A semiconductor light emitting structure and a method for preparing the same

By designing nano-scale concave and convex structures in the semiconductor light-emitting structure to increase the contact area and adhesion, the problem of contact resistance and stability of the semiconductor laser under high current is solved, and the effect of reducing the operating voltage and improving long-term stability is achieved.

CN118315923BActive Publication Date: 2024-10-11SUZHOU GANBRIGHT OPTOELECTRONIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410666958.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-10-11
Estimated Expiration
2044-05-28

Smart Images

  • Figure CN118315923B_ABST
    Figure CN118315923B_ABST
Patent Text Reader

Abstract

The present application provides a semiconductor light-emitting structure and a preparation method thereof, wherein the semiconductor light-emitting structure comprises: a stacked first limiting layer, a first waveguide layer, an active layer, a second waveguide layer, a second limiting layer, a contact layer and a front electrode layer; the surface of the contact layer facing away from the active layer has a first concave-convex structure of nanometer scale, the first concave-convex structure comprises a plurality of first protrusions and a first depression located between the first protrusions; the surface of the front electrode layer facing the contact layer has a second concave-convex structure of nanometer scale, the second concave-convex structure comprises a plurality of second protrusions and a second depression located between the second protrusions; wherein the first protrusion is located in the second depression, and the second protrusion is located in the first depression. The stability of the contact between the contact layer and the front electrode layer under high current is improved, the operating voltage of the semiconductor light-emitting structure is reduced, and the long-term working stability of the semiconductor light-emitting structure is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor light-emitting structure and a preparation method thereof. Background Art

[0002] The third generation semiconductor material gallium nitride (GaN) based light emitting diodes (LEDs) have been widely used in the fields of lighting and display. White light lighting, LED rear projection TVs, micro-LED displays (micro-LEDs) based on GaN-based LEDs have all set off changes in the corresponding industries. GaN-based semiconductor lasers with more complex epitaxial structures have the characteristics of good monochromaticity, high efficiency, high power density, good directionality, low cost, and small size. They have broader application prospects in the fields of laser projection display, laser lighting, and industrial laser processing. When semiconductor lasers work under the state of large current injection, they have higher requirements for the contact resistance of semiconductor lasers and the adhesion between the contact layer and the electrode. Summary of the invention

[0003] The present application provides a semiconductor light-emitting structure and a preparation method thereof, which improves the contact stability between the contact layer and the front electrode layer under large current, reduces the operating voltage of the semiconductor light-emitting structure, and improves the long-term working stability of the semiconductor light-emitting structure.

[0004] In order to solve the above technical problems, the present invention provides a semiconductor light-emitting structure, including: a stacked first limiting layer, a first waveguide layer, an active layer, a second waveguide layer, a second limiting layer, a contact layer and a front electrode layer; the surface of the contact layer facing away from the active layer has a first concave-convex structure of nanometer scale, and the first concave-convex structure includes a plurality of first protrusions and a first depression located between the first protrusions; the surface of the front electrode layer facing the contact layer has a second concave-convex structure of nanometer scale, and the second concave-convex structure includes a plurality of second protrusions and a second depression located between the second protrusions; wherein the first protrusion is located in the second depression, and the second protrusion is located in the first depression.

[0005] Optionally, an angle between a side wall of the first recess and a bottom surface of the first recess is less than 90 degrees, and an angle between a side wall of the second recess and a bottom surface of the second recess is less than 90 degrees.

[0006] Optionally, a depth of the first recess is less than or equal to 1 / 2 of a thickness of the contact layer.

[0007] Optionally, a depth of the first recess is less than or equal to 1 / 3 of the thickness of the contact layer.

[0008] Optionally, the value range of the nanoscale is 0.5nm~20nm.

[0009] Optionally, a doping concentration of a surface of the contact layer facing away from the active layer is greater than a doping concentration of a surface of the contact layer facing the active layer.

[0010] Optionally, the doping concentration of the contact layer increases gradually in a direction from the contact layer away from the active layer.

[0011] Optionally, the contact layer has a thickness of 1 nm to 50 nm.

[0012] The present application also provides a method for preparing a semiconductor light-emitting structure, comprising: forming a stacked first limiting layer, a first waveguide layer, an active layer, a second waveguide layer, and a second limiting layer; forming a contact layer on a surface of the second limiting layer facing away from the active layer, wherein a surface of the contact layer facing away from the active layer has a first nanoscale concave-convex structure, and the first concave-convex structure includes a plurality of first protrusions and a first depression located between the first protrusions; forming a front electrode layer on a surface of the contact layer facing away from the active layer, wherein a surface of the front electrode layer facing the contact layer has a second nanoscale concave-convex structure, and the second concave-convex structure includes a plurality of second protrusions and a second depression located between the second protrusions; wherein the first protrusion is located in the second depression, and the second protrusion is located in the first depression.

[0013] Optionally, a contact layer is formed on a surface of the second restricting layer that is away from the active layer, including: forming an initial contact layer on a surface of the second restricting layer that is away from the active layer; and etching a surface of the initial contact layer that is away from the active layer so that the initial contact layer forms the contact layer.

[0014] Optionally, the etching process includes one of an electron beam etching process and a plasma etching process.

[0015] Optionally, a contact layer is formed on the surface of the second confinement layer facing away from the active layer, including: forming an initial contact layer on the surface of the second confinement layer facing away from the active layer; and introducing a decomposition gas to decompose a local area of ​​the surface of the initial contact layer facing away from the active layer to form the contact layer.

[0016] Optionally, the decomposition gas includes H 2 and NH 3 One or more of .

[0017] Optionally, the initial contact layer is formed in an epitaxial growth process, and the epitaxial growth process includes a heat preservation process and a cooling process after the heat preservation process; during the cooling process, a decomposition gas is introduced.

[0018] The technical solution of this invention has the following technical effects:

[0019] The semiconductor light-emitting structure provided by the technical solution of the present invention has a second nanoscale concave-convex structure on the surface of the front electrode layer facing the contact layer, and the second concave-convex structure includes a plurality of second protrusions and a second depression between the second protrusions; the first protrusion is located in the second depression, and the second protrusion is located in the first depression. That is, the second concave-convex structure and the first concave-convex structure are engaged with each other, which increases the effective contact area, reduces the contact resistance, and improves the adhesion between the front electrode layer and the contact layer, thereby effectively improving the ohmic contact performance, reducing the operating voltage of the semiconductor light-emitting structure, and effectively improving the long-term working stability. Furthermore, the mechanical resistance provided by the "snap-on" engaging structure can prevent the front electrode layer and the contact layer from separating under high stress. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 A schematic diagram of a semiconductor light emitting structure provided by an embodiment of the present invention;

[0022] Figure 2 A schematic diagram of a contact layer in a semiconductor light emitting structure provided by an embodiment of the present invention;

[0023] Figure 3 A schematic diagram of the engagement between a contact layer and a front electrode layer in a semiconductor light emitting structure is provided for another embodiment of the present invention;

[0024] Figure 4 A schematic diagram of a semiconductor light emitting structure provided in another embodiment of the present invention. DETAILED DESCRIPTION

[0025] When LEDs and semiconductor lasers are working, current needs to be injected into the semiconductor laser through the front electrode layer. And only when the current input to the semiconductor laser is large enough to exceed the threshold current, the output optical power will suddenly increase and generate laser. The quality of the ohmic contact formed by the epitaxially grown contact layer and the front electrode layer prepared in the chip process, especially the ohmic contact between the p-type contact layer and the front electrode layer, has a direct impact on the luminous efficiency, operating voltage and long-term reliability of GaN-based LEDs and semiconductor lasers. In the field of LEDs, a GaN or InGaN structure with a step flow morphology, low roughness, and high Mg doping is grown on the epitaxial layer as a p-type contact layer, and its performance meets the working requirements of LEDs. However, compared with LEDs, the operating current density of semiconductor lasers is about 2 orders of magnitude higher, and the Joule heat generated under the same resistance is higher, so the contact resistance and stability of the ohmic contact are required to be higher.

[0026] One hope is to reduce the contact barrier by increasing the Mg doping concentration of the contact layer of the semiconductor laser. However, the study found that when the Mg doping concentration is too high, for example, greater than 4*10 19 atoms / cm 3 , inversion domains are easily formed during the growth process, causing the quality of the semiconductor crystal to deteriorate rapidly.

[0027] The inventors found during the research that the specific contact resistivity of the epitaxial layer is high, greater than 10 -4 When working under high current density, the contact resistance and voltage often increase, which is not conducive to the long-term stable operation of semiconductor lasers. And after aging under certain extreme conditions, the electrode layer and the contact layer separate, indicating that the electrode layer and the contact layer are not tightly or firmly attached.

[0028] To solve the above problems, the technical solution of the present invention provides a semiconductor light-emitting structure, which improves the contact layer of the semiconductor light-emitting structure to improve the performance of ohmic contact, reduce the operating voltage of the semiconductor light-emitting structure, and improve long-term working stability.

[0029] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0031] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can also be the internal connection of two components, it can be a wireless connection, or it can be a wired connection. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0032] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0033] An embodiment of the present invention provides a semiconductor light emitting structure, referring to Figures 1 to 4 ,include:

[0034] A stacked first confinement layer 102a, a first waveguide layer 103a, an active layer 104, a second waveguide layer 103b, a second confinement layer 102b, a contact layer 106 and a front electrode layer 200;

[0035] The surface of the contact layer 106 facing away from the active layer 104 has a first concave-convex structure of nanometer scale, and the first concave-convex structure includes a plurality of first protrusions 1061 (refer to Figure 2 ) and the first recess 1062 (reference Figure 2 );

[0036] The surface of the front electrode layer 200 facing the contact layer 106 has a second concave-convex structure of nanometer scale, wherein the second concave-convex structure includes a plurality of second protrusions and second depressions between the second protrusions;

[0037] The first protrusion 1061 is located in the second recess, and the second protrusion is located in the first recess 1062 .

[0038] In this embodiment, the surface of the front electrode layer 200 facing the contact layer 106 has a second nanoscale concave-convex structure, and the second concave-convex structure includes a plurality of second protrusions and a second depression between the second protrusions; the first protrusion is located in the second depression, and the second protrusion is located in the first depression. That is, the second concave-convex structure and the first concave-convex structure are engaged with each other, which increases the effective contact area, reduces the contact resistance, and improves the adhesion between the front electrode layer 200 and the contact layer 106, thereby effectively improving the ohmic contact performance, reducing the operating voltage of the semiconductor light-emitting structure, and effectively improving the long-term working stability. Furthermore, the mechanical resistance provided by the "snap-on" engaging structure can prevent the front electrode layer 200 and the contact layer 106 from separating under high stress.

[0039] In one embodiment, the angle θ between the sidewall of the first recess 1062 and the bottom of the first recess 1062 is less than 90 degrees, and the angle between the sidewall of the second recess and the bottom of the second recess is less than 90 degrees. In this way, the top width a of the first recess 1062 is smaller than the bottom width b of the first recess 1062, and the width of the second recess close to the active layer 104 is smaller than the width away from the active layer 104, so that the first recess 1062 and the second protrusion are better engaged, and the first protrusion 1061 and the second recess are better engaged, thereby reducing the risk of separation of the contact layer 106 and the front electrode layer 200.

[0040] In one embodiment, the angle θ between the side wall of the first recess 1062 and the bottom surface of the first recess 1062 is less than 87 degrees, such as 85 degrees, 80 degrees or 75 degrees; the angle between the side wall of the second recess and the bottom surface of the second recess is less than 87 degrees, such as 85 degrees, 80 degrees or 75 degrees.

[0041] In one embodiment, the doping concentration of the surface of the contact layer 106 facing away from the active layer 104 is greater than the doping concentration of the surface of the contact layer 106 facing the active layer 104. The doping concentration of the surface of the contact layer 106 facing away from the active layer 104 and the vicinity is higher, which is used to ensure a lower contact barrier with the front electrode layer 200. The doping concentration of the surface of the contact layer 106 facing the active layer 104 is lower, so that the material quality of the surface of the contact layer 106 facing the active layer 104 and the vicinity is higher.

[0042] In one embodiment, the doping concentration of the contact layer 106 increases gradually along a direction from the contact layer away from the active layer.

[0043] In one embodiment, the doping ions in the contact layer 106 include Mg ions.

[0044] In one embodiment, the doping concentration of the contact layer 106 is 1*10 18 atoms / cm 3 ~5*10 21 atoms / cm 3 , for example 1*10 18 atoms / cm 3 , 1*10 19 atoms / cm 3 , 3*10 19 atoms / cm 3 , 4*10 19 atoms / cm 3 , 5*10 20 atoms / cm 3 or 5*10 21 atoms / cm 3 .

[0045] In one embodiment, the doping concentration of the contact layer 106 is 3*10 18 atoms / cm 3 ~2*10 21 atoms / cm 3 .

[0046] In one embodiment, the depth of the first recess 1062 is less than or equal to 1 / 2 of the thickness of the contact layer 106. Because the doping concentration of the contact layer 106 decreases from the side away from the active layer 104 to the side facing the active layer 104, if the depth of the first recess 1062 is too deep, the doping concentration of the contact layer 106 at the bottom of the first recess 1062 is not high enough, and the degree of reducing the potential barrier between the contact layer 106 and the front electrode layer 200 is small; on the other hand, when the depth of the first recess 1062 is too deep, it is difficult for the prepared front electrode layer 200 to penetrate into the bottom of the first recess 1062, so the contact area between the front electrode layer 200 and the contact layer 106 at the bottom of the first recess 1062 is affected. If the depth of the first recess 1062 is too small, the first concave-convex structure is too flat, the degree of increasing the contact area is small, and the degree of improving the bite bonding force between the front electrode layer and the contact layer is small.

[0047] In one embodiment, the depth of the first recess 1062 is less than or equal to 1 / 3 of the thickness of the contact layer 106 . For example, the depth of the first recess 1062 is 1 / 4 of the thickness of the contact layer 106 .

[0048] In one embodiment, the value range of the nanometer scale is 0.5 nm to 20 nm. Preferably, the value range of the nanometer scale is 1 nm to 10 nm.

[0049] The first confinement layer 102a, the first waveguide layer 103a, the active layer 104, the second waveguide layer 103b, the second confinement layer 102b, the contact layer 106, and the front electrode layer 200 have a stacking direction.

[0050] It should be noted that the first concave-convex structure of nanometer scale means that: the first protrusion 1061 is of nanometer scale, and the first depression 1062 is of nanometer scale. The first protrusion 1061 is of nanometer scale, in other words, the size of the first protrusion 1061 in any direction is of nanometer scale, the size of the first protrusion 1061 in the stacking direction is of nanometer scale, and the size of the first protrusion 1061 in any direction perpendicular to the stacking direction is of nanometer scale. The first depression 1062 is of nanometer scale, in other words, the size of the first depression 1062 in any direction is of nanometer scale, the size of the first depression 1062 in the stacking direction is of nanometer scale, and the size of the first depression 1062 in any direction perpendicular to the stacking direction is of nanometer scale.

[0051] It should be noted that the second concave-convex structure of nanometer scale means that the second protrusion is of nanometer scale and the second depression is of nanometer scale. The second protrusion is of nanometer scale, in other words, the size of the second protrusion in any direction is of nanometer scale, the size of the second protrusion in the stacking direction is of nanometer scale, and the size of the second protrusion in any direction perpendicular to the stacking direction is of nanometer scale. The second depression is of nanometer scale, in other words, the size of the second depression in any direction is of nanometer scale, the size of the second depression in the stacking direction is of nanometer scale, and the size of the second depression in any direction perpendicular to the stacking direction is of nanometer scale.

[0052] In one embodiment, the contact layer 106 has a thickness of 1 nm to 50 nm.

[0053] In one embodiment, the contact layer 106 has a thickness of 3 nm to 30 nm.

[0054] The conductivity type of the first confinement layer 102a is opposite to the conductivity type of the second confinement layer 102b.

[0055] In one embodiment, the conductivity type of the first confinement layer 102a is n-type, and the conductivity type of the second confinement layer 102b is p-type.

[0056] The conductivity type of the first waveguide layer 103 a and the conductivity type of the second waveguide layer 103 b are opposite to each other.

[0057] In one embodiment, the conductivity type of the first waveguide layer 103 a is n-type, and the conductivity type of the second waveguide layer 103 b is p-type.

[0058] The n-type doping concentration in the first waveguide layer 103 a and the first confinement layer 102 a includes Si ions.

[0059] In one embodiment, the conductivity type of the second confinement layer 102b is p-type, the conductivity type of the contact layer 106 is p-type, the doping ions in the contact layer 106 are acceptor doping ions, the second confinement layer 102b has acceptor doping ions, and the concentration of the acceptor doping ions in the contact layer 106 is greater than the concentration of the acceptor doping ions in the second confinement layer 102b. The acceptor doping ions include Mg ions.

[0060] In one embodiment, the semiconductor light emitting structure further includes: a first carrier blocking layer 105, located between the second waveguide layer 103b and the second confinement layer 102b. When the conductivity type of the second waveguide layer 103b and the second confinement layer 102b is p-type, the first carrier blocking layer 105 contains acceptor doping ions, and the first carrier blocking layer 105 is an electron blocking layer.

[0061] The relative positions of the first carrier blocking layer 105 and the second confinement layer 102b are not restricted. The first carrier blocking layer 105 may be between the second confinement layer 102b and the active layer 104, inside the second confinement layer 102b, or between the second confinement layer 102b and the contact layer.

[0062] The bandgap width of the first carrier blocking layer 105 is greater than the bandgap width of the second waveguide layer 103 b .

[0063] In one embodiment, the doping concentration of the first carrier blocking layer 105 is 1*10 18 atom / cm 3 ~2*10 20 atom / cm 3 The material of the first carrier blocking layer 105 is Al x7 In y7 Ga 1-x7-y7 N. The first carrier blocking layer 105 is a single-layer structure or a multi-layer structure. When the first carrier blocking layer 105 is a multi-layer structure, Al x7 In y7 Ga 1-x7-y7 The value of x7 in the N layer is: 0.07≤x7≤0.3, Al x7 In y7 Ga 1-x7-y7 The value of y7 in layer N is: 0≤y7≤0.1.

[0064] In one embodiment, the doping concentration of the first carrier blocking layer 105 is 1*10 18 atom / cm 3~2*10 20 atom / cm 3 .

[0065] In one embodiment, reference Figure 4 The second confinement layer 102b includes a first upper confinement layer 102b1 and a second upper confinement layer 102b2, and the second upper confinement layer 102b2 is located on a surface of the first upper confinement layer 102b1 away from the active layer 104. The refractive index of the second upper confinement layer 102b2 is smaller than the refractive index of the first upper confinement layer 102b1.

[0066] In one embodiment, the material of the first upper confinement layer 102b1 includes p-type Al x41 Ga 1-x41 N, the material of the second upper confinement layer 102b2 includes p-type Al x42 Ga 1-x42 N, wherein x42 is greater than x41. In a specific embodiment, x41 is 0.01-0.15, such as 0.05, and x42 is 0.02-0.2, such as 0.08.

[0067] In one embodiment, the doping concentration of the second upper confinement layer 102b2 is greater than the doping concentration of the first upper confinement layer 102b1, and the effects include: the series resistance of the second upper confinement layer 102b2 and the contact layer 106 is reduced. The first upper confinement layer 102b1 is closer to the active layer 104 than the second upper confinement layer 102b2, and closer to the center of the light field. The doping concentration of the first upper confinement layer 102b1 is lower, which reduces the impurity absorption coefficient and thus reduces the light loss; the second upper confinement layer 102b2 is far away from the center of the light field, and the internal light field of the second upper confinement layer 102b is weak. Even if the absorption coefficient increases, its total absorption loss is relatively small. Therefore, the doping concentration of the second upper confinement layer 102b can be increased to reduce the series resistance to achieve a lower working voltage.

[0068] In other embodiments, the second confinement layer 102b is a single-layer structure, and the material of the second confinement layer 102b is p-type Al x4 Ga 1-x4 N, x4 is 0.02~0.5, for example 0.07.

[0069] In one embodiment, the material of the second confinement layer 102b is p-type Al x43 In y43 Ga 1-x43-y43 N. In a specific embodiment, x43 is greater than 0.02, and y43 is greater than 0. The second restriction layer 102b is a single-layer structure or a multi-layer structure. In an embodiment, when the second restriction layer 102b is a multi-layer structure, the multi-layer Al x43 In y43 Ga1-x43-y43 N has x43≥0.02, and the multilayer Al x43 In y43 Ga 1-x43-y43 The x43 in N increases layer by layer. In one embodiment, the refractive index in the second confinement layer 102 b of the multi-layer structure decreases layer by layer in a direction away from the active layer 104 .

[0070] At the same time, the changes of x43 and y43 must also meet the requirements of maintaining multilayer Al x43 In y43 Ga 1-x43-y43 The band gap of N is not lower than the band gap of the second waveguide layer.

[0071] In one embodiment, the second confinement layer 102b is Al a1 In b1 Ga 1-a1-b1 N / A a2 In b2 Ga 1-a2-b2 N superlattice structure, that is, Al a1 In b1 Ga 1-a1-b1 N and Al a2 In b2 Ga 1-a2-b2 N alternately stacked superlattice structure.

[0072] In one embodiment, reference Figure 4 The second waveguide layer 103b includes a first upper waveguide layer 103b1 and a second upper waveguide layer 103b2, wherein the second upper waveguide layer 103b2 is located on a surface of the first upper waveguide layer 103b1 that is away from the active layer 104, and the refractive index of the second upper waveguide layer 103b2 is less than the refractive index of the first upper waveguide layer 103b1. The provision of the second upper waveguide layer 103b2 can improve the growth quality of the second confinement layer 102b and reduce the stress of the second confinement layer 102b.

[0073] In one embodiment, the material of the second upper waveguide layer 103b2 is p-type GaN or undoped GaN, and the material of the first upper waveguide layer 103b1 is p-type In x3 Ga 1-x3 N. In one embodiment, x3 is 0.01-0.15, for example, 0.05.

[0074] In one embodiment, the doping concentration of the second upper waveguide layer 103b2 is greater than the doping concentration of the first upper waveguide layer 103b1. In one embodiment, the first upper waveguide layer 103b1 is not doped with conductive ions to reduce impurity absorption loss. In one embodiment, the first upper waveguide layer 103b1 is doped with conductive ions, and the concentration of conductive ions in the first upper waveguide layer 103b1 is less than the concentration of conductive ions in the second confinement layer 102b.

[0075] In one embodiment, the second waveguide layer 103b is a single-layer structure. For example, the material of the second waveguide layer 103b is p-type In x3 Ga 1-x3 In one embodiment, the second waveguide layer 103b is not doped with conductive ions to reduce impurity absorption loss. For example, the material of the second waveguide layer 103b is non-doped In x3 Ga 1-x3 N. In one embodiment, the second waveguide layer 103b is doped with conductive ions, and the concentration of the conductive ions in the second waveguide layer 103b is lower than the concentration of the conductive ions in the second confinement layer 102b.

[0076] In one embodiment, the material of the second waveguide layer 103b is Al x33 In y33 Ga 1-x33-y33 N, in a specific embodiment, x33 is greater than 0 and less than or equal to 0.1, and y33 is greater than 0 and less than or equal to 0.15. In one embodiment, the second waveguide layer 103b is a single-layer structure or a multi-layer structure. In one embodiment, when the second waveguide layer 103b is a multi-layer structure, the multi-layer Al x33 In y33 Ga 1-x33-y33 The x33 in N increases layer by layer. In one embodiment, the refractive index in the second waveguide layer 103b of the multilayer structure decreases layer by layer in a direction away from the active region. In one embodiment, the second waveguide layer 103b is not doped with conductive ions to reduce absorption loss.

[0077] In a specific embodiment, the first confinement layer 102a includes a first lower confinement layer 102a1 and a second lower confinement layer 102a2, wherein the second lower confinement layer 102a2 is located between the first lower confinement layer 102a1 and the first waveguide layer 103a. The refractive index of the first lower confinement layer 102a1 is smaller than that of the second lower confinement layer 102a2.

[0078] In one embodiment, the material of the first lower confinement layer 102a1 includes n-type Al x11 Ga 1-x11 N, the material of the second lower confinement layer 102a2 includes n-type Al x12 Ga1-x12 N, wherein x12 is greater than x11. In a specific embodiment, x11 is greater than 0 and less than or equal to 0.2, such as 0.03, and x12 is 0.02-0.3, such as 0.08.

[0079] In one embodiment, the doping concentration of the second lower confinement layer 102 a 2 is greater than the doping concentration of the first lower confinement layer 102 a 1 , which has the following functions: reducing the series resistance of the device and increasing the carriers of the active layer 104 .

[0080] In other embodiments, the first confinement layer 102a is a single-layer structure, and the material of the first confinement layer 102a is n-type Al x1 Ga 1-x1 N, in one embodiment, x1 is 0.02-0.3, for example 0.07.

[0081] In other embodiments, the material of the first confinement layer 102a is n-type Al x6 In y6 Ga 1-x6-y6 N, the first restriction layer 102a is a single layer or a multi-layer structure. When the first restriction layer 102a is a multi-layer structure, the multi-layer Al x6 In y6 Ga 1-x6-y6 In N, x6 is greater than 0, and multilayer Al x6 In y6 Ga 1-x6-y6 In N, y6 is greater than 0. In one embodiment, the doping concentration of the first confinement layer 102a is 1*10 18 atoms / cm 3 ~7*10 18 atoms / cm 3 In a specific embodiment, x6 is greater than 0, and y6 is greater than 0 and less than or equal to 0.3.

[0082] In a specific embodiment, the first waveguide layer 103a includes a first lower waveguide layer 103a1 and a second lower waveguide layer 103a2, wherein the second lower waveguide layer 103a2 is located between the first lower waveguide layer 103a1 and the active layer 104, and the refractive index of the second lower waveguide layer 103a2 is greater than the refractive index of the first lower waveguide layer 103a1. The provision of the first lower waveguide layer 103a1 can improve the growth quality of the second lower waveguide layer and reduce the stress of the second lower waveguide layer 103a2.

[0083] In one embodiment, the material of the first lower waveguide layer is n-type GaN, and the material of the second lower waveguide layer is n-type In x2 Ga 1-x2 N. In one embodiment, x2 is 0.01-0.15, for example, 0.05.

[0084] In one embodiment, the first waveguide layer 103a is a single-layer structure, for example, the material of the lower waveguide layer is n-type In x2 Ga 1-x2 In one embodiment, the first waveguide layer 103a is not doped with conductive ions to reduce impurity absorption loss. In one embodiment, the first waveguide layer 103a is doped with conductive ions. In one embodiment, the doping concentration of the first waveguide layer 103a is 5*10 17 atoms / cm 3 ~1*10 19 atoms / cm 3 .

[0085] In one embodiment, the material of the first waveguide layer 103a is n-type Al s1 In t1 Ga 1-s1-t1 In one embodiment, s1 is greater than 0, and t1 is less than or equal to 0.3. The first waveguide layer 103a is a multi-layer structure or a single-layer structure. When the first waveguide layer 103a is a multi-layer structure, the multi-layer Al s1 In t1 Ga 1-s1-t1 In N, s1 decreases layer by layer, and the multilayer Al s1 In t1 Ga 1-s1-t1 In N, t1 increases layer by layer.

[0086] At the same time, Al s1 In t1 Ga 1-s1-t1 The band gap of N is larger than the band gap of the quantum well in the active layer.

[0087] In one embodiment, the acceptor dopant ions include Mg ions.

[0088] In one embodiment, the active layer is a plurality of pairs of quantum barriers 104b and quantum wells 104a.

[0089] In one embodiment, the material of the quantum well includes In x5 Ga 1-x5 N, the material of the quantum barrier includes GaN.

[0090] In one embodiment, the thickness of the quantum well is 3 nm, and the thickness of the quantum barrier is 6 nm.

[0091] In this application, there is no restriction on the material of the active layer, and there is no restriction on the thickness of the quantum well and quantum barrier.

[0092] In one embodiment, the material of the contact layer 106 is p-type Inx91 Ga 1-x91 N, p-type Al x92 In y92 Ga 1-x92-y92 N, p-type GaN layer. In one embodiment, the contact layer 106 is a p-type GaN / InGaN composite layer.

[0093] In one embodiment, 0≤x91≤0.3. In one embodiment, 0≤x92≤0.1, 0≤y92≤0.3.

[0094] In one embodiment, the root mean square roughness of the surface of the contact layer 106 facing the front electrode layer 200 is between 0.3nm and 2nm, for example, 0.55nm. If the surface roughness of the contact layer 106 is too low, for example, <0.3nm, that is, when the surface of the contact layer 106 is very flat, it is difficult for the contact layer 106 and the front electrode layer 200 to form a close contact with a bite structure. If the surface roughness of the contact layer 106 is too high, for example, >2nm, the first concave of the first concave-convex structure may be too deep, and it is difficult for the front electrode layer to penetrate into the first concave.

[0095] In one embodiment, the front electrode layer 200 is a metal electrode layer, such as Ti, Pt, Au, Ni, Co, Pb, Ag or Cu. In one embodiment, the front electrode layer 200 is a transparent oxide conductive layer, such as indium tin oxide (ITO), fluorine-doped tin oxide (FTO), AZO (aluminum-doped zinc oxide), SnO2:Sb, CdIn 2 O 4 、Cd 2 SnO 4 、ZnSnO 3 、Zn 2 SnO 4 MgIn 2 O 4 、Zn 2 In 2 O 5 、GaInO 3 or In 4 Sn 3 O 12 .

[0096] In one embodiment, the semiconductor light emitting structure further includes: a substrate layer located on a side of the first confinement layer away from the active layer.

[0097] In one embodiment, the semiconductor light emitting structure further includes: a current spreading layer 101, wherein the current spreading layer 101 is located between the substrate layer and the first confinement layer and contacts the first confinement layer.

[0098] In one embodiment, the current spreading layer 101 is one of n-type doped AlGaN, GaN and SiC.

[0099] In one embodiment, the first limiting layer, the first waveguide layer, the active layer, the second waveguide layer and the second limiting layer are located on a side of the partial current spreading layer 101 away from the substrate layer, and the semiconductor light emitting structure further includes: a second electrode, which is located on a surface of a side of the partial current spreading layer 101 away from the substrate layer and is spaced apart from the first limiting layer.

[0100] In one embodiment, the semiconductor light emitting structure has a front cavity surface and a rear cavity surface that are arranged opposite to each other; the semiconductor light emitting structure further includes: an anti-reflection film located on the front cavity surface, and a reflective film located on the rear cavity surface.

[0101] In one embodiment, the semiconductor light emitting structure is an edge emitting semiconductor laser.

[0102]

[0103] It can be seen from the results that the solution provided by the present invention can effectively improve the ohmic contact characteristics of the semiconductor light-emitting structure, reduce the specific contact resistivity, reduce the operating voltage, and reduce the Joule heat of the semiconductor light-emitting structure during operation.

[0104] Another embodiment of the present invention also provides a method for preparing a semiconductor light-emitting structure, comprising: forming a stacked first restriction layer, a first waveguide layer, an active layer, a second waveguide layer, and a second restriction layer; forming a contact layer on a surface of the second restriction layer facing away from the active layer, wherein a surface of the contact layer facing away from the active layer has a first nanoscale concave-convex structure, and the first concave-convex structure includes a plurality of first protrusions and a first depression between the first protrusions; forming a front electrode layer on a surface of the contact layer facing away from the active layer, wherein a surface of the front electrode layer facing the contact layer has a second nanoscale concave-convex structure, and the second concave-convex structure includes a plurality of second protrusions and a second depression between the second protrusions; wherein the first protrusion is located in the second depression, and the second protrusion is located in the first depression.

[0105] In one embodiment, a contact layer is formed on a surface of the second restricting layer facing away from the active layer, comprising: forming an initial contact layer on a surface of the second restricting layer facing away from the active layer; and etching the surface of the initial contact layer facing away from the active layer so that the initial contact layer forms the contact layer; preferably, the etching process comprises one of electron beam etching process and plasma etching process.

[0106] In one embodiment, forming a contact layer on a surface of the second confining layer away from the active layer comprises: forming an initial contact layer on a surface of the second confining layer away from the active layer; and introducing a decomposition gas to decompose a local area of ​​the surface of the initial contact layer away from the active layer to form the contact layer. Preferably, the decomposition gas comprises H 2 and NH 3 One or more of. Preferably, the initial contact layer is formed in an epitaxial growth process, and the epitaxial growth process includes a heat preservation process and a cooling process after the heat preservation process; during the cooling process, a decomposition gas is introduced. The epitaxial growth process includes a heating process, a heat preservation process and a cooling process performed in sequence. The growth of the initial contact layer is performed during the heat preservation process.

[0107] The process of forming the initial contact layer on the surface of the second confinement layer facing away from the active layer includes an epitaxial growth process, such as an MOCVD process.

[0108] In one embodiment, forming a stacked first confinement layer, a first waveguide layer, an active layer, a second waveguide layer, and a second confinement layer includes forming a stacked first confinement layer, a first waveguide layer, an active layer, a second waveguide layer, and a second confinement layer on one side of a substrate layer.

[0109] In one embodiment, the method for preparing the semiconductor light emitting structure further includes: providing a current spreading layer between the substrate layer and the first confinement layer.

[0110] In one embodiment, the process of forming the stacked first confinement layer, the first waveguide layer, the active layer, the second waveguide layer, and the second confinement layer includes an epitaxial growth process, such as a metal organic compound chemical vapor deposition process.

[0111] In one embodiment, after the contact layer is formed, an annealing process is performed, and the parameters of the annealing process include: an annealing time of 10s to 120min, such as 30min, and an annealing temperature of 300°C to 800°C, such as 550°C. The annealing process uses a rapid annealing furnace or a tubular annealing furnace.

[0112] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A semiconductor light emitting structure, characterized in that: include: A first confinement layer, a first waveguide layer, an active layer, a second waveguide layer, a second confinement layer, a contact layer and a front electrode layer stacked in sequence; A surface of the contact layer on one side facing away from the active layer has a first concave-convex structure of nanometer scale, wherein the first concave-convex structure includes a plurality of first protrusions of nanometer scale and first depressions of nanometer scale located between the first protrusions; A surface of the front electrode layer facing the contact layer has a second concave-convex structure of nanometer scale, wherein the second concave-convex structure includes a plurality of second protrusions of nanometer scale and second depressions of nanometer scale located between the second protrusions; Wherein, the first protrusion is located in the second depression, and the second protrusion is located in the first depression; The included angle between the side wall of the first recess and the bottom surface of the first recess is less than 87 degrees, and the included angle between the side wall of the second recess and the bottom surface of the second recess is less than 87 degrees; The numerical range of the nanoscale is 0.5nm~20nm.

2. The semiconductor light emitting structure according to claim 1, characterized in that: The depth of the first recess is less than or equal to 1 / 2 of the thickness of the contact layer.

3. The semiconductor light emitting structure according to claim 2, characterized in that: The depth of the first recess is less than or equal to 1 / 3 of the thickness of the contact layer.

4. The semiconductor light emitting structure according to claim 1, characterized in that: The doping concentration of a surface of the contact layer facing away from the active layer is greater than the doping concentration of a surface of the contact layer facing the active layer.

5. The semiconductor light emitting structure according to claim 4, characterized in that: The doping concentration of the contact layer increases gradually along a direction in which the contact layer is away from the active layer.

6. The semiconductor light emitting structure according to claim 1, characterized in that: The thickness of the contact layer is 1 nm to 50 nm.

7. A method for preparing a semiconductor light-emitting structure, characterized in that: include: forming a first confinement layer, a first waveguide layer, an active layer, a second waveguide layer, and a second confinement layer stacked in sequence; A contact layer is formed on a surface of the second restriction layer on a side away from the active layer, wherein the surface of the contact layer on a side away from the active layer has a first concave-convex structure of nanometer scale, wherein the first concave-convex structure includes a plurality of first protrusions of nanometer scale and first depressions of nanometer scale located between the first protrusions; A front electrode layer is formed on a surface of the contact layer facing away from the active layer, and a surface of the front electrode layer facing the contact layer has a second concave-convex structure of nanometer scale, wherein the second concave-convex structure includes a plurality of second protrusions of nanometer scale and second depressions of nanometer scale located between the second protrusions; wherein the first protrusion is located in the second depression, and the second protrusion is located in the first depression; The included angle between the side wall of the first recess and the bottom surface of the first recess is less than 87 degrees, and the included angle between the side wall of the second recess and the bottom surface of the second recess is less than 87 degrees; The numerical range of the nanoscale is 0.5nm~20nm.

8. The method for preparing a semiconductor light emitting structure according to claim 7, characterized in that: A contact layer is formed on a surface of the second confinement layer facing away from the active layer, comprising: forming an initial contact layer on a surface of the second confinement layer facing away from the active layer; and The surface of the initial contact layer facing away from the active layer is etched to form the contact layer from the initial contact layer.

9. The method for preparing a semiconductor light emitting structure according to claim 8, characterized in that: The etching process includes one of an electron beam etching process and a plasma etching process.

10. The method for preparing a semiconductor light emitting structure according to claim 7, characterized in that: A contact layer is formed on a surface of the second confinement layer facing away from the active layer, comprising: forming an initial contact layer on a surface of the second confinement layer facing away from the active layer; and A decomposition gas is introduced to decompose a local area of ​​the surface of the initial contact layer facing away from the active layer to form the contact layer.

11. The method for preparing a semiconductor light emitting structure according to claim 10, characterized in that: The decomposition gas includes one or more of H2 and NH3.

12. The method for preparing a semiconductor light emitting structure according to claim 10, characterized in that: The initial contact layer is formed in an epitaxial growth process, which includes a heat preservation process and a cooling process after the heat preservation process; during the cooling process, decomposition gas is introduced.