A degradable buffer material containing wheat straw biomechanical pulp fiber and preparation method thereof

Through amination treatment of wheat straw biomechanical pulp fiber and bamboo fiber, modification of talc powder, and oxidation treatment of starch, an efficient composite material is formed, which solves the poor compression rebound performance and humidity of buffer materials in the existing technology. The problem of performance degradation in the environment has been achieved, and excellent mechanical properties and degradability have been achieved.

CN118325169BActive Publication Date: 2024-10-22SHANDONG KEMAI BIO-PULPING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410773212.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-22
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

Biodegradable cushioning materials containing plant fibers in the prior art have problems such as poor compression resilience and significant decreases in strength and compression resilience in environments with high humidity.

Method used

The composite fiber of wheat straw biomechanical pulp fiber and bamboo fiber is used for amination treatment, and is compounded with modified talc powder and oxidized starch. The dispersion of talc powder and the cross-linking reaction of starch are improved through ball milling and ultrasonic treatment to form a strong Powerful composite material, combined with specific biodegradable resins for foam molding.

Benefits of technology

It achieves excellent compression resilience and strength properties of the cushioning material, maintains high mechanical properties in a humid environment, and has good cell stability and cushioning properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a degradable buffer material containing wheat straw biomechanical pulp fiber and a preparation method thereof. The preparation method comprises the steps of amination of composite fibers, modified talcum powder, preparation of a composite fiber / talcum powder mixture, oxidized starch, and foaming molding. In the preparation of the composite fiber / talcum powder mixture, the modified talcum powder is mixed with deionized water, stirred evenly, and the amination composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide are added, the temperature is raised to 53-57°C for ultrasonic treatment, the ultrasonic time is 38-42min, the ultrasonic power is 86-88W, the ultrasonic frequency is 22-24kHz, the ultrasonic treatment is performed for 19-21h after the ultrasonic treatment is completed, and the composite fiber / talcum powder mixture is filtered, washed, and dried to obtain the composite fiber / talcum powder mixture. The degradable buffer material prepared by the invention has good compression resilience and high strength, and the compression recovery resilience and strength in a wet state still maintain a high level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of degradable buffer materials, and in particular relates to a degradable buffer material containing wheat straw biomechanical pulp fibers and a preparation method thereof. Background Art

[0002] Cushioning materials are mostly foam materials, which are soft materials with a porous structure inside. The rich pore structure inside gives them good cushioning and compressive properties. The current foam materials are mainly polystyrene foam plastics and polyethylene foam plastics, which are formed by adding foaming agents, initiators, dispersants and other additives, and extruding or molding under high temperature and high pressure. They have good flexibility and cushioning properties and are widely used in home furniture, fruits and vegetables, and electronic components. However, these plastics mainly come from non-renewable petroleum resources. With the gradual depletion of traditional petrochemical resources and the increase in carbon emission restrictions, providing a foaming material based on renewable resources to replace these difficult-to-degrade and recycle petroleum-based foaming materials is the research and development direction of existing technologies.

[0003] Plant fiber is a cellulose-based biodegradable and renewable resource that is widely found in nature. It has the advantages of low cost, high utilization value, low density and high strength. Using plant fiber as a base material and degradable polymers to prepare plant fiber degradable buffer materials can not only maintain the performance of the plant fiber itself, but also improve the mechanical properties and storage modulus of the buffer material. It also has additional properties such as shock absorption and cushioning.

[0004] CN104788979A discloses a method for preparing a fully degradable foam plastic, wherein the foam plastic is composed of plant fiber, starch, polyvinyl alcohol, nano-silicon dioxide, a plant fiber surface modifier, a starch composite plasticizer and water; the specific preparation method is to use trimethylsilyl isocyanate to modify the surface of the plant fiber, add water to heat the starch, and then add a plasticizer to plasticize it; finally, the surface-modified plant fiber, the plasticized starch, polyvinyl alcohol and nano-silicon dioxide are mixed and foamed, and molded to obtain a fully degradable foam plastic with good tensile strength and elastic modulus;

[0005] The fully degradable foamed plastics prepared by the method have poor foaming performance and still relatively poor compression rebound performance, and it is not easy to rebound after the foamed material is compressed.

[0006] It can be seen that the prior art has the problem of poor rebound performance when preparing degradable cushioning materials containing plant fibers.

[0007] CN115232453A discloses a completely biodegradable flame retardant foam material and a preparation method thereof. The flame retardant foam material comprises modified plant fiber, modified oil meal, polylactic acid, and an antioxidant. The preparation method of the flame retardant foam material comprises the steps of pretreatment of plant fiber and oil meal, modification of plant fiber and oil meal, mixed granulation, heating and foaming, etc. The flame retardant foam material produced by the method has good foaming performance, can be completely biodegraded, and meets environmental protection requirements.

[0008] The foamed material prepared by this method has a high foaming ratio, uniform foaming, and good compression rebound performance, but the tensile strength of the foamed material is low, and the hygroscopicity is high in an environment with high humidity, and its strength and compression rebound performance are significantly reduced.

[0009] As can be seen from the above, the degradable buffer material containing plant fibers and the preparation method thereof in the prior art have the following problems:

[0010] 1. The compression and rebound performance of the cushioning material is poor;

[0011] 2. While improving the compression rebound performance of the cushioning material, the strength decreases, and the strength and compression rebound performance of the cushioning material are significantly reduced in an environment with high humidity. Summary of the invention

[0012] In order to solve the technical problems existing in the prior art, the present invention provides a degradable buffer material containing wheat straw biomechanical pulp fiber and a preparation method thereof, which has excellent compression resilience and strength performance, and the compression resilience and strength performance are still high in an environment with high humidity.

[0013] In view of the above technical problems, the present invention adopts the following technical solutions:

[0014] A method for preparing a degradable buffer material containing wheat straw biomechanical pulp fibers, comprising the steps of amination of composite fibers, modified talcum powder, oxidized starch, and foaming molding, and the specific operations are as follows:

[0015] 1. Amination of composite fibers

[0016] (1) Preprocessing

[0017] The composite fiber is cut to a length of 0.5-0.8 mm, and then immersed in 9-11 times the volume of sodium hydroxide solution at a soaking temperature of 80-84° C. for a soaking time of 2.3-2.7 hours. After the soaking, the composite fiber is washed and dried to obtain a pretreated composite fiber;

[0018] The composite fiber is a mixture of absolute dry wheat straw biomechanical pulp fiber and bamboo fiber, and the mass ratio of the absolute dry wheat straw biomechanical pulp fiber to the bamboo fiber is 1.4-1.6:1;

[0019] The mass concentration of the sodium hydroxide solution is 32-36%;

[0020] (2) Amination

[0021] The pretreated composite fiber is placed in a first treatment liquid with a volume of 5-7 times for a first immersion treatment, the first immersion temperature is controlled to be 43-47° C., the immersion time is 32-38 minutes, after the first immersion is completed, the composite fiber is filtered out, and the composite fiber is placed in a second treatment liquid with a volume of 6-8 times for a second immersion treatment, the second immersion time is controlled to be 2.4-2.6 hours, the immersion temperature is 67-71° C. After the second immersion is completed, the composite fiber is filtered, washed and dried to obtain an amino composite fiber;

[0022] The first treatment liquid is composed of deionized water, polyethylene glycol 300 and glycerol, and the mass ratio of the deionized water, polyethylene glycol 300 and glycerol is 74-78:1.5-1.9:1.1-1.3;

[0023] The second treatment liquid is composed of anhydrous ethanol and γ-aminopropyltriethoxysilane, and the mass ratio of anhydrous ethanol to γ-aminopropyltriethoxysilane is 83-87:1.0-1.3.

[0024] 2. Modified talc

[0025] The talc powder is placed in a ball mill for ball milling, the ball milling time is 43-48 minutes, the ball milling speed is 442-457 rpm, the ball-to-material ratio is 4-8:1, and after the ball milling is completed, it is placed in a closed container, and the modified liquid is added. After stirring, nitrogen is introduced to increase the pressure to 1.0-1.4 MPa for static treatment, the static temperature is 70-76° C., and the static time is 3.3-3.7 hours. After the static treatment, the modified talc powder is obtained;

[0026] The particle size of the talc is 110-130 nm, and the mass content of silicon dioxide is 58.7-60.4%;

[0027] The mass ratio of the talcum powder to the modified liquid is 22-24:135-141;

[0028] The preparation method of the modified liquid comprises adding sodium dodecylbenzene sulfonate and tartaric acid to deionized water, and then performing ultrasonic oscillation treatment, wherein the ultrasonic time is 28-32 minutes, the ultrasonic power is 247-253W, the ultrasonic frequency is 34-38kHz, and the modified liquid is obtained after the ultrasonic treatment is completed;

[0029] The mass ratio of the deionized water, sodium dodecylbenzene sulfonate and tartaric acid is 117-123:1.2-1.4:1.5-1.7.

[0030] 3. Preparation of Composite Fiber / Talc Mixture

[0031] The modified talc powder is mixed with 6-8 times the mass of deionized water, and after stirring evenly, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide are added, and the temperature is raised to 53-57° C. at a rate of 1.4-1.6° C. / min, and ultrasonic treatment is performed. The ultrasonic time is 38-42 min, the ultrasonic power is 86-88 W, and the ultrasonic frequency is 22-24 kHz. After the ultrasonic treatment, the mixture is stirred at 226-234 rpm for 19-21 h, filtered, washed, and dried to obtain a composite fiber / talc powder mixture;

[0032] The mass ratio of the modified talc powder, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide is 27-29:71-75:8.2-8.6:8.2-8.6.

[0033] 4. Oxidized starch

[0034] The starch is placed in deionized water, and then a sulfuric acid solution is added for ultrasonic treatment, the ultrasonic time is 27-33 minutes, the ultrasonic frequency is 43-47kHz, the temperature is raised to 76-80°C after the ultrasonic treatment, and the mixture is stirred at 76-80°C for 3.0-3.4 hours. After the stirring is completed, the temperature is lowered to 36-38°C at a rate of 0.9-1.1°C / min, sodium periodate is added, and the mixture is stirred at 36-38°C for 4.3-4.7 hours. After the stirring is completed, the mixture is filtered and washed to obtain oxidized starch;

[0035] The starch is tapioca starch;

[0036] The mass concentration of the sulfuric acid solution is 58-62%;

[0037] The mass ratio of the starch, deionized water, sulfuric acid solution and sodium periodate is 15-19:143-151:12-14:17-19.

[0038] 5. Foaming

[0039] The composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, a foaming agent, stearic acid, and liquid paraffin are mixed and stirred to obtain a mixture, and the mixture is extruded into a mold for foaming through an extruder, and the mixing and extrusion temperature is controlled to be 140-145° C. and the foaming molding temperature is controlled to be 127-132° C. to obtain a degradable cushioning material;

[0040] The foaming agent is a mixture of sodium bicarbonate and azodicarbonamide, and the mass ratio of the sodium bicarbonate to azodicarbonamide is 1.1-1.3:1;

[0041] The mass ratio of the composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, foaming agent, stearic acid and liquid paraffin is 68-72:4.5-4.9:4.8-5.2:1.0-1.2:1.6-1.8:0.7-0.9.

[0042] A degradable buffer material containing wheat straw biomechanical pulp fibers is prepared by the above preparation method.

[0043] Compared with the prior art, the present invention achieves the following beneficial effects:

[0044] 1. The present invention first pre-treats the composite fiber, and then immerses it in a first treatment liquid, which mainly improves the dispersion performance of the composite fiber and increases the hydroxyl groups on the surface of the composite fiber. Then, the composite fiber is immersed in a second treatment liquid, and the aminosilane coupling agent in the second treatment liquid bonds with the hydroxyl groups on the fiber surface, so that the composite fiber surface contains amino groups; then, talcum powder is used as a filler, and ball milling treatment is first performed on it. Under the action of mechanical force, the talcum powder is subjected to the comprehensive effects of impact, friction, etc., so that the lattice defects and lattice distortion of the talcum powder particles are increased, the surface activity of the talcum powder particles is improved, and the aggregation between the particles is avoided. Combined with the treatment of the modified liquid, the talcum powder particles are subjected to the comprehensive effects of impact, friction, etc., so that the talcum powder particles are subjected to the comprehensive effects of impact, friction, etc., and the surface activity of the talcum powder particles is improved. The modified liquid can further promote the particle dispersibility of talcum powder on the one hand, so that the talcum powder particles are in a state of being individually dispersed. On the other hand, the modified liquid is rich in carboxyl groups. After the talcum powder is treated by the modified liquid, the surface of the talcum powder is rich in carboxyl groups, so that the talcum powder finally presents particles with good individual dispersibility and rich in carboxyl groups on the surface; the present invention composites the aminated composite fiber with the modified talcum powder, and the amino group of the composite fiber and the carboxyl group of the modified talcum powder undergo an amidation reaction, so that the composite fiber and the talcum powder are evenly dispersed and form a strong connection, so that the foaming is uniform, the foam stability is good, and the strength performance and stability performance of the buffer material are enhanced;

[0045] The present invention processes starch so that the hydroxyl groups of the starch are oxidized to aldehyde groups. In the foaming molding step, the aldehyde groups of the oxidized starch and the amide groups of the composite fiber / talcum powder can undergo a cross-linking reaction, which can weaken the hydrophilicity of the starch, improve the blending performance between the composite fiber, talcum powder and starch, enhance the bonding force, make the mixture dispersed uniformly and stably, thereby improving the stability during foaming molding. The mixture is combined with specific degradable resin components such as polyethylene glycol succinate to ensure a fine and uniform foam structure, so that the pores of the buffer material are stable, the pore wall strength is higher, the pores are not easy to deform and collapse, the buffer material has higher compression resilience and better mechanical properties, and has good stability and good degradability, and still has good mechanical properties in a humid environment;

[0046] 2. The degradable buffer material prepared by the present invention has a tensile strength of 3.91-3.99 MPa, an elongation at break of 219-228% (GB / T 6344-2008), and an impact strength of 1.04-1.13 kJ / m 2 (GB / T 1843-2008);

[0047] 3. The degradable buffer material prepared by the present invention has a compression rebound rate of 98.1-98.8% when the volume is compressed by 50% and maintained for 120 hours at a humidity of 20%, a compression rebound rate of 96.0-96.5% when the humidity is 40%, a compression rebound rate of 93.9-94.4% when the humidity is 80%, and a compression rebound rate of 91.9-92.3% when the humidity is 20%;

[0048] 4. The degradable buffer material prepared by the present invention was placed in an environment with a temperature of 45°C and a humidity of 75% and left to stand for 7 days. After the standing period, the tensile strength was measured again to be 3.81-3.92MPa, the elongation at break was 212-223%, and the impact strength was 1.00-1.11kJ / m 2 . DETAILED DESCRIPTION

[0049] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.

[0050] Example 1

[0051] 1. Amination of composite fibers

[0052] (1) Preprocessing

[0053] The composite fiber was cut to a length of 0.7 mm, and then immersed in a sodium hydroxide solution with a volume of 10 times, the immersion temperature was 82° C., the immersion time was 2.5 h, and after the immersion, it was washed and dried to obtain the pretreated composite fiber;

[0054] The composite fiber is a mixture of absolute dry wheat straw biomechanical pulp fiber and bamboo fiber, and the mass ratio of the absolute dry wheat straw biomechanical pulp fiber to the bamboo fiber is 1.5:1;

[0055] The mass concentration of the sodium hydroxide solution is 34%;

[0056] (2) Amination

[0057] The pretreated composite fiber is placed in a first treatment liquid with a volume of 6 times, and the first immersion temperature is controlled to be 45°C, and the immersion time is 35 minutes. After the first immersion is completed, the composite fiber is filtered out and placed in a second treatment liquid with a volume of 7 times, and the second immersion time is controlled to be 2.5 hours, and the immersion temperature is 69°C. After the second immersion is completed, it is filtered, washed, and dried to obtain an amino composite fiber;

[0058] The first treatment liquid is composed of deionized water, polyethylene glycol 300 and glycerol, and the mass ratio of the deionized water, polyethylene glycol 300 and glycerol is 76:1.7:1.2;

[0059] The second treatment liquid consists of anhydrous ethanol and γ-aminopropyltriethoxysilane, and the mass ratio of the anhydrous ethanol to γ-aminopropyltriethoxysilane is 85:1.2.

[0060] 2. Modified talc

[0061] The talc powder was placed in a ball mill for ball milling, the ball milling time was 45 minutes, the ball milling speed was 450 rpm, the ball-to-material ratio was 6:1, and after the ball milling was completed, it was placed in a closed container, and the modified liquid was added. After stirring, nitrogen was introduced to increase the pressure to 1.2 MPa for static treatment, the static temperature was 73°C, and the static time was 3.5 hours. After the static treatment, the modified talc powder was obtained;

[0062] The particle size of the talc is 120 nm, and the mass content of silicon dioxide is 60%;

[0063] The mass ratio of the talcum powder to the modified liquid is 23:138;

[0064] The preparation method of the modified liquid comprises adding sodium dodecylbenzene sulfonate and tartaric acid to deionized water, and then performing ultrasonic oscillation treatment, wherein the ultrasonic time is 30 minutes, the ultrasonic power is 250W, the ultrasonic frequency is 36kHz, and the modified liquid is obtained after the ultrasonic treatment is completed;

[0065] The mass ratio of the deionized water, sodium dodecylbenzene sulfonate and tartaric acid is 120:1.3:1.6.

[0066] 3. Preparation of Composite Fiber / Talc Mixture

[0067] The modified talc powder was mixed with 7 times the mass of deionized water, and after being stirred evenly, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide were added, and the temperature was raised to 55°C at a rate of 1.5°C / min, and ultrasonic treatment was performed. The ultrasonic time was 40min, the ultrasonic power was 87W, and the ultrasonic frequency was 23kHz. After the ultrasonic treatment, the mixture was stirred at 230rpm for 20h, filtered, washed, and dried to obtain a composite fiber / talc powder mixture;

[0068] The mass ratio of the modified talc powder, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide is 28:73:8.4:8.4.

[0069] 4. Oxidized starch

[0070] The starch was placed in deionized water, and then sulfuric acid solution was added for ultrasonic treatment. The ultrasonic time was 30 minutes and the ultrasonic frequency was 45 kHz. After the ultrasonic treatment, the temperature was raised to 78°C and stirred at 78°C for 3.2 hours. After the stirring was completed, the temperature was lowered to 37°C at a rate of 1.0°C / min, sodium periodate was added, and the mixture was stirred at 37°C for 4.5 hours. After the stirring was completed, the mixture was filtered and washed to obtain oxidized starch.

[0071] The starch is tapioca starch;

[0072] The mass concentration of the sulfuric acid solution is 60%;

[0073] The mass ratio of the starch, deionized water, sulfuric acid solution and sodium periodate is 17:147:13:18.

[0074] 5. Foaming

[0075] The composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, a foaming agent, stearic acid, and liquid paraffin are mixed and stirred to obtain a mixture, and the mixture is blended and extruded into a mold for foaming molding through an extruder, and the blending extrusion temperature is controlled to be 142° C. and the foaming molding temperature is controlled to be 130° C. to obtain a degradable cushioning material;

[0076] The foaming agent is a mixture of sodium bicarbonate and azodicarbonamide, and the mass ratio of the sodium bicarbonate to azodicarbonamide is 1.2:1;

[0077] The mass ratio of the composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, foaming agent, stearic acid and liquid paraffin is 70:4.7:5.0:1.1:1.7:0.8.

[0078] Example 2

[0079] 1. Amination of composite fibers

[0080] (1) Preprocessing

[0081] The composite fiber was cut to a length of 0.5 mm, and then immersed in 9 times the volume of sodium hydroxide solution at a soaking temperature of 80° C. for 2.3 h. After the soaking, the composite fiber was washed and dried to obtain the pretreated composite fiber.

[0082] The composite fiber is a mixture of absolute dry wheat straw biomechanical pulp fiber and bamboo fiber, and the mass ratio of the absolute dry wheat straw biomechanical pulp fiber to the bamboo fiber is 1.4:1;

[0083] The mass concentration of the sodium hydroxide solution is 32%;

[0084] (2) Amination

[0085] The pretreated composite fiber is placed in a first treatment liquid with a volume of 5 times, and the first immersion temperature is controlled to be 43°C, and the immersion time is 32 minutes. After the first immersion, the composite fiber is filtered out and placed in a second treatment liquid with a volume of 6 times, and the second immersion time is controlled to be 2.4 hours, and the immersion temperature is 67°C. After the second immersion, the composite fiber is filtered, washed, and dried to obtain an amino composite fiber.

[0086] The first treatment liquid is composed of deionized water, polyethylene glycol 300 and glycerol, and the mass ratio of the deionized water, polyethylene glycol 300 and glycerol is 74:1.5:1.1;

[0087] The second treatment liquid consists of anhydrous ethanol and γ-aminopropyltriethoxysilane, and the mass ratio of the anhydrous ethanol to γ-aminopropyltriethoxysilane is 83:1.0.

[0088] 2. Modified talc

[0089] The talc powder was placed in a ball mill for ball milling, the ball milling time was 43 minutes, the ball milling speed was 442 rpm, the ball-to-material ratio was 4:1, and after the ball milling was completed, it was placed in a closed container, and the modified liquid was added. After stirring, nitrogen was introduced to increase the pressure to 1.0 MPa for static treatment, the static temperature was 70°C, and the static time was 3.3 hours. After the static treatment, the modified talc powder was obtained;

[0090] The particle size of the talc is 110 nm, and the mass content of silicon dioxide is 58.7%;

[0091] The mass ratio of the talcum powder to the modified liquid is 22:135;

[0092] The preparation method of the modified liquid comprises adding sodium dodecylbenzene sulfonate and tartaric acid to deionized water, and then performing ultrasonic oscillation treatment, wherein the ultrasonic time is 28 minutes, the ultrasonic power is 247W, the ultrasonic frequency is 34kHz, and the modified liquid is obtained after the ultrasonic treatment is completed;

[0093] The mass ratio of the deionized water, sodium dodecylbenzene sulfonate and tartaric acid is 117:1.2:1.5.

[0094] 3. Preparation of Composite Fiber / Talc Mixture

[0095] The modified talc powder was mixed with 6 times the mass of deionized water, and after being stirred evenly, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide were added, and the temperature was raised to 53°C at a rate of 1.4°C / min, and ultrasonic treatment was performed. The ultrasonic time was 38 minutes, the ultrasonic power was 86W, and the ultrasonic frequency was 22kHz. After the ultrasonic treatment, the mixture was stirred at 226rpm for 19 hours, filtered, washed, and dried to obtain a composite fiber / talc powder mixture;

[0096] The mass ratio of the modified talc powder, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide is 27:71:8.2:8.2.

[0097] 4. Oxidized starch

[0098] The starch was placed in deionized water, and then sulfuric acid solution was added for ultrasonic treatment. The ultrasonic time was 27 minutes and the ultrasonic frequency was 43 kHz. After the ultrasonic treatment, the temperature was raised to 76°C and stirred at 76°C for 3.0 hours. After the stirring was completed, the temperature was lowered to 36°C at a rate of 0.9°C / min, sodium periodate was added, and the mixture was stirred at 36°C for 4.3 hours. After the stirring was completed, the mixture was filtered and washed to obtain oxidized starch.

[0099] The starch is tapioca starch;

[0100] The mass concentration of the sulfuric acid solution is 58%;

[0101] The mass ratio of the starch, deionized water, sulfuric acid solution and sodium periodate is 15:143:12:17.

[0102] 5. Foaming

[0103] The composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, a foaming agent, stearic acid, and liquid paraffin are mixed and stirred to obtain a mixture, and the mixture is extruded into a mold for foaming through an extruder, and the mixing and extrusion temperature is controlled to be 140° C. and the foaming molding temperature is controlled to be 127° C. to obtain a degradable cushioning material;

[0104] The foaming agent is a mixture of sodium bicarbonate and azodicarbonamide, and the mass ratio of the sodium bicarbonate to azodicarbonamide is 1.1:1;

[0105] The mass ratio of the composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, foaming agent, stearic acid and liquid paraffin is 68:4.5:4.8:1.0:1.6:0.7.

[0106] Example 3

[0107] 1. Amination of composite fibers

[0108] (1) Preprocessing

[0109] The composite fiber was cut to a length of 0.8 mm, and then immersed in 11 times the volume of sodium hydroxide solution at a soaking temperature of 84° C. for 2.7 h. After the soaking, the composite fiber was washed and dried to obtain the pretreated composite fiber.

[0110] The composite fiber is a mixture of absolute dry wheat straw biomechanical pulp fiber and bamboo fiber, and the mass ratio of the absolute dry wheat straw biomechanical pulp fiber to the bamboo fiber is 1.6:1;

[0111] The mass concentration of the sodium hydroxide solution is 36%;

[0112] (2) Amination

[0113] The pretreated composite fiber is placed in a first treatment liquid with a volume of 7 times, and the first immersion temperature is controlled to be 47°C, and the immersion time is 38 minutes. After the first immersion, the composite fiber is filtered out and placed in a second treatment liquid with a volume of 8 times, and the second immersion time is controlled to be 2.6 hours, and the immersion temperature is 71°C. After the second immersion, the composite fiber is filtered, washed, and dried to obtain an amino composite fiber.

[0114] The first treatment liquid is composed of deionized water, polyethylene glycol 300 and glycerol, and the mass ratio of the deionized water, polyethylene glycol 300 and glycerol is 78:1.9:1.3;

[0115] The second treatment liquid consists of anhydrous ethanol and γ-aminopropyltriethoxysilane, and the mass ratio of the anhydrous ethanol to γ-aminopropyltriethoxysilane is 87:1.3.

[0116] 2. Modified talc

[0117] The talc powder was placed in a ball mill for ball milling, the ball milling time was 48 minutes, the ball milling speed was 457 rpm, the ball-to-material ratio was 8:1, and after the ball milling was completed, it was placed in a closed container, and the modified liquid was added. After stirring, nitrogen was introduced to increase the pressure to 1.4 MPa for static treatment. The static temperature was 76° C. and the static time was 3.7 hours. After the static treatment, the modified talc powder was obtained;

[0118] The particle size of the talc is 130 nm, and the mass content of silicon dioxide is 60.4%;

[0119] The mass ratio of the talcum powder to the modified liquid is 24:141;

[0120] The preparation method of the modified liquid comprises adding sodium dodecylbenzene sulfonate and tartaric acid to deionized water, and then performing ultrasonic oscillation treatment, wherein the ultrasonic time is 32 minutes, the ultrasonic power is 253W, the ultrasonic frequency is 38kHz, and the modified liquid is obtained after the ultrasonic treatment is completed;

[0121] The mass ratio of the deionized water, sodium dodecylbenzene sulfonate and tartaric acid is 123:1.4:1.7.

[0122] 3. Preparation of Composite Fiber / Talc Mixture

[0123] The modified talc powder was mixed with 8 times the mass of deionized water, and after being stirred evenly, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide were added, and the temperature was raised to 57°C at a rate of 1.6°C / min, and ultrasonic treatment was performed. The ultrasonic time was 42 minutes, the ultrasonic power was 88W, and the ultrasonic frequency was 24kHz. After the ultrasonic treatment, the mixture was stirred at 234 rpm for 21 hours, filtered, washed, and dried to obtain a composite fiber / talc powder mixture;

[0124] The mass ratio of the modified talc powder, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide is 29:75:8.6:8.6.

[0125] 4. Oxidized starch

[0126] The starch was placed in deionized water, and then sulfuric acid solution was added for ultrasonic treatment. The ultrasonic time was 33 minutes and the ultrasonic frequency was 47 kHz. After the ultrasonic treatment, the temperature was raised to 80°C and stirred at 80°C for 3.4 hours. After the stirring was completed, the temperature was lowered to 38°C at a rate of 1.1°C / min, sodium periodate was added, and the mixture was stirred at 38°C for 4.7 hours. After the stirring was completed, the mixture was filtered and washed to obtain oxidized starch.

[0127] The starch is tapioca starch;

[0128] The mass concentration of the sulfuric acid solution is 62%;

[0129] The mass ratio of the starch, deionized water, sulfuric acid solution and sodium periodate is 19:151:14:19.

[0130] 5. Foaming

[0131] The composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, a foaming agent, stearic acid, and liquid paraffin are mixed and stirred to obtain a mixture, and the mixture is blended and extruded into a mold for foaming molding through an extruder, and the blending extrusion temperature is controlled to be 145° C. and the foaming molding temperature is controlled to be 132° C. to obtain a degradable cushioning material;

[0132] The foaming agent is a mixture of sodium bicarbonate and azodicarbonamide, and the mass ratio of the sodium bicarbonate to azodicarbonamide is 1.3:1;

[0133] The mass ratio of the composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, foaming agent, stearic acid and liquid paraffin is 72:4.9:5.2:1.2:1.8:0.9.

[0134] Comparative Example 1

[0135] Based on Example 1, the changes are as follows:

[0136] ① In the amination step of the composite fiber, the amination step is omitted;

[0137] ② The modified talc powder step is omitted, and talc powder without any treatment is directly used; the particle size of the talc powder is 120nm, and the mass content of silicon dioxide is 60%;

[0138] ③ In the step of preparing the composite fiber / talc mixture, the modified talc is replaced by untreated talc in equal amounts, the amination composite fiber is replaced by pretreated composite fiber in equal amounts, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide components are omitted;

[0139] The rest of the operations are the same.

[0140] Comparative Example 2

[0141] The oxidized starch step was omitted;

[0142] In the foaming and molding step, an equal amount of oxidized starch is replaced by starch that has not been treated in any way, and the starch is cassava starch;

[0143] The rest of the operations are the same.

[0144] Performance Testing

[0145] (1) Strength performance

[0146] The strength performance test of the degradable buffer materials prepared in Examples 1-3 and Comparative Examples 1-2 was carried out, and the tensile performance was tested according to the method in GB / T 6344-2008; the impact resistance was tested according to the method in GB / T 1843-2008; the test results are as follows:

[0147]

[0148] (2) Compression rebound performance

[0149] The compression rebound performance test was performed on the degradable cushioning materials prepared in Examples 1-3 and Comparative Examples 1-2. The specific method was as follows: first, the volume V1 of the degradable cushioning material was measured, and then its volume was compressed by 50% and maintained for 120 hours. The humidity of the test was 20%, 40%, 80%, and 90%, respectively. The volume V2 of the product was tested again. The compression rebound rate = V2 / V1×100%. The test results are as follows:

[0150]

[0151] (3) Strength retention performance

[0152] The degradable cushioning materials prepared in Examples 1-3 and Comparative Examples 1-2 were placed in an environment with a temperature of 45° C. and a humidity of 75% and left to stand for 7 days. After the standing period, the strength performance of the degradable cushioning materials was tested again. The specific results are as follows:

[0153]

[0154] It can be seen from the above results that Comparative Example 1 omits the amination step of the composite fiber and uses talcum powder that has not been treated in any way. In the step of preparing the composite fiber / talcum powder mixture, the composite fiber and talcum powder can only be physically mixed, and cannot undergo an amidation reaction. The dispersion and bonding force between the composite fiber and talcum powder are poor, which in turn affects the uniformity and stability of foaming, and reduces the strength and stability of the buffer material. In addition, in the foaming molding step, the oxidized starch cannot react with the amide bond, thereby failing to weaken the hydrophilicity of the starch. The buffer material finally obtained has poor strength performance, low compression resilience, and low strength performance retention in a humid environment.

[0155] In Comparative Example 2, the starch oxidation step is omitted, and the starch without any treatment cannot be bonded with the amide bond, resulting in poor bonding between the starch and the composite fiber and talcum powder, uneven foaming in the foaming molding step, and unstable bubbles, resulting in low and unstable mechanical properties of the cushioning material and poor compression resilience.

[0156] The present invention first pre-treats the composite fiber, and then places it in a first treatment liquid for dipping, which mainly improves the dispersion performance of the composite fiber and increases the hydroxyl groups on the surface of the composite fiber. Then, the composite fiber is placed in a second treatment liquid for dipping treatment, and the aminosilane coupling agent in the second treatment liquid bonds with the hydroxyl groups on the fiber surface, so that the composite fiber surface contains amino groups; then talcum powder is used as a filler, and is first ball-milled. Under the action of mechanical force, the talcum powder is subjected to the comprehensive effects of impact, friction, etc., so that the lattice defects and lattice distortion of the talcum powder particles are increased, the surface activity of the talcum powder particles is improved, and aggregation between particles is avoided. Combined with the treatment of the modification liquid, the talcum powder particles are subjected to the comprehensive effects of impact, friction, etc., so that ... and the surface activity of the talcum powder particles is improved. Aggregation between particles is avoided, and the talcum powder particles are subjected to the treatment of the modification liquid. On the one hand, the modified liquid can further promote the particle dispersibility of talcum powder, so that the talcum powder particles are in a state of being individually dispersed. On the other hand, the modified liquid is rich in carboxyl groups. After the talcum powder is treated by the modified liquid, the surface of the talcum powder is rich in carboxyl groups, so that the talcum powder finally presents particles with good individual dispersibility and rich in carboxyl groups on the surface; the present invention composites the amino composite fiber with the modified talcum powder, and the amino group of the composite fiber and the carboxyl group of the modified talcum powder undergo an amidation reaction, so that the composite fiber and the talcum powder are evenly dispersed and form a strong connection, so that the foaming is uniform, the foam stability is good, and the strength and stability of the buffer material are enhanced;

[0157] The present invention processes starch so that the hydroxyl groups of the starch are oxidized into aldehyde groups. In the foaming molding step, the aldehyde groups of the oxidized starch and the amide groups of the composite fiber / talcum powder can undergo a cross-linking reaction, which can weaken the hydrophilicity of the starch, improve the blending performance between the composite fiber, the talcum powder and the starch, enhance the bonding force, make the mixture dispersed uniformly and stably, thereby improving the stability during foaming molding. The mixture is combined with specific degradable resin components such as polyethylene glycol succinate to ensure the fineness and uniformity of the foam structure, so that the pores of the buffer material are stable, the pore wall strength is higher, the pores are not easy to deform and collapse, the buffer material has higher compression resilience and better mechanical properties, and has good stability and good degradability, and still has good mechanical properties in a humid environment.

[0158] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.

[0159] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a degradable buffer material containing wheat straw biomechanical pulp fibers, characterized in that: The preparation method comprises the steps of amination of composite fibers, modification of talcum powder, preparation of a composite fiber / talcum powder mixture, oxidizing starch, and foaming molding; The composite fiber amination comprises pretreatment and amination steps; The pretreatment step comprises cutting the composite fiber to a length of 0.5-0.8 mm, and then soaking it in a sodium hydroxide solution of 9-11 times the volume, at a soaking temperature of 80-84° C. for a soaking time of 2.3-2.7 hours, washing it after soaking, and drying it to obtain the pretreated composite fiber; The amination step comprises placing the pretreated composite fiber in a first treatment liquid with a volume of 5-7 times, performing a first immersion treatment, controlling the first immersion temperature to be 43-47° C., and the immersion time to be 32-38 minutes. After the first immersion is completed, filtering out the composite fiber, placing it in a second treatment liquid with a volume of 6-8 times, performing a second immersion treatment, controlling the second immersion time to be 2.4-2.6 hours, and the immersion temperature to be 67-71° C., and after the second immersion is completed, filtering, washing, and drying to obtain the amination composite fiber; The first treatment liquid consists of deionized water, polyethylene glycol 300 and glycerol; The second treatment liquid is composed of anhydrous ethanol and γ-aminopropyltriethoxysilane; The step of modifying talcum powder is to place talcum powder in a ball mill for ball milling, wherein the ball milling time is 43-48 minutes, the ball milling speed is 442-457 rpm, and the ball-to-material ratio is 4-8:1; after the ball milling, the talcum powder is placed in a closed container, a modifying liquid is added, and after stirring evenly, nitrogen is introduced to increase the pressure to 1.0-1.4 MPa for standing treatment, the standing temperature is 70-76° C., and the standing time is 3.3-3.7 hours. After the standing, the modified talcum powder is obtained; The preparation method of the modified liquid comprises adding sodium dodecylbenzene sulfonate and tartaric acid to deionized water, and then performing ultrasonic oscillation treatment, wherein the ultrasonic time is 28-32 minutes, the ultrasonic power is 247-253W, the ultrasonic frequency is 34-38kHz, and the modified liquid is obtained after the ultrasonic treatment is completed; The step of preparing the composite fiber / talcum powder mixture is as follows: mixing the modified talcum powder with 6-8 times the mass of deionized water, stirring evenly, adding the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide, heating to 53-57° C. at a rate of 1.4-1.6° C. / min, performing ultrasonic treatment, wherein the ultrasonic time is 38-42 min, the ultrasonic power is 86-88 W, and the ultrasonic frequency is 22-24 kHz. After the ultrasonic treatment is completed, stirring at 226-234 rpm for 19-21 h, filtering, washing, and drying to obtain the composite fiber / talcum powder mixture; The starch oxidation step comprises placing starch in deionized water, then adding sulfuric acid solution for ultrasonic treatment, wherein the ultrasonic time is 27-33 minutes, the ultrasonic frequency is 43-47kHz, heating to 76-80°C after the ultrasonic treatment, stirring at 76-80°C for 3.0-3.4 hours, cooling to 36-38°C at a rate of 0.9-1.1°C / min after the stirring, adding sodium periodate, stirring at 36-38°C for 4.3-4.7 hours, filtering and washing after the stirring, and obtaining the oxidized starch; The foaming molding step comprises mixing a composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, a foaming agent, stearic acid, and liquid paraffin, stirring the mixture evenly to obtain a mixture, and extruding the mixture into a mold for foaming molding through an extruder, controlling the mixing and extrusion temperature to be 140-145° C. and the foaming molding temperature to be 127-132° C. to obtain a degradable cushioning material; The foaming agent is a mixture of sodium bicarbonate and azodicarbonamide, and the mass ratio of the sodium bicarbonate to azodicarbonamide is 1.1-1.3:1; The mass ratio of the composite fiber / talcum powder mixture, oxidized starch, polyethylene glycol succinate, foaming agent, stearic acid and liquid paraffin is 68-72:4.5-4.9:4.8-5.2:1.0-1.2:1.6-1.8:0.7-0.

9.

2. The method for preparing a degradable buffer material containing wheat straw biomechanical pulp fiber according to claim 1, characterized in that: In the fiber pretreatment step, the composite fiber is a mixture of absolute dry wheat straw biomechanical pulp fiber and bamboo fiber, and the mass ratio of the absolute dry wheat straw biomechanical pulp fiber to the bamboo fiber is 1.4-1.6:1; The mass concentration of the sodium hydroxide solution is 32-36%.

3. The method for preparing a degradable buffer material containing wheat straw biomechanical pulp fiber according to claim 1, characterized in that: In the amination step, in the first treatment solution, the mass ratio of the deionized water, polyethylene glycol 300 and glycerol is 74-78: 1.5-1.9:1.1-1.3; In the second treatment liquid, the mass ratio of the anhydrous ethanol to γ-aminopropyltriethoxysilane is 83-87:1.0-1.

3.

4. The method for preparing a degradable buffer material containing wheat straw biomechanical pulp fiber according to claim 1, characterized in that: In the modified talc step, the particle size of the talc is 110-130 nm, and the mass content of silicon dioxide is 58.7-60.4%; The mass ratio of the talcum powder to the modified liquid is 22-24:135-141; The mass ratio of the deionized water, sodium dodecylbenzene sulfonate and tartaric acid is 117-123:1.2-1.4:1.5-1.

7.

5. The method for preparing a degradable buffer material containing wheat straw biomechanical pulp fiber according to claim 1, characterized in that: In the step of preparing the composite fiber / talc mixture, the mass ratio of the modified talc, the amino composite fiber, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and N-hydroxysuccinimide is 27-29:71-75:8.2-8.6:8.2-8.

6.

6. The method for preparing a degradable buffer material containing wheat straw biomechanical pulp fiber according to claim 1, characterized in that: In the step of oxidizing starch, the starch is tapioca starch; The mass concentration of the sulfuric acid solution is 58-62%; The mass ratio of the starch, deionized water, sulfuric acid solution and sodium periodate is 15-19:143-151:12-14:17-19.

7. A degradable buffer material containing wheat straw biomechanical pulp fibers obtained according to the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Preparation method of fully-degradable foamed plastic

    CN104788979A

  • Completely biodegradable flame-retardant foaming material and preparation method thereof

    CN115232453A

  • Preparation method of bamboo powder-filled reinforced starch-based degradable composite foaming material

    CN109054104A

  • Preparation method of composite plant fiber buffer packaging material

    CN110408225A

  • Preparation method of degradable bamboo fiber straw

    CN112961394A