Denim composite fabric and preparation method thereof
The denim fabric is processed through mechanical polishing and alkali washing processes, and combined with nano-membrane and knitted lining, which solves the problem of delamination and bubbling of denim composite fabric during the washing process, and achieves a three-layer structure with high elasticity and breathability. Composite fabrics enhance market competitiveness.
Patent Information
- Application Number
- CN202410581335.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-05-11
AI Technical Summary
The existing three-layer denim composite fabric is prone to delamination and blistering during the washing process, making it difficult to meet the needs of being lightweight, warm and breathable.
Mechanical grinding process is used to control the fiber height of the denim fabric to less than 3mm, and impurities are removed through an alkali washing process. It is combined with the composite process of nano-membrane and knitted lining to form a three-layer composite fabric, using low glue content composite technology and SURFORCE nano membrane to improve the elasticity and breathability of the fabric.
It significantly reduces the probability of fabric delamination and blistering, improves market competitiveness, achieves the comprehensive effect of high elasticity, warmth and breathability, and is adaptable to a variety of washing processes.
Smart Images

Figure CN118322680B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of high-performance fibers and products and composite materials in the new material industry, and in particular to a denim composite fabric and a preparation method thereof. Background Art
[0002] As the market demand for functional fabrics grows, composite fabrics are favored due to their simple structure and outstanding functions. However, existing three-layer denim composite fabrics are prone to stratification and blistering during washing, while double-layer composite fabrics are difficult to meet the requirements of lightness, warmth and breathability.
[0003] In the process of realizing the present invention, the applicant discovered that traditional denim composite fabrics are prone to delamination and blistering during the washing process, which seriously affects the appearance and wearing experience of the clothing. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] The present invention is expected to at least partially solve one of the above technical problems.
[0006] (II) Technical solution
[0007] The first aspect of the present invention provides a denim composite fabric, comprising: a denim face fabric; a nano-membrane composited on the denim face fabric; and a knitted lining composited on the nano-membrane; wherein the fiber height of the denim face fabric facing the nano-membrane side is not higher than 3 mm.
[0008] The second aspect of the present invention provides a method for preparing a denim composite fabric, comprising: step A, obtaining a denim surface cloth, including: a mechanical polishing process, mechanically polishing the surface of the denim surface cloth to be composited with a nanofilm, wherein the polished fiber height is not higher than 3 mm; an alkali washing process, alkali washing the denim surface cloth in an alkali washing solution; a cleaning process, washing the denim surface cloth after alkali washing with clean water; step B, composite the nanofilm on the denim surface cloth; and step C, composite the knitted lining on the nanofilm.
[0009] A third aspect of the present invention provides a denim composite fabric, which is prepared by the above preparation method.
[0010] (III) Beneficial effects
[0011] It can be seen from the above technical solution that the present invention has at least one of the following beneficial effects compared with the prior art:
[0012] (1) The denim composite fabric of the present invention comprises a three-layer composite structure, which combines the durability of the denim fabric, the warmth and breathability of the nano-membrane, and the comfort, warmth and breathability of the knitted lining, and in particular greatly reduces the probability of fabric delamination and blistering, thereby improving the market competitiveness of the denim fabric.
[0013] (2) The specific surface area of denim fabric is significantly increased through mechanical grinding process, and impurities of denim fabric are removed through alkali washing process. The weight range of 140-165gsm can ensure the elasticity level of this specification fabric and provide synergy for high fastness. With the composite process, it provides a basis for the high fastness of denim fabric and nano film composite. At the same time, the original elasticity of the fabric is also maintained through low glue compounding.
[0014] (3) The three-layer composite fabric used in the present invention is processed by fabric treatment before lamination and low-glue lamination, and is used in combination with the SURFORCE nanofilm to utilize its high elasticity to ultimately achieve high elasticity of the entire composite fabric. At the same time, it also has excellent warmth retention, weft elasticity and breathability. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Schematic diagram of a denim composite fabric according to an embodiment of the present invention.
[0016] Figure 2 The present invention is a flow chart of a method for preparing a denim composite fabric according to an embodiment of the present invention. DETAILED DESCRIPTION
[0017] The present invention composites denim surface fabric with nano-membrane and knitted lining to develop a highly elastic and lightweight denim fabric, which still has an excellent fastness level after washing, greatly reduces the probability of delamination and blistering, has wide adaptability, and can adapt to most washing processes.
[0018] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods and with reference to the accompanying drawings.
[0019] A first aspect of the present invention provides a denim composite fabric. Figure 1 Schematic diagram of a denim composite fabric according to an embodiment of the present invention. As shown in the figure, the denim composite fabric according to this embodiment includes:
[0020] Denim fabric 10;
[0021] Nano film 20, compounded on denim fabric;
[0022] Knitted lining 30, compounded on the nano film;
[0023] Wherein, the fiber height of the denim fabric facing the nano-membrane side is not higher than 3 mm.
[0024] In this embodiment, the nanofilm is compounded on the denim fabric by polyurethane hot melt adhesive 11, and the range of the amount of polyurethane hot melt adhesive is: 5±0.5g / m 2 The knitted lining is compounded on the nano film by polyurethane hot melt adhesive 21, and the range of polyurethane hot melt adhesive is: 3±0.5g / m 2 .
[0025] Those skilled in the art should understand that, in addition to polyurethane materials, other composite adhesive materials may be used to achieve the composite between the two layers of fabrics, which can also implement the present invention and is also within the protection scope of the present invention.
[0026] In this embodiment, the side of the knitted lining that is not facing the nano-membrane is subjected to a raising treatment, and the length of the fibers on the raising surface after the treatment is between 4 and 10 mm, and the heat preservation rate of the lining reaches more than 20%.
[0027] In this embodiment, the denim surface fabric has a gram weight between 140 and 165 gsm and a weft elasticity greater than 40%. The nano-membrane has a fiber diameter of 0.1-2 um, a gram weight range of 5-30 gsm, a membrane elasticity range of 200 ± 30%, and an air permeability range of 1-100 mm / s. The knitted lining has a gram weight range of 110 ± 5 gsm and a horizontal and vertical elasticity range of 50 ± 5%.
[0028] At present, there is a great demand for lightweight, warm, breathable and highly elastic denim composite fabrics in the textile market. In the present invention, the denim composite fabric including a three-layer composite structure combines the durability of the denim fabric, the warmth and breathability of the nano film, and the comfort, warmth and breathability of the knitted lining, especially greatly reduces the probability of fabric delamination and blistering, and improves the market competitiveness of the denim fabric.
[0029] A second aspect of the present invention provides a method for preparing a denim composite fabric. Figure 2 The flowchart of the method for preparing the denim composite fabric according to the embodiment of the present invention is shown in the figure. As shown in the figure, the method for preparing the denim composite fabric according to the embodiment of the present invention comprises:
[0030] Step A, obtaining a denim fabric, comprises:
[0031] Mechanical grinding process: the denim surface to be compounded with the nanofilm is mechanically polished, and the polished fiber height is no more than 3mm;
[0032] Alkaline washing process, the denim fabric is washed in an alkaline washing solution;
[0033] The cleaning process is to wash the denim fabric after mechanical polishing with clean water;
[0034] Step B, compounding the nanofilm on the denim fabric;
[0035] Step C, compounding the knitted lining onto the nano-membrane.
[0036] The denim composite fabric of this embodiment has a three-layer structure, the surface layer is denim fabric, the middle layer is nanofilm (SURFORCE nanofilm produced by Lianrunxiang (Qingdao) Textile Technology Co., Ltd., electrospinning film, TPU or PU material), the inner layer is knitted fabric, composite bonding is performed by reactive polyurethane hot melt adhesive, and new fabric processing and composite processes are used according to fabric characteristics. These process steps work together to improve the composite fastness performance of the fabric, reduce the probability of fabric delamination and blistering, and improve the market competitiveness of denim fabric.
[0037] The following is a detailed description of each step of the method for preparing the denim composite fabric of this embodiment.
[0038] In this embodiment, the weight of the denim surface fabric is between 140 and 165 gsm, and its weft elasticity is greater than 40%. More specifically, the specifications of the denim surface fabric are: CM40*P100D (SP40D)*150*75, 3 / 1 right twill, woven from 74% cotton, 23% polyester, and 3% spandex fibers; wherein the F number of the P100D filament is 288.
[0039] After the denim surface fabric is woven, it needs to go through the "mechanical polishing (reverse side) process → alkali washing process → cleaning process" process for the subsequent lamination process.
[0040] 1. Mechanical grinding process
[0041] The specific process of mechanical grinding process is: vehicle speed: 15±2m / min, rotation speed 80±10 rpm, large cylinder speed 60±5 rpm, tension 3.5±0.5kg.
[0042] In the present invention, the mechanical grinding process not only increases the specific surface area of the denim fabric, but also maintains the integrity of the fiber. After mechanical grinding, the specific surface area increases by more than 8 times, providing a basis for high composite fastness.
[0043] 2. Alkaline washing process
[0044] In this embodiment, the alkali washing process uses caustic soda to remove impurities, and the medium concentration of caustic soda has a reduction effect on short fluff and floating hair. The specific process of the effective alkali washing process is to place the denim surface in the caustic soda cleaning solution: caustic soda content: 5±1g / L, the penetrant is a fatty alcohol polyoxyethylene ether component, and its content is: 1±0.5g / L, the water temperature is 60℃, the washing time is 40min, and the equipment is Circular Model CF, Nisaka (China) Textile Technology Co., Ltd.
[0045] In the present invention, the denim surface fabric can be washed with alkali to remove impurities from the denim surface fabric and reduce the polyester short fluff, which plays an important role in removing floating hair and can significantly improve the composite fastness.
[0046] 3. Cleaning process
[0047] In this embodiment, the specific process of the cleaning process is: cleaning time, 5 to 30 minutes; water temperature gradient: 95°C ± 2, 65°C ± 2, 40°C ± 2, room temperature water.
[0048] Among them, the selected weft yarn P100D / 288F has excellent strength and wear resistance. The specific surface area of the denim fabric is significantly increased through mechanical grinding, and impurities in the denim surface fabric are removed through alkali washing. The weight range of 140-165gsm can ensure the elasticity level of this specification fabric and provide synergy for high fastness. With the composite process, it provides a basis for the high fastness of the composite of denim surface fabric and nano film. At the same time, the original elasticity of the fabric is also retained through low glue compounding.
[0049] Those skilled in the art should understand that the above process parameters are only examples, and those skilled in the art can adjust the process according to actual needs. For example, in the alkaline washing process, the water temperature can be between 70°C and 90°C, the washing time can be between 30 and 60 minutes, and the alkaline substance in the cleaning liquid can also be other alkaline substances besides caustic soda.
[0050] In this embodiment, the nanomembrane is an electrospun nanomembrane made of TPU material. Specifically, a SURFORCE nanomembrane (Lianrunxiang (Qingdao) Textile Technology Co., Ltd.) is used, with a fiber diameter of 0.1-2um, a gram weight range of 5-30gsm, a membrane elasticity range of 200±30%, and an air permeability range of 1-100mm / s.
[0051] Those skilled in the art should understand that the above nanomembranes are only examples. Those skilled in the art can also use nanomembranes of other materials, types, and parameter specifications. For example, the electrostatic textile nanomembrane made of PU material produced by Lianrunxiang (Qingdao) Textile Technology Co., Ltd., although the effect is not as good as the SURFORCE nanomembrane made of TPU material in this embodiment, it can also partially realize the present invention and is also within the scope of protection of the present invention.
[0052] It should be noted that the nanofilm in this embodiment has a specific weight and thickness. This material selection and structural design ensures the elasticity and air permeability of the nanofilm and has excellent anti-fatigue ability.
[0053] In this embodiment, the knitted lining has a gram weight range of 110±5gsm, and its horizontal and vertical elasticity range is 50±5%. Specifically, the knitted lining has a structure specification of AR 40S+P75D / 144F+PU 20D, jersey, horizontal and vertical elasticity of 50±5%, and a gram weight of 110±5gsm. More specifically, the knitted lining is woven from 45% acrylic, 30% viscose, 20% polyester, and 5% spandex, wherein the F number of the P75D filament is 144 or 216. The selected specifications match the surface material specifications, which can ensure the composite fastness, and will not cause the fabric curling and delamination problems.
[0054] In this embodiment, the knitted lining needs to be raised before compounding, and the raised surface fiber length is required to be between 4-10 mm, and the thermal insulation rate is not less than 20%. Specifically, the raising process is: vehicle speed: 10±2 m / min, large cylinder: 50±5 rpm, rotation speed: 40±5 rpm, tension 5±0.2 kg. Among them, this lining specification, through the reverse side raising finishing, makes the fabric have excellent warmth retention, and ensures lightness, thinness and breathability.
[0055] In this embodiment, the equipment used in step B and step C is a PUR hot melt adhesive compounding machine (YD-095B, Dongguan Yuanda Machinery Co., Ltd.).
[0056] In step B, the nanofilm is compounded on the denim fabric by polyurethane hot melt adhesive. The specific compounding process is: vehicle speed 15±5m / min, polyurethane hot melt adhesive amount 5±0.5g / m2, gel time 24±0.5 hours, adhesive temperature 105±5℃, adhesive application temperature 90±5℃.
[0057] In step C, the knitted lining is compounded on the nano film by polyurethane hot melt adhesive. The specific compounding process is: vehicle speed 10±5m / min, polyurethane hot melt adhesive amount 3±0.5g / m2, gel time 24±0.5 hours, adhesive temperature 105±5℃, adhesive application temperature 90±5℃.
[0058] It should be noted that, in order to ensure that the three-layer denim composite fabric in the prior art does not delaminate or bubble, the composite process used is heavy, resulting in low elasticity of the composite fabric, and in the three-layer composite structure, a non-elastic film or a low-elastic film is used, which further limits the technical problem of fabric elasticity. The three-layer composite fabric adopted in the present invention, through fabric treatment before composite and low-glue composite and other processes, is used in conjunction with the use of SURFORCE nano-membrane, utilizing its high elasticity, ultimately achieving high elasticity of the entire composite fabric, while also having excellent warmth retention, weft elasticity and breathability.
[0059] The third aspect of the present invention also provides a denim composite fabric. The denim composite fabric is prepared by the above-mentioned preparation method. In the denim composite fabric of this embodiment, its weft elasticity is greater than 30%, and its air permeability is greater than 15mm / s; its warmth retention is greater than 45%, and its gram weight range is: 270-300gsm.
[0060] The present invention is further described below in conjunction with more specific embodiments.
[0061] Example 1
[0062] The high-elastic and lightweight denim composite fabric of this embodiment has a three-layer structure, wherein one layer is a denim face fabric, CM40*P100D / 288F(SP40D)*150*75, 3 / 1 right twill, composed of 74% cotton, 23% polyester, and 3% spandex fiber, with a gram weight of 140gsm; one layer is a Surforce nano-membrane, with a gram weight of 8±0.5gsm, an air permeability of 100mm / s, and a water pressure resistance of 80kpa after washing; the innermost layer is AR 40S+P75D / 216F+PU 20D, a sweat cloth, with a horizontal and vertical elasticity of 50%, and a gram weight of 110gsm knitted fabric.
[0063] After the denim surface cloth is woven, it is processed through the process of "mechanical grinding (reverse side) → alkali washing → clean water washing".
[0064] 1. Mechanical grinding process: vehicle speed: 20m / min, rotation speed 80 rpm, large cylinder speed 60 rpm, tension 3.5bar.
[0065] 2. Alkali washing process: caustic soda content in the alkali washing solution: 6g / L, penetrant: 0.5g / L, water temperature 80℃, bath ratio 1:10, washing for 40min, alkali washing equipment is Circular Model CF, Nisaka (China) Textile Technology Co., Ltd., and then the alkali washing solution is discharged after cooling to 25℃;
[0066] 3. Washing water process, water temperature gradient is: 95℃±2, 65℃±2, 40℃±2, normal temperature water, washing time is 15min (time is evenly distributed), and the denim fabric with impurities washed away is obtained.
[0067] After the knitted fabric is processed normally, it needs to be raised on the reverse side. The raising process is: speed: 10m / min, large cylinder: 50 rpm, rotation speed: 40 rpm, tension 5Kg.
[0068] The compounding equipment is a PUR hot melt adhesive compounding machine (YD-095B, Dongguan Yuanda Machinery Co., Ltd.).
[0069] Among them, denim fabric and nano film composite process: speed 15m / min, polyurethane hot melt glue amount 5g / m2 , gel time 24 hours, gelling temperature 105℃, and gluing temperature 90℃.
[0070] Among them, knitted lining and nano-film composite process: speed 10m / min, polyurethane hot melt glue amount 3g / m 2 , gel time 24 hours, gelling temperature 105℃, and gluing temperature 90℃.
[0071] Example 2
[0072] The high-elastic and lightweight denim composite fabric in this embodiment has a three-layer structure, wherein one layer is a denim face fabric, CM40*P100D / 288F(SP40D)*170*85, 3 / 1 right twill, composed of 74% cotton, 23% polyester, and 3% spandex fiber, with a gram weight of 165gsm; one layer is a surforce nano-membrane, with a gram weight of 8±0.5gsm, an air permeability of 100mm / s, and a water pressure resistance of 80kPa after washing; the innermost layer is AR 40S+P75D / 144F+PU 20D, a sweat cloth, with a horizontal and vertical elasticity of 50%, and a gram weight of 110gsm knitted fabric.
[0073] After the denim surface cloth is woven, it is processed through the process of "mechanical grinding (reverse side) → alkali washing → clean water washing".
[0074] 1. Mechanical grinding process: vehicle speed: 20m / min, rotation speed 80 rpm, large cylinder speed 60 rpm, tension 3.5bar.
[0075] 2. The alkaline washing process is to place the fabric in a caustic soda solution with a caustic soda content of 5.5 g / L and a penetrant of 1.5 g / L, and wash it in the alkaline washing solution at a water temperature of 80°C for 40 minutes.
[0076] After the knitted lining is processed normally, it also needs to be raised on the reverse side. The raising process is: speed: 10m / min, large cylinder: 50 rpm, rotation speed: 40 rpm, tension 5kg.
[0077] The fabric compounding equipment used is a PUR hot melt adhesive compounding machine (YD-095B, Dongguan Yuanda Machinery Co., Ltd.)
[0078] Among them, the surface material and nano film composite process: vehicle speed 15m / min, polyurethane hot melt adhesive amount 5g / m 2 , gel time 24 hours, gelling temperature 105℃, and gluing temperature 90℃.
[0079] Among them, the lining and nano-film composite process: the speed is 10m / min, the amount of polyurethane hot melt glue is 3g / m 2 , gel time 24 hours, gelling temperature 105℃, and gluing temperature 90℃.
[0080] Comparative Example 1
[0081] All process parameters are consistent with those in Example 1, except that the surface material used is: CM40*P100D / 144F(SP40D)*180*105, 3 / 1 right twill, gram weight 185gsm. The surface material is heavy, and the weight difference between the surface material and the nano film is large. The denim shrinks inconsistently during washing, and is prone to bulging. After bulging, the film will be torn, affecting the thermal insulation performance; 144F polyester yarn is not easy to improve the mechanical polishing effect, and cannot effectively increase the specific surface area of the fabric, which affects the composite fastness of the surface material and the nano film, causing the delamination problem.
[0082] Comparative Example 2
[0083] All process parameters are consistent with those in Example 1, except that the surface material is not mechanically polished. Without mechanical polishing, the composite fastness of the surface material and the nanofilm will be affected, resulting in delamination.
[0084] Comparative Example 3
[0085] All process parameters are the same as those in Example 1, except that the lining material used is: AR 50S+P75D / 72F+PU20D, the weight is 90gsm knitted lining material, and the unprocessed reverse side is raised. The warmth retention does not reach the level of 45%.
[0086] Comparative Example 4
[0087] All process parameters are consistent with those in Example 1, the only difference being a two-layer structure, no middle layer and no surforce nanofilm. The warmth retention does not reach 45%.
[0088] Comparative Example 5
[0089] All process parameters are consistent with those in Example 1, except that a non-elastic TPU film is used in the middle layer. The fabric has low elasticity and no air permeability.
[0090] The performance parameters of each embodiment and comparative example are shown in Table 1.
[0091] Table 1 Performance parameters of various embodiments and comparative examples
[0092]
[0093] So far, the various embodiments of the present invention have been introduced. According to the above description, those skilled in the art should have a clear understanding of the present invention.
[0094] It should be noted that, unless explicitly indicated to the contrary, the numerical parameters in the description and claims of the present invention may be approximate values and may be changed according to the content of the present invention. Specifically, all the numbers recorded in the description and claims indicating the content of the composition, reaction conditions, etc., should be understood to be modified by the term "about" in all cases, and the meaning of the expression is to include a change of ±10% from a specific number in some embodiments.
[0095] Those skilled in the art should understand that in the claims and description of the present invention, the word "comprising" does not exclude the existence of elements (or steps) not listed in the claims. The word "a" or "an" preceding an element (or step) does not exclude the existence of multiple such elements (or steps).
[0096] For certain implementations, if they are not the key content of the present invention and are well known to ordinary technicians in the relevant technical field, they are not described in detail in the drawings or text of the specification due to space limitations. In this case, reference can be made to relevant existing technologies for understanding.
[0097] Furthermore, the above embodiments are provided solely to enable the present invention to satisfy legal requirements, and the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.
[0098] Similarly, it should be understood that in order to simplify the present invention, in the above description of the exemplary embodiments of the present invention, the various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, the method of the invention should not be interpreted as reflecting the following intention: the claimed invention requires more features than the features explicitly stated in each claim. More specifically, as reflected in the claims, each inventive aspect lies in less than all the features of the previous single embodiment. Moreover, the embodiments can be mixed and matched with each other or with other embodiments based on design and reliability considerations, that is, the technical features in different embodiments can be freely combined to form more embodiments. Therefore, the claims following the specific embodiment are hereby explicitly incorporated into the specific embodiment, wherein each claim itself serves as a separate embodiment of the present invention.
[0099] The above specific embodiments provide a detailed description of the objectives, technical means and beneficial effects of the present invention. It should be understood that the purpose of the detailed description is to enable those skilled in the art to understand the present invention more clearly, and it is not used to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A denim composite fabric, It is characterized in that include: Denim fabric, with a grammage between 140 and 165 gsm; Its weft elasticity is greater than 40%; the surface of the denim fabric to be composited with the nano-film is mechanically polished, and the polished fiber height is no more than 3mm; The nano-membrane is compounded on the denim surface fabric, and its fiber diameter is 0.1-2um, its gram weight range is: 5-30gsm, its membrane elasticity range is: 200±30%, and its air permeability range is: 1-100mm / s; The knitted lining is compounded on the nano-film, and its gram weight range is: 110±5gsm, and its horizontal and vertical elasticity range is: 50±5%; The fiber height of the denim fabric facing the nano-membrane is not higher than 3mm; the knitted lining is subjected to a raising treatment on the side not facing the nano-membrane, and the fiber length of the raising surface is between 4-10mm after the treatment, and the thermal insulation rate of the lining reaches more than 20%.
2. The denim composite fabric according to claim 1, It is characterized in that The nano film is compounded on the denim fabric by polyurethane hot melt adhesive, and the range of polyurethane hot melt adhesive is: 5±0.5g / m 2 ; And / or, the knitted lining is compounded on the nano film by polyurethane hot melt adhesive, and the range of polyurethane hot melt adhesive is: polyurethane hot melt adhesive 3±0.5g / m 2 .
3. A method for preparing the denim composite fabric according to claim 1 or 2, It is characterized in that include: Step A, obtaining a denim fabric, comprises: Mechanical grinding process: the surface of the denim fabric to be composited with the nanofilm is mechanically polished, and the polished fiber height is no more than 3mm; Alkaline washing process, the denim fabric is washed in an alkaline washing solution; The washing process is to wash the denim fabric after alkali washing with clean water; Step B, compounding the nanofilm on the denim fabric; Step C, compounding the knitted lining onto the nano film.
4. The preparation method according to claim 3, It is characterized in that Before step C, the following steps are also included: The denim fabric has a gram weight between 140 and 165 gsm; its weft elasticity is greater than 40%, and its weft yarn is P100D / 288F; And / or, in the step A, the specific surface area of the denim fabric surface increases by more than 8 times after the mechanical polishing process; And / or, the step B comprises: compounding the nano film on the denim fabric by polyurethane hot melt adhesive, wherein the amount of polyurethane hot melt adhesive is in the range of 5±0.5g / m 2 ; And / or, the step C comprises: compounding the knitted lining on the nano film by polyurethane hot melt adhesive, wherein the range of the amount of polyurethane hot melt adhesive is: 3±0.5g / m 2 .
5. The preparation method according to claim 4, It is characterized in that Before step C, the following steps are also included: Raising process: the knitted lining is subjected to reverse raising finishing, and the raising surface fiber length is required to be between 4-10mm and the thermal insulation rate is not less than 20%.
6. The preparation method according to claim 5, It is characterized in that In the mechanical grinding process, the mechanical grinding process parameters are: vehicle speed, 15±2m / min; rotation speed, 80±10 rpm; large cylinder speed, 60±5 rpm; tension, 3.5±0.5kg; And / or, in the alkali washing process, the content of alkaline material in the alkali washing solution is: 5±1 g / L, the penetrant is: 1±0.5 g / L, the water temperature is 60°C, and the alkali washing time is greater than 10 min; And / or, the process parameters of the cleaning process are: cleaning time, 5 to 30 min; water temperature gradient: 95°C ± 2, 65°C ± 2, 40°C ± 2, room temperature water; And / or, in step B, the parameters of the polyurethane hot melt adhesive laminating process are: vehicle speed 15±5 m / min; gel time 24±0.5 hours; gelling temperature 105±5°C; gluing temperature 90±5°C; And / or, in the raising process, the raising process is: vehicle speed: 10±2 m / min, large cylinder: 50±5 rpm, rotation speed: 40±5 rpm, tension 5±0.2 kg; And / or, in step C, the parameters of the polyurethane hot melt adhesive composite process are: vehicle speed 10±5m / min; gel time 24±0.5 hours; gelling temperature 105±5°C; gluing temperature 90±5°C.
7. The preparation method according to claim 3, It is characterized in that The nano-membrane has a fiber diameter of 0.1-2um, a gram weight range of 5-30gsm, a membrane elasticity range of 200±30%, and an air permeability range of 1-100mm / s; And / or, the knitted lining has a gram weight range of 110±5gsm and a horizontal and vertical elasticity range of 50±5%.
8. The preparation method according to claim 7, It is characterized in that The specifications of the denim fabric are: CM40*P100D (SP40D)*150*75, 3 / 1 right twill, woven from 74% cotton, 23% polyester, and 3% spandex fibers; wherein the F number of the P100D filament is 288; And / or, the nanomembrane is: an electrospun nanomembrane made of TPU or PU; And / or, the specification of the knitted lining is: A / R 40S+P75D+PU 20D, jersey, woven from 45% acrylic, 30% viscose, 20% polyester, and 5% spandex, wherein the F number of the P75D filament is 144 or 216.
9. A denim composite fabric, It is characterized in that Prepared by the preparation method described in any one of claims 3 to 8.