A high voltage cable and its production process
By using low-density polyethylene, cross-linking agent, methyl vinyl silicone rubber, anti-UV agent and voltage stabilizer in the cable insulation layer, combined with the graft structure of nano-cerium oxide and diphenylamine antioxidant, It solves the aging problem of cross-linked polyethylene insulation material and improves the thermal stability and anti-aging performance of the cable.
Patent Information
- Application Number
- CN202410431948.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-04-10
AI Technical Summary
Cross-linked polyethylene insulation materials are easily affected by factors such as oxygen aging, photo aging, electrical aging and water tree aging during use, leading to insulation breakdown and affecting the safe and stable operation of cables. Existing UV shielding agents and voltage stabilizers There are problems such as poor thermal stability, poor compatibility and easy migration and failure.
It uses high-density polyethylene sheath tube, flame-retardant tape layer, copper conductor and polypropylene filling rope. The insulation layer is composed of low-density polyethylene, cross-linking agent, methyl vinyl silicone rubber, anti-UV agent and voltage stabilizer. , the anti-UV agent is prepared through specific steps, and the intermediate is grafted with nanometer cerium oxide and diphenylamine antioxidants. The voltage stabilizer contains benzophenone and benzothiadiazole structures, which enhances the thermal stability and electrical tree properties of the material. .
It significantly improves the thermal stability, waterproofness, oxidative aging resistance, ultraviolet aging resistance and flame retardancy of the cable, extends the service life, and enhances the electrical branch resistance and waterproofing capabilities of the insulation layer.
Smart Images

Figure CN118315105B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials, and in particular relates to a high-voltage cable and a production process thereof. Background Art
[0002] Power cables usually include several conductors, an insulating layer wrapped around the conductors, a filling and fixing layer in the middle, and an outermost insulating protective sheath. The insulating layer is generally made of polyvinyl chloride or cross-linked polyethylene insulation material. Compared with polyvinyl chloride insulated cables, cross-linked polyethylene has the characteristics of simple structure, light weight, good heat resistance, strong load capacity, non-melting, chemical corrosion resistance, and high mechanical strength. However, during the use of cross-linked polyethylene insulation materials, it is inevitable to withstand aging effects such as oxygen aging, light aging, electrical aging, and water tree aging, which will lead to insulation breakdown, thereby affecting the safe and stable operation of the cable.
[0003] Choosing a suitable UV shielding agent can effectively slow down the photoaging phenomenon of insulating materials. At present, most commercial organic UV shielding agents are small molecules, which are prone to direct photoaging degradation and migration from the matrix to fail. At the same time, poor thermal stability also limits the protection life of organic UV shielding agents. Inorganic UV shielding agents have the advantages of good thermal stability and are not susceptible to free radical attacks, but they have poor compatibility with polymer matrices and a large difference in refractive index between the two, which easily causes the system to be opaque, thereby affecting the appearance of the material. Most inorganic UV shielding agents are semiconductor materials with high photocatalytic activity. Under ultraviolet light, they can trigger photochemical reactions, accelerate the aging and degradation of the polymer matrix, and shorten the service life of the protected material, limiting the use of inorganic UV shielding agents. In view of this, finding a suitable UV shielding agent and overcoming the shortcomings of existing UV shielding agents is still the goal that scholars today are striving to pursue.
[0004] The electrical aging of cable insulation materials refers to electrical tree aging, which is a cumulative breakdown phenomenon related to charge movement and trap distribution. In the process of electron capture and recombination, hot electrons gain energy, impact and destroy the molecular chain of the polymer, and then form a dendritic electron channel. Voltage stabilizer is an antioxidant that improves the electrical resistance of cross-linked polyethylene insulation materials by inhibiting electrical tree formation. Additive voltage stabilizers are prone to migration failure, and cross-linked polyethylene materials have certain flammability. It is necessary to find a suitable voltage stabilizer to improve the current problems. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a high voltage cable and a production process thereof.
[0006] The purpose of the present invention can be achieved through the following technical scheme: a high-voltage cable includes a sheath tube, a tape layer, an insulating layer, a conductor and a filling rope, the outer periphery of the conductor is coated with an insulating layer, the insulation layer and the tape layer are filled with filling ropes, and the outer periphery of the tape layer is coated with a sheath tube.
[0007] Furthermore, the sheath tube is a high-density polyethylene sheath tube, the tape layer is composed of a flame-retardant tape, the conductor is a copper conductor, the filling rope is a polypropylene filling rope, and the insulating layer is cross-linked polyethylene. The cross-linked polyethylene includes the following raw materials in parts by weight: 150-160 parts of low-density polyethylene, 10-12 parts of a cross-linking agent, 30-40 parts of methyl vinyl silicone rubber, 6.5-7.5 parts of an anti-ultraviolet agent, and 5.5-6.5 parts of a voltage stabilizer.
[0008] Furthermore, the cross-linking agent is benzoyl peroxide.
[0009] The anti-ultraviolet agent is prepared by the following steps:
[0010] Step A1: o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide are added into a flask to obtain a mixed solution a, and then 3,4-dihydroxybenzoyl chloride is added into the dimethyl sulfoxide solution to obtain a mixed solution b. The mixed solution b is slowly added dropwise into the mixed solution a in an ice-water bath at 0°C. After the addition is completed, the temperature is raised to 50-60°C, the reaction is carried out at a constant temperature for 6-8 hours, and distilled under reduced pressure to obtain an intermediate 1;
[0011] Further, the usage ratio of 3,4-dihydroxybenzoyl chloride, o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.1 mol: 0.01-0.015 mol: 100 mL;
[0012] During the reaction of step A1, o-aminodiphenylamine reacts with 3,4-dihydroxybenzoyl chloride to generate an amidation product intermediate 1. The structure of intermediate 1 is shown below:
[0013]
[0014] Step A2: Add toluene, hydrogenated silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum in a certain proportion into a three-necked flask, stir and introduce nitrogen protection, add 7-bromohept-1-en-3-one dropwise, slowly heat to 70-80°C, stir and react for 3-4h, and evacuate to obtain intermediate 2;
[0015] Further, the amount ratio of 7-bromohept-1-en-3-one, toluene, hydrogen-containing silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1-1.5 mol: 100 ml: 1 mol: 0.5 mol: 0.015-0.020 mol;
[0016] During the reaction of step A2, the hydrogen-containing silicone oil reacts with 7-bromohept-1-en-3-one under the catalysis of cis-dichlorobis(pyridyl)platinum, and the Si-H bond and the C=C bond are added to generate intermediate 2. The structure of intermediate 2 is shown below:
[0017]
[0018] Step A3: Add intermediate 2, intermediate 1 and methanol into a flask, add 2-dicyclohexylphosphine-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and stir at 80°C under nitrogen protection for 4-5h, and dry under vacuum at 50°C to obtain intermediate 3;
[0019] Further, the usage ratio of intermediate 2, intermediate 1, methanol, 2-dicyclohexylphosphino-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.06 mol: 300-350 mL: 0.0025 g: 0.0025 g: 0.15-0.18 mol;
[0020] During the reaction of step A3, intermediate 2 undergoes a dehydrobromination coupling reaction with intermediate 1 to generate intermediate 3. The structure of intermediate 3 is shown below:
[0021]
[0022] Step A4: adding nano-cerium oxide powder to an ethanol aqueous solution, stirring for 10 minutes to obtain a mixed solution c; then adding the intermediate 3 to the ethanol aqueous solution, stirring for 20 minutes to obtain a mixed solution d; then adding the mixed solution c and the mixed solution d to a flask, ultrasonically dispersing for 40 minutes to obtain a mixed system, and then adding acetic acid solution to the mixed system under stirring, adjusting the pH of the mixed system to 5.5-6.5, heating to 50° C., stirring for reaction for 10 hours, cooling to room temperature, centrifuging, washing three times with anhydrous ethanol, and then drying in an oven at 70° C. for 12 hours, grinding to obtain an anti-ultraviolet agent;
[0023] Furthermore, the dosage ratio of the nano-cerium oxide powder, the intermediate 3, the ethanol aqueous solution and the acetic acid solution is 0.1 g: 0.0012 mol: 55 mL: 0.3-0.4 mL, the volume fraction of the ethanol aqueous solution is 10%, and the concentration of the acetic acid solution is 1 mol / L;
[0024] During the reaction of step A4, the hydroxyl groups on the surface of nano-cerium oxide are grafted with the intermediate 3 to generate an anti-ultraviolet agent. In the anti-ultraviolet agent, the diphenylamine antioxidant structure inhibits or delays the breakage of the polymer molecular chain to generate free radicals, preventing the oxidation and aging of the polymer material; the flexible polysiloxane chain has high thermal stability, which improves the thermal stability of the anti-ultraviolet agent; after being grafted with the intermediate 3, the compatibility and dispersibility of the nano-cerium oxide and the polymer are increased, and the 3,4-dihydroxybenzene structure itself has strong anti-ultraviolet performance, and the ultraviolet absorption effect of the anti-ultraviolet agent is greatly improved.
[0025] The voltage stabilizer is prepared by the following steps:
[0026] Step B1: maleic anhydride and 2,4-dihydroxybenzophenone are added to a flask containing tetrahydrofuran, and concentrated sulfuric acid is added dropwise, the temperature is raised to 70-80°C, and the mixture is refluxed and stirred for reaction for 9-10 hours to obtain a reaction solution, the reaction solution is poured into deionized water, allowed to stand for 10-20 minutes, and the lower layer of oil is taken out after centrifugation, and placed in a vacuum drying oven at 80°C for drying for 2-4 hours to obtain intermediate a;
[0027] Furthermore, the dosage ratio of maleic anhydride, 2,4-dihydroxybenzophenone, concentrated sulfuric acid and deionized water is 0.11 mol: 0.10 mol: 10-12 mL: 200 mL, and the mass fraction of concentrated sulfuric acid is 98%;
[0028] During the reaction of step B1, maleic anhydride undergoes an esterification reaction with the less hindered phenolic hydroxyl group in 2,4-dihydroxybenzophenone to generate intermediate a. The structure of intermediate a is shown below:
[0029]
[0030] Step B2: In a nitrogen atmosphere, add intermediate a into a round-bottom flask, heat to 45°C, add tetrabutylammonium bromide, start stirring, slowly drop epichlorohydrin into the round-bottom flask, stir and react for 5-6 hours to obtain intermediate b;
[0031] Further, the usage ratio of intermediate a, tetrabutylammonium bromide and epichlorohydrin is 0.1 mol: 0.001-0.0012 mol: 0.1 mol;
[0032] During the reaction of step B2, intermediate a and epichlorohydrin undergo ring opening to generate intermediate b. The structure of intermediate b is shown below:
[0033]
[0034] Step B3: Add 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol to DMF, add intermediate b and sodium hydroxide under stirring, react at 40° C. for 4-4.5 hours, filter, wash with water, and dry to obtain a voltage stabilizer;
[0035] Further, the amount ratio of 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethan-1-ol, DMF, intermediate b and sodium hydroxide is: 0.1 mol: 180 mL: 0.1 mol: 0.1-0.2 g;
[0036] During the reaction of step B3, 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazine-1-yl)ethane-1-ol reacts with intermediate b to form a voltage stabilizer. In the voltage stabilizer, the benzophenone structure captures hot electrons under a high electric field and absorbs the energy of hot electrons by excitation. At the same time, the keto-enol tautomerism reaction also consumes the electron energy, weakening the effect of electrons on the molecular chain, thereby inhibiting the breakage of the polymer chain and making the voltage stabilizer have good resistance to electrical treeing; the benzothiadiazole structure has a large electron affinity, which has the greatest impact on the efficiency of the voltage stabilizer, and the larger the electron affinity, the better the ability to inhibit electrical treeing, thereby improving the ability of the voltage stabilizer to inhibit electrical treeing; in the piperazine ring and the thiadiazole structure It contains more nitrogen atoms and produces a large amount of inert gases when decomposed by heat. These inert non-flammable gases absorb heat and isolate oxygen. The endothermic reaction occurring during the decomposition process consumes most of the heat, reducing the surface temperature of the material and further preventing combustion and the spread of flames. The unsaturated double bonds allow the voltage stabilizer to be grafted into the cross-linked polyethylene through free radical reactions to avoid migration failure. The hydroxyl, carbonyl and nitrogen atoms can form hydrogen bonds with water molecules, thereby preventing diffusion to form water droplets, inhibiting the growth of water trees and playing an anti-water tree aging role.
[0037] The structure of the stabilizer is shown below:
[0038]
[0039] Beneficial effects of the present invention: The high-voltage cable prepared by the present invention comprises a sheath tube, a tape layer is arranged in the sheath tube, a plurality of conductors are arranged in the tape layer, an insulating layer is arranged on the periphery of the conductor, and a filling rope is filled between the tape and the insulating layer. The insulating layer is cross-linked polyethylene, and the cross-linked polyethylene includes raw materials such as low-density polyethylene, a cross-linking agent, methyl vinyl silicone rubber, an anti-ultraviolet agent and a voltage stabilizer. The insulating layer uses a mixture of low-density polyethylene with excellent electrical insulation performance and methyl vinyl silicone rubber with small compression deformation, which not only makes the insulation and pressure resistance of the material outstanding, but also the good dispersion and compatibility of methyl vinyl silicone rubber in low-density polyethylene also improve the strength of the cable. In the synthesized UV inhibitor, the diphenylamine antioxidant structure inhibits or delays the breakage of polymer molecular chains to produce free radicals, prevents the oxidation aging of cross-linked polyethylene, and prolongs the service life of the cable; the flexible polysiloxane chain has high thermal stability and is entangled with the cross-linked polyethylene chain to form a three-dimensional network, which improves the thermal stability and waterproofness of the cross-linked polyethylene, thereby improving the thermal stability and waterproofness of the cable; after being grafted with intermediate 3, the compatibility and dispersibility of nano-cerium oxide with the polymer increase, and with the entanglement of the polysiloxane chain and the cross-linked polyethylene chain, the 3,4-dihydroxybenzene structure is not easy to migrate and fail in the matrix, greatly improving the UV aging resistance of the cable. In addition, methyl vinyl silicone rubber still has thermal oxidation aging at high temperatures. The addition of cerium oxide helps to improve the thermal oxidation aging resistance of methyl vinyl silicone rubber.
[0040] In the synthesized voltage stabilizer, the benzophenone structure captures hot electrons under high electric fields and absorbs the energy of hot electrons by excitation. At the same time, the keto-enol tautomerism reaction also consumes the electron energy, weakening the influence of electrons on the molecular chain, thereby inhibiting the breakage of the polymer chain, improving the breakdown field strength and resistance to electrical treeing of the insulating layer, and inhibiting the electrical aging phenomenon of the cable; the benzothiadiazole structure has a large electron affinity, which has the greatest influence on the efficiency of the voltage stabilizer, and the larger the electron affinity, the better the ability to inhibit electrical treeing, thereby improving the ability of the insulating layer to inhibit electrical treeing, and further improving the resistance to electrical aging of the cable; The azine ring and thiadiazole structure contain a large number of nitrogen atoms. When decomposed by heat, a large amount of inert gas is produced. These inert non-flammable gases absorb heat and isolate oxygen. The endothermic reaction occurring during the decomposition process consumes most of the heat, reducing the surface temperature of the insulation layer, and further preventing combustion and the spread of flames, thereby improving the flame retardancy of the cable. The unsaturated double bond allows the voltage stabilizer to be grafted into the cross-linked polyethylene through a free radical reaction to avoid migration failure. The hydroxyl group, carbonyl group and nitrogen atoms can form hydrogen bonds with water molecules, thereby preventing the diffusion of water molecules to form water droplets, inhibiting the growth of water trees, and improving the cable's ability to resist water tree aging. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0042] Figure 1 The present invention is a schematic structural diagram of a high voltage-withstand cable.
[0043] In the accompanying drawings, the components represented by the reference numerals are listed as follows:
[0044] A. Sheath; B. Tape layer; C. Insulation layer; D. Conductor; E. Filling rope. DETAILED DESCRIPTION
[0045] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] Example 1
[0047] An anti-ultraviolet agent is prepared by the following steps:
[0048] Step A1: o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide are added to a flask to obtain a mixed solution a, and then 3,4-dihydroxybenzoyl chloride is added to the dimethyl sulfoxide solution to obtain a mixed solution b. The mixed solution b is slowly added dropwise to the mixed solution a in an ice-water bath at 0°C. After the addition is completed, the temperature is raised to 50°C, and the reaction is carried out at a constant temperature for 6 hours, and distillation is performed under reduced pressure to obtain an intermediate 1; the amount ratio of 3,4-dihydroxybenzoyl chloride, o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.1 mol: 0.01 mol: 100 mL;
[0049] Step A2: Toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum are added into a three-necked flask in a certain proportion, stirred and nitrogen is introduced for protection, 7-bromohept-1-en-3-one is added dropwise, the temperature is slowly raised to 70° C., stirred for reaction for 3 hours, and vacuumed to obtain intermediate 2; the amount ratio of 7-bromohept-1-en-3-one, toluene, hydrogen-containing silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1 mol: 100 ml: 1 mol: 0.5 mol: 0.015 mol;
[0050] Step A3: Add intermediate 2, intermediate 1 and methanol into a flask, add 2-dicyclohexylphosphine-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and react for 4 hours at 80°C under nitrogen protection, and vacuum dry at 50°C to obtain intermediate 3; the amount ratio of intermediate 2, intermediate 1, methanol, 2-dicyclohexylphosphine-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.06 mol: 300 mL: 0.0025 g: 0.0025 g: 0.15 mol;
[0051] Step A4: adding nano cerium oxide powder to an ethanol aqueous solution, stirring for 10 minutes to obtain a mixed solution c; then adding the intermediate 3 to the ethanol aqueous solution, stirring for 20 minutes to obtain a mixed solution d; then adding the mixed solution c and the mixed solution d to a flask, ultrasonically dispersing for 40 minutes to obtain a mixed system, then adding an acetic acid solution to the mixed system under stirring, adjusting the pH of the mixed system to 5.5, heating to 50° C., stirring for reaction for 10 hours, cooling to room temperature, centrifuging, washing three times with anhydrous ethanol, and then drying in an oven at 70° C. for 12 hours, grinding to obtain an anti-ultraviolet agent; the amount ratio of nano cerium oxide powder, intermediate 3, ethanol aqueous solution and acetic acid solution is 0.1g: 0.0012mol: 55mL: 0.3mL, the volume fraction of the ethanol aqueous solution is 10%, and the concentration of the acetic acid solution is 1mol / L.
[0052] Example 2
[0053] An anti-ultraviolet agent is prepared by the following steps:
[0054] Step A1: o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide are added into a flask to obtain a mixed solution a, and then 3,4-dihydroxybenzoyl chloride is added into the dimethyl sulfoxide solution to obtain a mixed solution b. The mixed solution b is slowly added dropwise into the mixed solution a in an ice-water bath at 0°C. After the addition is completed, the temperature is raised to 55°C, and the reaction is carried out at a constant temperature for 7 hours, and distilled under reduced pressure to obtain an intermediate 1; the amount ratio of 3,4-dihydroxybenzoyl chloride, o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.1 mol: 0.012 mol: 100 mL;
[0055] Step A2: Toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum are added into a three-necked flask in a certain proportion, stirred and nitrogen is introduced for protection, 7-bromohept-1-en-3-one is added dropwise, the temperature is slowly raised to 75° C., the reaction is stirred for 3.5 hours, and vacuum is applied to obtain intermediate 2; the amount ratio of 7-bromohept-1-en-3-one, toluene, hydrogen-containing silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1.2 mol: 100 ml: 1 mol: 0.5 mol: 0.017 mol;
[0056] Step A3: Add intermediate 2, intermediate 1 and methanol into a flask, add 2-dicyclohexylphosphine-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and react for 4.5 hours at 80°C under nitrogen protection, and vacuum dry at 50°C to obtain intermediate 3; the amount ratio of intermediate 2, intermediate 1, methanol, 2-dicyclohexylphosphine-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.06 mol: 320 mL: 0.0025 g: 0.0025 g: 0.16 mol;
[0057] Step A4: adding nano cerium oxide powder to an ethanol aqueous solution, stirring for 10 minutes to obtain a mixed solution c; then adding the intermediate 3 to the ethanol aqueous solution, stirring for 20 minutes to obtain a mixed solution d; then adding the mixed solution c and the mixed solution d to a flask, ultrasonically dispersing for 40 minutes to obtain a mixed system, then adding an acetic acid solution to the mixed system under stirring, adjusting the pH of the mixed system to 6.0, heating to 50° C., stirring for reaction for 10 hours, cooling to room temperature, centrifuging, washing three times with anhydrous ethanol, and then drying in an oven at 70° C. for 12 hours, grinding to obtain an anti-ultraviolet agent; the amount ratio of nano cerium oxide powder, intermediate 3, ethanol aqueous solution and acetic acid solution is 0.1g: 0.0012mol: 55mL: 0.35mL, the volume fraction of the ethanol aqueous solution is 10%, and the concentration of the acetic acid solution is 1mol / L.
[0058] Example 3
[0059] An anti-ultraviolet agent is prepared by the following steps:
[0060] Step A1: o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide are added into a flask to obtain a mixed solution a, and then 3,4-dihydroxybenzoyl chloride is added into the dimethyl sulfoxide solution to obtain a mixed solution b. The mixed solution b is slowly added dropwise into the mixed solution a in an ice-water bath at 0°C. After the addition is completed, the temperature is raised to 60°C, and the reaction is carried out at a constant temperature for 8 hours, and distillation is performed under reduced pressure to obtain an intermediate 1; the amount ratio of 3,4-dihydroxybenzoyl chloride, o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.1 mol: 0.015 mol: 100 mL;
[0061] Step A2: Toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum are added into a three-necked flask in a certain proportion, stirred and nitrogen is introduced for protection, 7-bromohept-1-en-3-one is added dropwise, the temperature is slowly raised to 80° C., stirred for reaction for 4 hours, and vacuumed to obtain intermediate 2; the amount ratio of 7-bromohept-1-en-3-one, toluene, hydrogen-containing silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1.5 mol: 100 ml: 1 mol: 0.5 mol: 0.020 mol;
[0062] Step A3: Add intermediate 2, intermediate 1 and methanol into a flask, add 2-dicyclohexylphosphine-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and react for 5 h at 80°C under nitrogen protection, and vacuum dry at 50°C to obtain intermediate 3; the amount ratio of intermediate 2, intermediate 1, methanol, 2-dicyclohexylphosphine-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.06 mol: 350 mL: 0.0025 g: 0.0025 g: 0.18 mol;
[0063] Step A4: adding nano cerium oxide powder to ethanol aqueous solution, stirring for 10 minutes to obtain a mixed solution c; then adding intermediate 3 to ethanol aqueous solution, stirring for 20 minutes to obtain a mixed solution d; then adding mixed solution c and mixed solution d to a flask, ultrasonically dispersing for 40 minutes to obtain a mixed system, then adding acetic acid solution to the mixed system under stirring, adjusting the pH of the mixed system to 6.5, heating to 50° C., stirring for reaction for 10 hours, cooling to room temperature, centrifuging, washing three times with anhydrous ethanol, and then drying in an oven at 70° C. for 12 hours, grinding to obtain an anti-ultraviolet agent; the amount ratio of nano cerium oxide powder, intermediate 3, ethanol aqueous solution and acetic acid solution is 0.1g: 0.0012mol: 55mL: 0.4mL, the volume fraction of ethanol aqueous solution is 10%, and the concentration of acetic acid solution is 1mol / L.
[0064] Example 4
[0065] A voltage stabilizer is prepared by the following steps:
[0066] Step B1: maleic anhydride and 2,4-dihydroxybenzophenone are added to a flask containing tetrahydrofuran, and then concentrated sulfuric acid is added dropwise, the temperature is raised to 70°C, and the mixture is refluxed and stirred for reaction for 9 hours to obtain a reaction solution, the reaction solution is poured into deionized water, allowed to stand for 10 minutes, and the lower layer of oil is taken out after centrifugation, and placed in a vacuum drying oven at 80°C for 2 hours to obtain intermediate a; the dosage ratio of maleic anhydride, 2,4-dihydroxybenzophenone, concentrated sulfuric acid and deionized water is 0.11 mol: 0.10 mol: 10 mL: 200 mL, and the mass fraction of concentrated sulfuric acid is 98%;
[0067] Step B2: In a nitrogen atmosphere, add intermediate a into a round-bottom flask, heat to 45°C, add tetrabutylammonium bromide, start stirring, slowly drop epichlorohydrin into the round-bottom flask, stir and react for 5 hours to obtain intermediate b; the amount ratio of intermediate a, tetrabutylammonium bromide and epichlorohydrin is 0.1 mol: 0.001 mol: 0.1 mol;
[0068] Step B3: Add 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol to DMF, add intermediate b and sodium hydroxide under stirring, react at 40°C with stirring for 4 hours, filter, wash with water, and dry to obtain a voltage stabilizer; the dosage ratio of 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol, DMF, intermediate b and sodium hydroxide is: 0.1 mol: 180 mL: 0.1 mol: 0.1 g.
[0069] Example 5
[0070] A voltage stabilizer is prepared by the following steps:
[0071] Step B1: maleic anhydride and 2,4-dihydroxybenzophenone are added to a flask containing tetrahydrofuran, and then concentrated sulfuric acid is added dropwise, the temperature is raised to 75°C, and the mixture is refluxed and stirred for reaction for 9.5 hours to obtain a reaction solution, the reaction solution is poured into deionized water, allowed to stand for 15 minutes, and the lower layer of oil is taken out after centrifugation, and placed in a vacuum drying oven at 80°C for 3 hours to obtain intermediate a; the dosage ratio of maleic anhydride, 2,4-dihydroxybenzophenone, concentrated sulfuric acid and deionized water is 0.11 mol: 0.10 mol: 11 mL: 200 mL, and the mass fraction of concentrated sulfuric acid is 98%;
[0072] Step B2: In a nitrogen atmosphere, add intermediate a into a round-bottom flask, heat to 45°C, add tetrabutylammonium bromide, start stirring, slowly drop epichlorohydrin into the round-bottom flask, stir and react for 5.5h to obtain intermediate b; the amount ratio of intermediate a, tetrabutylammonium bromide and epichlorohydrin is 0.1mol:0.0011mol:0.1mol;
[0073] Step B3: Add 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol to DMF, add intermediate b and sodium hydroxide under stirring, react at 40°C with stirring for 4.2h, filter, wash with water, and dry to obtain a voltage stabilizer; the dosage ratio of 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol, DMF, intermediate b and sodium hydroxide is: 0.1mol:180mL:0.1mol:0.15g.
[0074] Example 6
[0075] A voltage stabilizer is prepared by the following steps:
[0076] Step B1: maleic anhydride and 2,4-dihydroxybenzophenone are added to a flask containing tetrahydrofuran, and then concentrated sulfuric acid is added dropwise, the temperature is raised to 80°C, and the mixture is refluxed and stirred for reaction for 10 hours to obtain a reaction solution, the reaction solution is poured into deionized water, allowed to stand for 20 minutes, and the lower layer of oil is taken out after centrifugation, and placed in a vacuum drying oven at 80°C for 4 hours to obtain intermediate a; the dosage ratio of maleic anhydride, 2,4-dihydroxybenzophenone, concentrated sulfuric acid and deionized water is 0.11 mol: 0.10 mol: 12 mL: 200 mL, and the mass fraction of concentrated sulfuric acid is 98%;
[0077] Step B2: In a nitrogen atmosphere, add intermediate a into a round-bottom flask, heat to 45°C, add tetrabutylammonium bromide, start stirring, slowly drop epichlorohydrin into the round-bottom flask, stir and react for 6 hours to obtain intermediate b; the amount ratio of intermediate a, tetrabutylammonium bromide and epichlorohydrin is 0.1 mol: 0.0012 mol: 0.1 mol;
[0078] Step B3: Add 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol to DMF, add intermediate b and sodium hydroxide under stirring, react at 40°C with stirring for 4.5h, filter, wash with water, and dry to obtain a voltage stabilizer; the dosage ratio of 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol, DMF, intermediate b and sodium hydroxide is: 0.1mol:180mL:0.1mol:0.2g.
[0079] Example 7
[0080] like Figure 1 A high-voltage cable is shown, comprising a sheath tube A, a tape layer B, an insulating layer C, a conductor D and a filling rope E, wherein the outer periphery of the conductor D is coated with the insulating layer C, the filling rope E is filled between the insulating layer C and the tape layer B, and the outer periphery of the tape layer B is coated with the sheath tube A. The sheath tube A is a high-density polyethylene sheath tube, the tape layer B is composed of a flame-retardant tape, the conductor D is a copper conductor, the filling rope E is a polypropylene filling rope, the insulating layer C is cross-linked polyethylene, and the cross-linked polyethylene comprises the following raw materials in parts by weight: 150 parts of low-density polyethylene, 10 parts of a cross-linking agent, 30 parts of methyl vinyl silicone rubber, 6.5 parts of an anti-ultraviolet agent and 5.5 parts of a voltage stabilizer.
[0081] The high voltage cable is prepared by the following steps:
[0082] Step S1: low-density polyethylene is placed in a rheometer for melt blending, mixed at 105° C. and a rotation speed of 50 r / min for 4 min, then the voltage stabilizer and cross-linking agent obtained in Example 4 are added, mixed for another 3 min, methyl vinyl silicone rubber and the anti-ultraviolet agent obtained in Example 1 are added, and finally mixed for 10 min to obtain cross-linked polyethylene;
[0083] Step S2: using an extruder to extrude cross-linked polyethylene on the outside of the copper conductor to form an insulating layer wrapped around the conductor, and then annealing the conductor after extrusion to obtain a cable core; placing the cable core and the polypropylene filling rope, and then wrapping it with a flame-retardant tape to form a tape layer, so that the space between the tape layer and the insulating layer is filled with polypropylene filling rope, and then using an extruder to extrude high-density polyethylene on the outside of the tape layer to form a sheath layer wrapped around the tape layer, and then annealing the conductor after extrusion to obtain a high-voltage cable.
[0084] Example 8
[0085] like Figure 1 A high-voltage cable is shown, comprising a sheath tube A, a tape layer B, an insulating layer C, a conductor D and a filling rope E, wherein the outer periphery of the conductor D is coated with the insulating layer C, the filling rope E is filled between the insulating layer C and the tape layer B, and the outer periphery of the tape layer B is coated with the sheath tube A. The sheath tube A is a high-density polyethylene sheath tube, the tape layer B is composed of a flame-retardant tape, the conductor D is a copper conductor, the filling rope E is a polypropylene filling rope, the insulating layer C is cross-linked polyethylene, and the cross-linked polyethylene comprises the following raw materials in parts by weight: 155 parts of low-density polyethylene, 11 parts of a cross-linking agent, 35 parts of methyl vinyl silicone rubber, 7 parts of an anti-ultraviolet agent and 6 parts of a voltage stabilizer.
[0086] The high voltage cable is prepared by the following steps:
[0087] Step S1: low-density polyethylene is placed in a rheometer for melt blending, mixed at 105° C. and a rotation speed of 50 r / min for 5 minutes, and then the voltage stabilizer and cross-linking agent obtained in Example 5 are added, and then mixed for another 3 minutes, and then methyl vinyl silicone rubber and the anti-ultraviolet agent obtained in Example 2 are added, and finally mixed for 12 minutes to obtain cross-linked polyethylene;
[0088] Step S2: using an extruder to extrude cross-linked polyethylene on the outside of the copper conductor to form an insulating layer wrapped around the conductor, and then annealing the conductor after extrusion to obtain a cable core; placing the cable core and the polypropylene filling rope, and then wrapping it with a flame-retardant tape to form a tape layer, so that the space between the tape layer and the insulating layer is filled with polypropylene filling rope, and then using an extruder to extrude high-density polyethylene on the outside of the tape layer to form a sheath layer wrapped around the tape layer, and then annealing the conductor after extrusion to obtain a high-voltage cable.
[0089] Example 9
[0090] like Figure 1A high-voltage cable is shown, comprising a sheath tube A, a tape layer B, an insulating layer C, a conductor D and a filling rope E, wherein the outer periphery of the conductor D is coated with the insulating layer C, the filling rope E is filled between the insulating layer C and the tape layer B, and the outer periphery of the tape layer B is coated with the sheath tube A. The sheath tube A is a high-density polyethylene sheath tube, the tape layer B is composed of a flame-retardant tape, the conductor D is a copper conductor, the filling rope E is a polypropylene filling rope, the insulating layer C is cross-linked polyethylene, and the cross-linked polyethylene comprises the following raw materials in parts by weight: 160 parts of low-density polyethylene, 12 parts of a cross-linking agent, 40 parts of methyl vinyl silicone rubber, 7.5 parts of an anti-ultraviolet agent and 6.5 parts of a voltage stabilizer.
[0091] The high voltage cable is prepared by the following steps:
[0092] Step S1: low-density polyethylene is placed in a rheometer for melt blending, mixed at 110° C. and a rotation speed of 50 r / min for 6 min, then the voltage stabilizer and cross-linking agent obtained in Example 6 are added, mixed for another 3 min, methyl vinyl silicone rubber and the anti-ultraviolet agent obtained in Example 3 are added, and finally mixed for 15 min to obtain cross-linked polyethylene;
[0093] Step S2: using an extruder to extrude cross-linked polyethylene on the outside of the copper conductor to form an insulating layer wrapped around the conductor, and then annealing the conductor after extrusion to obtain a cable core; placing the cable core and the polypropylene filling rope, and then wrapping it with a flame-retardant tape to form a tape layer, so that the space between the tape layer and the insulating layer is filled with polypropylene filling rope, and then using an extruder to extrude high-density polyethylene on the outside of the tape layer to form a sheath layer wrapped around the tape layer, and then annealing the conductor after extrusion to obtain a high-voltage cable.
[0094] Comparative Example 1
[0095] This comparative example is a commercially available voltage-resistant cable.
[0096] Comparative Example 2
[0097] The anti-ultraviolet agent was replaced with nano-cerium oxide modified with ethyl 3,4-dihydroxybenzoate, and the other steps were exactly the same as those in Example 9 to prepare a high-voltage cable.
[0098] Comparative Example 3
[0099] The voltage stabilizer was replaced by the esterification product of 2,4-dihydroxybenzophenone and maleic anhydride, namely intermediate a, and the other steps were exactly the same as in Example 9 to obtain a high-voltage cable.
[0100] The high voltage cable prepared by the present invention is further tested for its effect, and the test results are as follows.
[0101] In order to test the high-voltage cable prepared by the present invention, according to GB / T 2951-2008 "General test methods for insulation and sheath materials of electric and optical cables", ASTM D624, GB / T11017.1 "Rated voltage 110kV cross-linked polyethylene insulated power cable and its accessories", the ultraviolet aging condition is 0.89W / m 2 The test was carried out according to the method of temperature of 50℃, aging time of 500h, "GB / T 2406-93 Plastic Combustion Performance Test Method", etc. The results are shown in Table 1.
[0102] Table 1:
[0103]
[0104]
[0105] The test method of the AC and DC breakdown field strength in Table 1 is: apply a linearly increasing AC or DC voltage to a 100 μm film sample of a cross-linked polyethylene material until the sample breaks down, and obtain the average AC and DC breakdown field strength of 10 samples;
[0106] The test method for the average electrical tree initiation voltage in Table 1 is: the electrical tree initiation voltage of the cross-linked polyethylene material is tested using a needle-plate electrode structure, the needle-plate distance is 3 mm, the needle tip curvature radius is 5 μm, the boost method is linear boost, and the average electrical tree initiation voltage of 10 samples is obtained.
[0107] According to the data in Table 1, compared with Example 1, Example 7, Example 8 and Example 9, it can be seen that the high-voltage cable prepared by the present invention has higher thermal stability, strength, water resistance, resistance to oxygen aging and resistance to ultraviolet aging than commercially available high-voltage cables; compared with Comparative Example 2, Example 9 shows that the use of a synthetic anti-ultraviolet agent, the introduction of a diphenylamine antioxidant structure, a flexible polysiloxane chain, a 3,4-dihydroxybenzene structure and nano-cerium oxide, improves the thermal stability, water resistance, resistance to oxygen aging and resistance to ultraviolet aging of the high-voltage cable; compared with Comparative Example 3, Example 9 shows that the use of a voltage stabilizer improves the flame retardancy and electrical aging resistance of the high-voltage cable.
[0108] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A high voltage cable, characterized in that: It comprises a sheath tube A, a tape layer B, an insulating layer C, a conductor D and a filling rope E, wherein the outer periphery of the conductor D is coated with the insulating layer C, the filling rope E is filled between the insulating layer C and the tape layer B, and the outer periphery of the tape layer B is coated with the sheath tube A; the sheath tube A is a high-density polyethylene sheath tube, the tape layer B is composed of a flame-retardant tape, the conductor D is a copper conductor, the filling rope E is a polypropylene filling rope, the insulating layer C is cross-linked polyethylene, and the cross-linked polyethylene comprises the following raw materials in parts by weight: 150-160 parts of low-density polyethylene, 10-12 parts of a cross-linking agent, 30-40 parts of methyl vinyl silicone rubber, 6.5-7.5 parts of an anti-ultraviolet agent and 5.5-6.5 parts of a voltage stabilizer; the cross-linking agent is benzoyl peroxide; The anti-ultraviolet agent is prepared by the following steps: Step A1: o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide are added into a flask to obtain a mixed solution a, and then 3,4-dihydroxybenzoyl chloride is added into the dimethyl sulfoxide solution to obtain a mixed solution b. The mixed solution b is slowly added dropwise into the mixed solution a in an ice water bath at 0°C. After the addition is completed, the temperature is raised to 50-60°C, the reaction is carried out at a constant temperature for 6-8 hours, and distilled under reduced pressure to obtain an intermediate 1; Step A2: Add toluene, hydrogenated silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum in a certain proportion into a three-necked flask, stir and introduce nitrogen protection, add 7-bromohept-1-en-3-one dropwise, slowly heat to 70-80°C, stir and react for 3-4h, and evacuate to obtain intermediate 2; Step A3: add intermediate 2, intermediate 1 and methanol into a flask, add 2-dicyclohexylphosphino-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and stir at 80°C under nitrogen protection for 4-5h, and dry under vacuum at 50°C to obtain intermediate 3; Step A4: adding nano-cerium oxide powder to an ethanol aqueous solution, stirring for 10 minutes to obtain a mixed solution c; then adding the intermediate 3 to the ethanol aqueous solution, stirring for 20 minutes to obtain a mixed solution d; Then, the mixed solution c and the mixed solution d are added to the flask, and ultrasonically dispersed for 40 minutes to obtain a mixed system, and then the acetic acid solution is added to the mixed system under stirring, and the pH of the mixed system is adjusted to 5.5-6.5, and the temperature is raised to 50° C., and the mixture is stirred for reaction for 10 hours, cooled to room temperature, centrifuged, washed three times with anhydrous ethanol, and then dried in an oven at 70° C. for 12 hours, and ground to obtain an anti-ultraviolet agent; The voltage stabilizer is prepared by the following steps: Step B1: maleic anhydride and 2,4-dihydroxybenzophenone are added to a flask containing tetrahydrofuran, and concentrated sulfuric acid is added dropwise, the temperature is raised to 70-80°C, and the mixture is refluxed and stirred for reaction for 9-10 hours to obtain a reaction solution, the reaction solution is poured into deionized water, allowed to stand for 10-20 minutes, and the lower layer of oil is taken out after centrifugation, and placed in a vacuum drying oven at 80°C for drying for 2-4 hours to obtain intermediate a; Step B2: In a nitrogen atmosphere, add intermediate a into a round-bottom flask, heat to 45°C, add tetrabutylammonium bromide, start stirring, slowly drop epichlorohydrin into the round-bottom flask, stir and react for 5-6 hours to obtain intermediate b; Step B3: Add 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol to DMF, add intermediate b and sodium hydroxide under stirring, react at 40°C with stirring for 4-4.5h, filter, wash with water, and dry to obtain a voltage stabilizer.
2. A high voltage cable according to claim 1, characterized in that: In step A1, the usage ratio of 3,4-dihydroxybenzoyl chloride, o-aminodiphenylamine, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.1 mol: 0.01-0.015 mol: 100 mL; In step A2, the amount ratio of 7-bromohept-1-en-3-one, toluene, hydrogenated silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1-1.5 mol: 100 ml: 1 mol: 0.5 mol: 0.015-0.020 mol.
3. A high voltage cable according to claim 1, characterized in that: In step A3, the usage ratio of intermediate 2, intermediate 1, methanol, 2-dicyclohexylphosphino-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.06 mol: 300-350 mL: 0.0025 g: 0.0025 g: 0.15-0.18 mol.
4. A high voltage cable according to claim 1, characterized in that: In step A4, the dosage ratio of nano-cerium oxide powder, intermediate 3, ethanol aqueous solution and acetic acid solution is 0.1g:0.0012mol:55mL:0.3-0.4mL, the volume fraction of ethanol aqueous solution is 10%, and the concentration of acetic acid solution is 1mol / L.
5. A high voltage cable according to claim 1, characterized in that: In step B1, the dosage ratio of maleic anhydride, 2,4-dihydroxybenzophenone, concentrated sulfuric acid and deionized water is 0.11 mol: 0.10 mol: 10-12 mL: 200 mL, and the mass fraction of concentrated sulfuric acid is 98%.
6. A high voltage cable according to claim 1, characterized in that: In step B2, the usage ratio of intermediate a, tetrabutylammonium bromide and epichlorohydrin is 0.1 mol: 0.001-0.0012 mol: 0.1 mol.
7. A high voltage cable according to claim 1, characterized in that: In step B3, the usage ratio of 2-(4-(benzo[C][1,2,5]thiadiazol-5-ylmethyl)piperazin-1-yl)ethane-1-ol, DMF, intermediate b and sodium hydroxide is: 0.1 mol: 180 mL: 0.1 mol: 0.1-0.2 g.
8. The production process of a high voltage cable according to claim 1, characterized in that: Prepared by the following steps: Step S1: low-density polyethylene is placed in a rheometer for melt blending, mixed at 105-110° C. and a rotation speed of 50 r / min for 4-6 minutes, then a voltage stabilizer and a cross-linking agent are added, mixed for another 3 minutes, methyl vinyl silicone rubber and an anti-ultraviolet agent are added, and finally mixed for 10-15 minutes to obtain cross-linked polyethylene; Step S2: using an extruder to extrude cross-linked polyethylene on the outside of the copper conductor to form an insulating layer wrapped around the conductor, and then annealing the conductor after extrusion to obtain a cable core; placing the cable core and the polypropylene filling rope, and then wrapping it with a flame-retardant tape to form a tape layer, so that the space between the tape layer and the insulating layer is filled with polypropylene filling rope, and then using an extruder to extrude high-density polyethylene on the outside of the tape layer to form a sheath layer wrapped around the tape layer, and then annealing the conductor after extrusion to obtain a high-voltage cable.
Citation Information
Patent Citations
Silicone rubber power cable insulating layer and sheath material
CN103333504A
Crosslinked polyethylene insulated corrosion-resistant power cable
CN114300188A
Tree resistant cable
WO1998059348A1