for N sampling cycles. The monitoring cycle is , get the amplitude of the waveguide signal of the nth sampling period ;
[0046] Calculation module I: The input end is connected to the output end of acquisition module I, and the output end is connected to the input end of calculation module II, which is used to calculate the historical corrosion thinning rate of the monitored pipe section according to the linear regression time factor expression ;
[0047] Calculation module II: The input end is connected to the output end of calculation module I, and the output end is connected to the input end of calculation module III, which is used to calculate the linear regression intercept b of the amplitude of the waveguide signal in the first N sampling periods. GW ;
[0048] Calculation module III: The input end is connected to the output end of calculation module II, and the output end is connected to the input end of prediction module, which is used to calculate the guided wave amplitude prediction error according to the historical guided wave signal amplitude data of the monitored pipeline. ;
[0049] Prediction module: The input end is connected to the output end of the calculation module III, and the output end is connected to the input end of the judgment module I, which is used to calculate the predicted guided wave amplitude of the monitored pipe section in the N+1th sampling period predicted based on historical data ;
[0050] Judgment module I: The input end is connected to the output end of the prediction module, and the output end is connected to the input end of the acquisition module II, which is used to obtain the amplitude of the waveguide signal in the N+1th sampling period , if satisfied , it is judged that the pipe section has local corrosion abnormality and recorded as a corrosion defective pipe section. Otherwise, it is judged that no local corrosion abnormality has occurred;
[0051] Acquisition module II: The input end is connected to the output end of the judgment module I, and the output end is connected to the input end of the calculation module IV, which is used to perform instantaneous electromagnetic scanning of the corrosion defective pipe section for N sampling cycles. The monitoring cycle is , obtain the instantaneous electromagnetic signal amplitude of the nth sampling period , phase angle ;
[0052] Calculation module IV: The input end is connected to the output end of the acquisition module II, and is used to calculate the equivalent diameter of the local corrosion defect according to the instantaneous electromagnetic signal amplitude of the Nth sampling period, the waveguide signal amplitude, and the fitting coefficient and fitting constant obtained by fitting the historical data through the least squares linear regression algorithm. .
[0053] By adopting the above technical solution, for a certain pipe section of the coated pipeline, the local corrosion of the pipe section is monitored online periodically by using ultrasonic guided waves without destroying the integrity of the coating layer. The acquisition module I obtains the amplitude of the guided wave signal. , the calculation module I calculates the historical corrosion thinning rate of the monitored pipe section in the first N sampling periods according to the linear regression time factor expression , calculation module II calculates the linear regression intercept b GW , calculation module III according to Calculate the prediction error of guided wave amplitude , the prediction module calculates the predicted guided wave amplitude of the N+1th sampling period The judgment module I judges whether local corrosion abnormality occurs in the pipe section, and realizes the identification and location of local corrosion defects; the corrosion defect pipe section is subjected to instantaneous electromagnetic scanning, and the acquisition module II acquires the instantaneous electromagnetic signal amplitude and phase angle After the scanning is completed, the calculation module IV uses the mathematical relationship that the amplitude of the ultrasonic guided wave echo is proportional to the cross-sectional area of the local corrosion defect, and the amplitude of the low-frequency electromagnetic signal is proportional to the volume of the local corrosion defect, and calculates the equivalent diameter of the local corrosion defect according to η, ε, λ, and κ obtained by fitting the least squares linear regression algorithm. ,Such setting improves the accuracy of corrosion defect detection and meets the ,needs of safety risk monitoring of local corrosion defects of ,coated pipelines in practical applications.
[0054] Optionally, in calculation module IV, the diameter correction coefficient is also calculated based on the inner diameter of the monitored pipe section, the electromagnetic footprint diameter of the instantaneous electromagnetic sensor, and the length of a single sensor in the waveguide array group. , and according to right Make corrections.
[0055] By adopting the above technical solution, the equivalent diameter of the local corrosion defect is calculated , and use right Corrections are made to reduce the impact of differences in sensor length and diameter on detection accuracy, improve the accuracy of defect diameter calculation, and thus improve the accuracy of corrosion defect detection.
[0056] Optionally, it also includes a judgment module II: the input end is connected to the output end of the acquisition module II, and the output end is connected to the input end of the calculation module IV, which is used to determine if the nth sampling period meets the requirements. and , then judge is the effective instantaneous electromagnetic signal amplitude of the nth sampling period, otherwise, the acquisition module II is repeatedly executed until the effective instantaneous electromagnetic signal amplitude is obtained.
[0057] By adopting the above technical solution, the corrosion defective pipe section is subjected to instantaneous electromagnetic scanning to obtain the instantaneous electromagnetic signal amplitude. and phase angle , if satisfied and , then the judgment module II judges is the effective electromagnetic signal amplitude, otherwise the scan is repeated until a valid value is obtained; considering the possible non-ideal measurement state of the pipeline, the interval is enlarged to 45°. Because the weld is the interference source in actual measurement, the interference of the weld can be eliminated. Further narrowing the range limit will have no obvious beneficial effect.
[0058] Optionally, it also includes a calculation module V: the input end is connected to the output end of the calculation module IV, and is used to calculate the equivalent depth of the local corrosion defect according to the instantaneous electromagnetic signal amplitude of the Nth sampling period, the waveguide signal amplitude, and the fitting coefficient and fitting constant obtained by fitting the historical data through the least squares linear regression algorithm. .
[0059] By adopting the above technical solution, the calculation module V calculates the equivalent depth of the local corrosion defect according to the fitting coefficient and the fitting constant. , which is conducive to further determining the corrosion state of the local corrosion defects in the pipe section, thereby improving the accuracy of corrosion defect detection and meeting the needs of safety risk monitoring of local corrosion defects in coated pipelines in practical applications.
[0060] Optionally, in the calculation module V, the depth correction coefficient is also calculated based on the designed wall thickness, inner diameter, electromagnetic footprint diameter of the transient electromagnetic sensor, and the length of a single sensor in the waveguide array group of the monitored pipe section. , and according to right Make corrections.
[0061] By adopting the above technical solution, according to Different values calculate different depth correction factors ,use right Correction is made based on the statistics of actual measurement data, due to the diameter of local corrosion defects When the cross section of the local corrosion defect is ≤10mm, it can be approximated as a circle, and the equivalent depth can be calculated according to the circular cross section. On the contrary, the cross section of a local corrosion defect is closer to an oblong or rectangular cross section, so it is advisable to use a rectangular cross section to calculate the equivalent depth. , thereby improving the accuracy of defect depth calculation.
[0062] In summary, the present invention includes at least one of the following beneficial technical effects:
[0063] 1.Use ultrasonic guided waves to perform online periodic monitoring of local corrosion of pipe sections, and calculate the historical corrosion thinning rate of the monitored pipe section in the first N sampling periods based on the linear regression time factor expression. ,according to Calculate the prediction error of guided wave amplitude and the predicted guided wave amplitude of the N+1th sampling period , and then determine whether local corrosion abnormalities occur in the pipe section, and realize the identification and location of local corrosion defects; perform instantaneous electromagnetic scanning on the corrosion defect pipe section, and calculate the equivalent diameter of the local corrosion defect based on η, ε, λ, and κ obtained by fitting the least squares linear regression algorithm Such a setting can quantitatively identify local corrosion defects of equipment, improve the accuracy of corrosion defect detection, and meet the needs of safety risk monitoring of local corrosion defects of coated pipelines in practical applications.
[0064] 2. Calculate the equivalent diameter of local corrosion defects by setting the diameter correction coefficient , and according to , , Calculate the diameter correction factor ,use right Corrections are made to reduce the impact of differences in sensor length and diameter on detection accuracy, improve the accuracy of defect diameter calculation, and thus improve the accuracy of corrosion defect detection.
[0065] 3. Through the setting of the judgment step, since the local corrosion defect is a concave geometric shape, the corresponding initial phase angle of the electromagnetic signal is 90°±30°, while the weld is 270°±30°. Considering the possible non-ideal measurement state of the pipeline, the interval is enlarged to 45°. Because the weld is an interference source in actual measurement, eliminating the interference of the weld for sampling is beneficial to improve the accuracy of corrosion defect detection.
[0066] 4. By setting the defect depth calculation step, calculate the equivalent depth of the local corrosion defect according to the fitting coefficient and fitting constant ,according to Different values calculate different depth correction factors ,use right Correction is made and the equivalent depth is calculated using cross sections of different shapes The calculation is conducive to further determining the corrosion state of the local corrosion defects in the pipe section, thereby improving the accuracy of corrosion defect detection and meeting the needs of safety risk monitoring of local corrosion defects in coated pipelines in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 is a flow chart of Embodiment 1 of the present invention;
[0068] Figure 2 Schematic diagram of a corrosion anomaly identification double-fold line and a determination method thereof according to Embodiment 1 of the present invention;
[0069] Figure 3 Schematic diagram showing that the amplitude of the ultrasonic guided wave signal is proportional to the defect cross-sectional area in Example 1 of the present invention;
[0070] Figure 4 Schematic diagram showing that the instantaneous electromagnetic signal amplitude is proportional to the defect volume in Example 1 of the present invention;
[0071] Figure 5 It is a system diagram of embodiment 2 of the present invention. DETAILED DESCRIPTION
[0072] The following combination Figures 1 to 5 The present invention is described in further detail.
[0073] Example 1: This example discloses a quantitative identification method for local corrosion defects of equipment, referring to Figures 1 to 4 , including the following steps:
[0074] S1: Acquisition of data I: Ultrasonic guided wave monitoring of the pipe section for N sampling cycles, the monitoring cycle is , get the amplitude of the waveguide signal of the nth sampling period ;
[0075] S2: Calculate the corrosion rate: Calculate the historical corrosion thinning rate of the monitored pipe section , The calculation model is:
[0076] ;
[0077] S3: Calculate the regression intercept: Calculate the linear regression intercept b of the waveguide signal amplitude in the first N sampling periods GW , b GW The calculation model is:
[0078] ;
[0079] S4: Obtain prediction error: Calculate the prediction error of the guided wave amplitude based on the historical guided wave signal amplitude data of the monitored pipeline , The calculation model is:
[0080] ;
[0081] S5: Guided wave amplitude prediction: Calculate the predicted guided wave amplitude of the monitored pipe section in the N+1th sampling period based on historical data , The calculation model is:
[0082] ;
[0083] S6: Determine corrosion anomaly: Obtain the amplitude of the guided wave signal in the N+1th sampling period , if satisfied , it is judged that the pipe section has local corrosion abnormality and recorded as a corrosion defective pipe section. Otherwise, it is judged that no local corrosion abnormality has occurred;
[0084] S7: Acquiring data II: Perform instantaneous electromagnetic scanning of the corrosion defective pipe section for N sampling cycles, with a monitoring period of , obtain the instantaneous electromagnetic signal amplitude of the nth sampling period , phase angle ;
[0085] S8: Judgment: If the nth sampling period satisfies and , then judge is the effective instantaneous electromagnetic signal amplitude of the nth sampling period, otherwise, repeatedly execute the step of obtaining data II until the effective instantaneous electromagnetic signal amplitude is obtained;
[0086] S9: Calculate defect diameter: Calculate the equivalent diameter of localized corrosion defects , The calculation model is:
[0087] ;
[0088] Among them, η is the instantaneous electromagnetic linear fitting coefficient, ε is the instantaneous electromagnetic linear fitting constant, λ is the waveguide linear fitting coefficient, κ is the waveguide linear fitting constant, η and ε are obtained by fitting the historical instantaneous electromagnetic signal amplitude through the least squares linear regression algorithm, λ and κ are obtained by fitting the historical waveguide signal amplitude through the least squares linear regression algorithm, is the instantaneous electromagnetic signal amplitude of the Nth sampling period, is the amplitude of the waveguide signal in the Nth sampling period, is the diameter correction factor, The calculation model is:
[0089] ;
[0090] in, is the inner diameter of the monitored pipe section, is the electromagnetic footprint diameter of the instantaneous electromagnetic sensor of the monitored pipe section, is the length of a single sensor in the waveguide array group of the monitored pipe section;
[0091] S10: Calculate defect depth: Calculate the equivalent depth of local corrosion defects , The calculation model is:
[0092] ;
[0093] in is the depth correction factor, The calculation model is:
[0094] ;
[0095] Where t is the designed wall thickness of the monitored pipe section, is the inner diameter of the monitored pipe section, is the electromagnetic footprint diameter of the instantaneous electromagnetic sensor of the monitored pipe section, is the length of a single sensor in the waveguide array group of the monitored pipe section.
[0096] The implementation principle of the quantitative identification method of local corrosion defects of equipment in this embodiment is:
[0097] For a certain section of the coated pipeline, the local corrosion of the section is monitored online periodically using ultrasonic guided waves without destroying the integrity of the coating layer. The historical corrosion thinning rate of the monitored section within the first N sampling periods is calculated based on the linear regression time factor expression. ,according to Calculate the prediction error of guided wave amplitude and the predicted guided wave amplitude of the N+1th sampling period , and then through the ultrasonic guided wave signal amplitude of the N+1th sampling period and predicted guided wave amplitude Determine whether local corrosion abnormalities occur in the pipe section and identify and locate local corrosion defects.
[0098] Perform instantaneous electromagnetic scanning on the corrosion defective pipe section to obtain the instantaneous electromagnetic signal amplitude and phase angle , if satisfied and , then judge is the effective electromagnetic signal amplitude, otherwise the scan is repeated until the effective value is obtained; since the local corrosion defect is a concave geometric shape, the corresponding initial phase angle of the electromagnetic signal is 90°±30°, while that of the weld is 270°±30°. Considering the possible non-ideal measurement state of the pipeline, the interval is enlarged to 45°. Because the weld is the interference source in the actual measurement, the interference of the weld can be eliminated. Further narrowing the range limit has no obvious beneficial effect.
[0099] After scanning, the equivalent diameter of the local corrosion defect is calculated based on the mathematical relationship that the amplitude of the ultrasonic guided wave echo is proportional to the cross-sectional area of the local corrosion defect, and the amplitude of the low-frequency electromagnetic signal is proportional to the volume of the local corrosion defect, and the η, ε, λ, and κ obtained by fitting the least squares linear regression algorithm. , and according to , , Calculate the diameter correction factor ,use right Corrections are made to improve the accuracy of defect diameter calculation.
[0100] Calculate the equivalent depth of local corrosion defects based on the fitting coefficient and fitting constant ,according to Different values calculate different depth correction factors ,use right Correction; According to the statistics of actual measurement data, due to the diameter of local corrosion defects When the cross section of the local corrosion defect is ≤10mm, it can be approximated as a circle, and the equivalent depth can be calculated according to the circular cross section. On the contrary, the cross section of a local corrosion defect is closer to an oblong or rectangular cross section, so it is advisable to use a rectangular cross section to calculate the equivalent depth. , thereby improving the accuracy of defect depth calculation.
[0101] Such a setting improves the accuracy of corrosion defect detection, and on this basis, the corrosion state of the local corrosion defects in the pipe section can be further determined, and targeted corrosion online monitoring and regular inspection plans can be adopted to reduce the safe operation risks of risky corrosion circuits in process industries, and meet the needs of safety risk monitoring of local corrosion defects in coated pipelines in practical applications.
[0102] Reference Figure 2 , Figure 2 The mathematical principle of the double-fold line for identifying corrosion anomalies is that when the double-fold line presents a "concave" inflection point U, it can be judged that a dangerous corrosion anomaly has occurred at the corrosion defect point. Its mathematical expression is: if the predicted value Compared with the measured value Satisfies the following inequality , it is determined that local corrosion abnormality has occurred.
[0103] Example 2: This example discloses a quantitative identification system for local corrosion defects of equipment, referring to Figure 5 , including the following modules:
[0104] Acquisition module I: The output end is connected to the input end of the calculation module I, and is used to perform ultrasonic guided wave monitoring on the pipe section for N sampling cycles. The monitoring cycle is , get the amplitude of the waveguide signal of the nth sampling period ;
[0105] Calculation module I: The input end is connected to the output end of acquisition module I, and the output end is connected to the input end of calculation module II, which is used to calculate the historical corrosion thinning rate of the monitored pipe section according to the linear regression time factor expression ;
[0106] Calculation module II: The input end is connected to the output end of calculation module I, and the output end is connected to the input end of calculation module III, which is used to calculate the linear regression intercept b of the amplitude of the waveguide signal in the first N sampling periods. GW ;
[0107] Calculation module III: The input end is connected to the output end of calculation module II, and the output end is connected to the input end of prediction module, which is used to calculate the guided wave amplitude prediction error according to the historical guided wave signal amplitude data of the monitored pipeline. ;
[0108] Prediction module: The input end is connected to the output end of the calculation module III, and the output end is connected to the input end of the judgment module I, which is used to calculate the predicted guided wave amplitude of the monitored pipe section in the N+1th sampling period predicted based on historical data ;
[0109] Judgment module I: The input end is connected to the output end of the prediction module, and the output end is connected to the input end of the acquisition module II, which is used to obtain the amplitude of the waveguide signal in the N+1th sampling period , if satisfied , it is judged that the pipe section has local corrosion abnormality and recorded as a corrosion defective pipe section. Otherwise, it is judged that no local corrosion abnormality has occurred;
[0110] Acquisition module II: The input end is connected to the output end of judgment module I, and the output end is connected to the input end of judgment module II, which is used to perform instantaneous electromagnetic scanning of the corrosion defective pipe section for N sampling cycles. The monitoring cycle is , obtain the instantaneous electromagnetic signal amplitude of the nth sampling period , phase angle ;
[0111] Judgment module II: the input end is connected to the output end of acquisition module II, and the output end is connected to the input end of calculation module IV, which is used to determine if the nth sampling period meets the requirements. and , then judge is the effective instantaneous electromagnetic signal amplitude of the nth sampling period, otherwise, repeatedly execute the acquisition module II until the effective instantaneous electromagnetic signal amplitude is obtained;
[0112] Calculation module IV: The input end is connected to the output end of the acquisition module II, and the output end is connected to the input end of the calculation module V, which is used to calculate the equivalent diameter of the local corrosion defect according to the instantaneous electromagnetic signal amplitude of the Nth sampling period, the waveguide signal amplitude, and the fitting coefficient and fitting constant obtained by fitting the historical data through the least squares linear regression algorithm. The diameter correction factor is calculated based on the inner diameter of the monitored pipe section, the electromagnetic footprint diameter of the transient electromagnetic sensor, and the length of a single sensor in the waveguide array group. , and according to right Make corrections.
[0113] Calculation module V: The input end is connected to the output end of calculation module IV, and is used to calculate the equivalent depth of local corrosion defects according to the instantaneous electromagnetic signal amplitude of the Nth sampling period, the waveguide signal amplitude, and the fitting coefficient and fitting constant obtained by fitting the historical data through the least squares linear regression algorithm. The depth correction factor is calculated based on the designed wall thickness, inner diameter, electromagnetic footprint diameter of the transient electromagnetic sensor, and the length of a single sensor in the waveguide array group. , and according to right Make corrections.
[0114] The implementation principle of a quantitative identification system for local corrosion defects of equipment in this embodiment is as follows:
[0115] For a certain pipe section of the coated pipeline, without destroying the integrity of the coating layer, the local corrosion of the pipe section is monitored online periodically using ultrasonic guided waves. The acquisition module I obtains the amplitude of the guided wave signal. , the calculation module I calculates the historical corrosion thinning rate of the monitored pipe section in the first N sampling periods according to the linear regression time factor expression , calculation module II calculates the linear regression intercept b GW , calculation module III according to Calculate the prediction error of guided wave amplitude , the prediction module calculates the predicted guided wave amplitude of the N+1th sampling period , the judgment module I passes the ultrasonic guided wave signal amplitude of the N+1th sampling period and predicted guided wave amplitude Determine whether local corrosion abnormalities occur in the pipe section and identify and locate local corrosion defects.
[0116] Perform instantaneous electromagnetic scanning on the corrosion defective pipe section, and obtain the instantaneous electromagnetic signal amplitude in the acquisition module II and phase angle , if satisfied and , then the judgment module II judges is the effective electromagnetic signal amplitude, otherwise the scan is repeated until a valid value is obtained;
[0117] After scanning, the calculation module IV calculates the equivalent diameter of the local corrosion defect according to η, ε, λ, and κ obtained by fitting the least squares linear regression algorithm. , and according to , , Calculate the diameter correction factor ,use right After correction, calculation module IV calculates the equivalent depth of local corrosion defects based on the fitting coefficient and fitting constant. ,according to Different values calculate different depth correction factors ,use right Make corrections.
[0118] This setting improves the accuracy of corrosion defect detection, and thus the corrosion resistance of the equipment can be further judged based on this. Targeted online corrosion monitoring and regular inspection plans can be adopted to meet the needs of safety risk monitoring of local corrosion defects in coated pipelines in actual applications.
[0119] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A quantitative identification method for local corrosion defects of equipment, characterized in that: The following steps are involved: Acquisition of data I: Ultrasonic guided wave monitoring of the pipe section for N sampling cycles, the monitoring cycle is , get the amplitude of the waveguide signal of the nth sampling period ; Calculate corrosion rate: Calculate the historical corrosion thinning rate of the monitored pipe section , The calculation model is: ; Calculate the regression intercept: Calculate the linear regression intercept b of the waveguide signal amplitude in the first N sampling periods GW , b GW The calculation model is: ; Obtain prediction error: Calculate the prediction error of the guided wave amplitude based on the historical guided wave signal amplitude data of the monitored pipeline , The calculation model is: ; Guided wave amplitude prediction: Calculate the predicted guided wave amplitude of the monitored pipe section in the N+1th sampling period based on historical data , The calculation model is: ; Determine corrosion anomaly: obtain the amplitude of the guided wave signal in the N+1th sampling period , if satisfied , it is judged that the pipe section has local corrosion abnormality and recorded as a corrosion defective pipe section. Otherwise, it is judged that no local corrosion abnormality has occurred; Data acquisition II: Perform instantaneous electromagnetic scanning of the corrosion defective pipe section for N sampling cycles, with a monitoring period of , obtain the instantaneous electromagnetic signal amplitude of the nth sampling period , phase angle ; Calculate defect diameter: Calculate the equivalent diameter of localized corrosion defects , The calculation model is: ; Among them, η is the instantaneous electromagnetic linear fitting coefficient, ε is the instantaneous electromagnetic linear fitting constant, λ is the waveguide linear fitting coefficient, κ is the waveguide linear fitting constant, η and ε are obtained by fitting the historical instantaneous electromagnetic signal amplitude through the least squares linear regression algorithm, λ and κ are obtained by fitting the historical waveguide signal amplitude through the least squares linear regression algorithm, is the instantaneous electromagnetic signal amplitude of the Nth sampling period, is the amplitude of the waveguide signal in the Nth sampling period.
2. The method for quantitatively identifying local corrosion defects of equipment according to claim 1, characterized in that: In the step of calculating the defect diameter, The calculation model is updated as follows: ; in, is the diameter correction factor, The calculation model is: ; in, is the inner diameter of the monitored pipe section, is the electromagnetic footprint diameter of the instantaneous electromagnetic sensor of the monitored pipe section, is the length of a single sensor in the waveguide array group of the monitored pipe section.
3. The method for quantitatively identifying local corrosion defects of equipment according to claim 1, characterized in that: A judgment step is also provided between the step of obtaining data II and the step of calculating the defect diameter; Judgment: If the nth sampling period satisfies and , then judge is the effective instantaneous electromagnetic signal amplitude of the nth sampling period, otherwise, repeatedly execute the step of acquiring data II until the effective instantaneous electromagnetic signal amplitude is obtained.
4. A method for quantitatively identifying local corrosion defects of equipment according to any one of claims 1 to 3, characterized in that: After the defect diameter calculation step, there is also a defect depth calculation step; Calculate defect depth: Calculate the equivalent depth of localized corrosion defects , The calculation model is: 。 5. A quantitative identification method for local corrosion defects of equipment according to claim 4, characterized in that: In the step of calculating the defect depth, The calculation model is updated as follows: ; in is the depth correction factor, The calculation model is: ; Where t is the designed wall thickness of the monitored pipe section, is the inner diameter of the monitored pipe section, is the electromagnetic footprint diameter of the instantaneous electromagnetic sensor of the monitored pipe section, is the length of a single sensor in the waveguide array group of the monitored pipe section.
6. A quantitative identification system for local corrosion defects of equipment, using a quantitative identification method for local corrosion defects of equipment as claimed in any one of claims 1 to 5, characterized in that: Includes the following modules: Acquisition module I: The output end is connected to the input end of the calculation module I, and is used to perform ultrasonic guided wave monitoring on the pipe section for N sampling cycles. The monitoring cycle is , get the amplitude of the waveguide signal of the nth sampling period ; Calculation module I: The input end is connected to the output end of acquisition module I, and the output end is connected to the input end of calculation module II, which is used to calculate the historical corrosion thinning rate of the monitored pipe section according to the linear regression time factor expression ; Calculation module II: The input end is connected to the output end of calculation module I, and the output end is connected to the input end of calculation module III, which is used to calculate the linear regression intercept b of the amplitude of the waveguide signal in the first N sampling periods. GW ; Calculation module III: The input end is connected to the output end of calculation module II, and the output end is connected to the input end of prediction module, which is used to calculate the guided wave amplitude prediction error according to the historical guided wave signal amplitude data of the monitored pipeline. ; Prediction module: The input end is connected to the output end of the calculation module III, and the output end is connected to the input end of the judgment module I, which is used to calculate the predicted guided wave amplitude of the monitored pipe section in the N+1th sampling period predicted based on historical data ; Judgment module I: The input end is connected to the output end of the prediction module, and the output end is connected to the input end of the acquisition module II, which is used to obtain the amplitude of the waveguide signal in the N+1th sampling period , if satisfied , it is judged that the pipe section has local corrosion abnormality and recorded as a corrosion defective pipe section. Otherwise, it is judged that no local corrosion abnormality has occurred; Acquisition module II: The input end is connected to the output end of the judgment module I, and the output end is connected to the input end of the calculation module IV, which is used to perform instantaneous electromagnetic scanning of the corrosion defective pipe section for N sampling cycles. The monitoring cycle is , obtain the instantaneous electromagnetic signal amplitude of the nth sampling period , phase angle ; Calculation module IV: The input end is connected to the output end of the acquisition module II, and is used to calculate the equivalent diameter of the local corrosion defect according to the instantaneous electromagnetic signal amplitude of the Nth sampling period, the waveguide signal amplitude, and the fitting coefficient and fitting constant obtained by fitting the historical data through the least squares linear regression algorithm. .
7. A quantitative identification system for local corrosion defects of equipment according to claim 6, characterized in that: In calculation module IV, the diameter correction factor is also calculated based on the inner diameter of the monitored pipe section, the electromagnetic footprint diameter of the transient electromagnetic sensor, and the length of a single sensor in the waveguide array group. , and according to right Make corrections.
8. The quantitative identification system for local corrosion defects of equipment according to claim 6 is characterized by: It also includes a judgment module II; Judgment module II: the input end is connected to the output end of acquisition module II, and the output end is connected to the input end of calculation module IV, which is used to determine if the nth sampling period meets the requirements. and , then judge is the effective instantaneous electromagnetic signal amplitude of the nth sampling period, otherwise, the acquisition module II is repeatedly executed until the effective instantaneous electromagnetic signal amplitude is obtained.
9. A quantitative identification system for local corrosion defects of equipment according to any one of claims 6 to 8, characterized in that: It also includes a calculation module V: the input end is connected to the output end of the calculation module IV, and is used to calculate the equivalent depth of the local corrosion defect according to the instantaneous electromagnetic signal amplitude of the Nth sampling period, the waveguide signal amplitude, and the fitting coefficient and fitting constant obtained by fitting the historical data through the least squares linear regression algorithm. .
10. A quantitative identification system for local corrosion defects of equipment according to claim 9, characterized in that: In the calculation module V, the depth correction coefficient is also calculated based on the designed wall thickness, inner diameter, electromagnetic footprint diameter of the transient electromagnetic sensor, and the length of a single sensor in the waveguide array group. , and according to right Make corrections.