Method for producing steelmaking slag-forming accelerator and steelmaking slag-forming accelerator
By sorting, crushing and sintering the aluminum electrolytic cell overhaul slag, a steelmaking slag accelerator is obtained, which solves the problems of pollution and resource utilization, achieves the multiple goals of harmless treatment and environmental protection, and improves the quality of steelmaking. Efficiency and effectiveness of the steelmaking process.
Patent Information
- Application Number
- CN202410755764.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Due to the corrosiveness and toxicity of fluoride and cyanide, the treatment and landfilling of aluminum electrolytic cell overhaul slag poses serious pollution risks, and the country has banned new overhaul slag storage slag yards. It is necessary to seek harmless treatment and resource utilization. Utilization method.
By sorting and crushing the overhaul slag of the aluminum electrolytic cell, adding alumina or aluminum hydroxide as an additive, and sintering it through a rotary kiln, a steelmaking slag accelerator is produced. The ingredients include fluoride, alumina, and silicon oxide. etc., used for deoxidation, desulfurization and slagging in the steelmaking process.
It realizes resource recovery and harmless treatment of aluminum electrolytic cell overhaul slag, eliminates hidden dangers of pollution, provides environmentally friendly and economical solutions, and improves the efficiency and effectiveness of the steelmaking process.
Smart Images

Figure CN118326120B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of comprehensive utilization of solid waste, and in particular to a method for producing a steelmaking slag accelerator using aluminum electrolytic cell overhaul slag and the corresponding steelmaking slag accelerator. Background Art
[0002] The statements in this section are merely intended to provide background information related to the technical solution of the present application to aid understanding, and they do not necessarily constitute prior art for the technical solution of the present application.
[0003] Aluminum electrolytic cell overhaul slag is a solid waste generated during the production of electrolytic aluminum. Previously, the main treatment method was landfill. However, the relevant national departments have clearly prohibited the construction of new overhaul slag storage sites. The cathode lining of the aluminum electrolytic cell needs to be repaired and replaced after a period of operation. According to the current production technology status and development status, the overhaul cycle of the aluminum electrolytic cell is generally designed to be 2200 days. The waste cathode steel bars, silicon nitride combined with silicon carbide side blocks, waste cathodes, anti-seepage materials, and others (mainly including: paste, ceramic fiberboard, calcium silicate board, refractory bricks, high-strength castables, etc.) removed during the overhaul of the aluminum electrolytic cell are collectively referred to as aluminum electrolytic cell overhaul slag.
[0004] Since electrolytes - fluoride salts and cryolite need to be added during the aluminum electrolysis production process, about 27kg of fluoride salts and 5kg of cryolite are consumed per ton of aluminum. In addition to a part of these fluorides being discharged from the atmosphere, the other part undergoes an electrochemical reaction with the cathode lining at high temperature and remains in the cell lining, resulting in a high fluoride content in the aluminum electrolytic cell overhaul slag. Carbonaceous materials account for about 50% of the aluminum electrolytic cell overhaul slag, and fluoride salts account for about 30%. Other substances are mainly nepheline, β-alumina, a small amount of aluminum carbide, aluminum nitride, aluminum-iron alloy and trace cyanide, among which fluoride is highly corrosive and cyanide is a toxic substance. Aluminum electrolytic cell overhaul slag is a hazardous waste, with cyanide and fluoride as the main pollutants, and has been included in the "National Hazardous Waste List" (hazardous waste code: 321-023-48).
[0005] For the above reasons, whether it is storage or landfill, there are extremely strict requirements for aluminum electrolytic cell overhaul slag, which requires huge investment and operation and management costs, and there are long-term potential pollution risks. Therefore, the best and final solution is to harmlessly treat the aluminum electrolytic cell overhaul slag, turn it into treasure, and fundamentally eliminate the pollution risks. Summary of the invention
[0006] In order to realize the comprehensive resource utilization of aluminum electrolytic cell overhaul slag, one aspect of the present invention provides a method for producing a steelmaking slag-forming promoter, comprising: sorting the aluminum electrolytic cell overhaul slag to sort out silicon nitride combined with silicon carbide side blocks, waste cathode steel bars and waste cathodes; after the sorting, crushing the remaining materials in the aluminum electrolytic cell overhaul slag to obtain scraps; mixing additives into the scraps, the additives containing aluminum oxide or aluminum hydroxide, wherein the aluminum content in the material obtained after mixing the additives is required to be 10-30% in terms of the percentage of the mass of aluminum oxide; and sintering the material obtained after mixing the additives to obtain a steelmaking slag-forming promoter.
[0007] In one embodiment, the additive includes a scarring material containing aluminum oxide or aluminum hydroxide.
[0008] In one embodiment, the particle size of the crushed material obtained after the crushing process is less than 30 mm.
[0009] In one embodiment, sintering the material obtained after mixing the additives comprises: using a rotary kiln to sinter the material obtained after mixing the additives, wherein the sintering temperature range of the rotary kiln is 700-900°C.
[0010] Another aspect of the present invention relates to a steelmaking slag-forming accelerator produced by the above method, characterized in that it comprises the following components in weight percentage: fluoride 13-30%; Al2O3 8-26%; SiO2 0.5-3%; MgO 1.5-26%; CaO 0.5-12%.
[0011] In one embodiment, the steelmaking slag-forming promoter further comprises the following components in weight percentage: 0%<C<2%; 0%<N<0.5%; 0%<S<0.3%.
[0012] The steelmaking slag-forming accelerator of the present invention is made from the sorted aluminum electrolytic cell overhaul slag residue, which is crushed and sieved, combined with other additives, and sintered in a rotary kiln to form granular, powdery, and spherical (round, elliptical, and oblate) products. The slag-forming accelerator is used as a steelmaking slag-forming accelerator. After being mixed with other raw materials to form a slag-forming agent, it is used for deoxidation, desulfurization, and slag-forming in molten steel.
[0013] The solution of the present application can recycle and comprehensively utilize the overhaul slag of aluminum electrolytic cells. It treats the overhaul slag harmlessly, fundamentally eliminates the potential pollution risks, and achieves multiple goals such as turning waste into treasure and protecting the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] The embodiments of the present invention are further described below with reference to the accompanying drawings, in which:
[0015] Figure 1 A method for producing a slag accelerator for steelmaking using aluminum electrolytic cell overhaul slag according to one embodiment is shown;
[0016] Figure 2 A partial schematic diagram of a production device for producing a slag-forming accelerator for steelmaking using aluminum electrolytic cell overhaul slag according to one embodiment is shown. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below through specific embodiments in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0018] Figure 1 A method for producing a steelmaking slag accelerator using aluminum electrolysis cell overhaul slag according to an embodiment is shown, and mainly comprises the following steps:
[0019] Step 101: sorting the aluminum electrolytic cell overhaul slag to separate silicon nitride combined with silicon carbide side blocks, waste cathode steel rods and waste cathodes.
[0020] The overhaul slag produced during the overhaul of aluminum electrolytic cells mainly includes waste cathode steel bars, silicon nitride combined with silicon carbide side blocks, waste cathodes, anti-seepage materials, and others (mainly including: paste, ceramic fiberboard, calcium silicate board, refractory bricks, high-strength castables, etc.).
[0021] Since the components of aluminum electrolytic cell overhaul slag are complex and the economic value and recycling methods of various components vary greatly, the method first sorts the aluminum electrolytic cell overhaul slag to sort out silicon nitride combined with silicon carbide side blocks, waste cathode steel rods and waste cathodes. In one embodiment, in addition to sorting out silicon nitride combined with silicon carbide side blocks, waste cathode steel rods and waste cathodes, other components can also be sorted out.
[0022] In one embodiment, the sorting and processing operation may include: (1) protective cleaning of the silicon nitride bonded silicon carbide side blocks during the planing process. The complete silicon nitride bonded silicon carbide side blocks can be recycled and reused, for example, for tank overhaul or online minor repair. The damaged silicon nitride bonded silicon carbide side blocks can be sold after cleaning; (2) picking out the waste cathode steel bars and waste cathodes. The waste cathodes can be made into carburizers for sale or used in other comprehensive utilization methods. The waste cathode carbon blocks in the overhaul slag account for more than 30% of the total slag. The cathode carbon blocks contain fixed carbon and have a certain calorific value, which can be fully utilized. They can be added to the alumina clinker kiln to replace part of the anthracite. The waste cathode carbon blocks can also be used in the sintering process of alumina. By crushing the waste carbon blocks to less than 25 mm and entering the alumina production process together with the anthracite, the dissolution conditions can be improved. They can also be crushed and added to the cement clinker to replace part of the fuel. It can also be used as a raw material for preparing ferroalloy electrode paste. The cathode carbon block has good conductivity and can replace part of the metallurgical coke to prepare electrode paste after being crushed to a certain particle size.
[0023] Step 102: After the sorting process, the remaining materials in the aluminum electrolysis cell overhaul slag are crushed to obtain crushed materials.
[0024] After sorting, the remaining materials in the aluminum electrolytic cell overhaul slag can be used as raw materials for producing steelmaking slag accelerators, and they are crushed to obtain scraps.
[0025] In one embodiment, the particle size of the crushed material obtained after the crushing process is 30 mm or less. In one embodiment, the particle size of the crushed material obtained after the crushing process is 20 mm or less.
[0026] In one embodiment, the crushing process is followed by a screening process to obtain crushed materials with a particle size of less than 30 mm or less than 20 mm.
[0027] Step 103: mixing additives into the crushed material, wherein the additives include aluminum oxide or aluminum hydroxide.
[0028] After the crushing process, an additive is mixed into the aluminum electrolytic cell overhaul slag fragments, wherein the additive includes aluminum oxide or aluminum hydroxide. The additive may be, for example, aluminum oxide, aluminum hydroxide, a scab material containing aluminum oxide or aluminum hydroxide, or a mixture of two or more thereof.
[0029] In one embodiment, the additive is a scaling material containing alumina or aluminum hydroxide. Since scaling materials containing alumina or aluminum hydroxide are generally produced in the alumina production process, using them as additives can greatly save costs and improve the comprehensive utilization efficiency of solid waste.
[0030] In one embodiment, the aluminum content in the material obtained after mixing the crushed material with the additive is required to be 10-30% (calculated as the percentage of aluminum oxide mass).
[0031] Step 104: Sintering the material obtained after mixing the additives to obtain a steelmaking slag-forming accelerator.
[0032] The mixed materials are sintered in a rotary kiln to prepare a steelmaking slag accelerator. In one embodiment, the sintering temperature of the rotary kiln can range from 700 to 900° C. Preferably, the sintering temperature of the rotary kiln can range from 800 to 850° C.
[0033] The main components of the steelmaking slag accelerator made by rotary kiln sintering include: fluoride (such as AlF3·xNaF) 13-30%; Al2O3 8-26%; SiO2 0.5-3%; MgO 1.5-26%; CaO 0.5-12%, all in weight percentage. In one embodiment, the main components of the steelmaking slag accelerator include: fluoride (such as AlF3·xNaF) 13-30%; Al2O3 8-26%; SiO2 0.5-3%; MgO 1.5-26%; CaO 0.5-12%; C < 2%; N < 0.5%; S < 0.3%.
[0034] The steelmaking slag accelerator made by rotary kiln sintering can be made into powder (particle size range 0-3mm), granular (particle size range 3-5mm), spherical (round sphere, ellipsoidal sphere, oblate sphere, particle size range 10-50mm) products, which are used as steelmaking slag accelerator. After being mixed with other raw materials to form a slag-forming agent, it is used for deoxidation, desulfurization and slag-forming in molten steel.
[0035] In one embodiment, the steelmaking slag-forming promoter is made of the residue after sorting of the overhaul slag of aluminum electrolytic cells (the residue after sorting of silicon nitride combined with silicon carbide side blocks, waste cathode steel bars and waste cathodes, etc.) as raw materials, which is crushed and then added with alumina scarring material in a certain proportion and mixed evenly. It has the characteristics of low cost, rapid slag formation, and resource recycling of industrial solid waste. It can promote rapid slag formation and improve the deoxidation and dephosphorization effects of the steelmaking process.
[0036] Figure 2 A partial schematic diagram of a production device for producing a steelmaking slag accelerator using aluminum electrolytic cell overhaul slag according to one embodiment is shown. Figure 2 In the process, the feed belt transports the crushed materials and additives to the feed silo and vertical preheater, after which the crushed materials and additives enter the rotary kiln body for sintering. The steelmaking slag accelerator obtained after sintering then passes through the vertical cooler and the discharge belt in turn to the discharge silo.
[0037] The solution of the present application can recycle and comprehensively utilize the overhaul slag of aluminum electrolytic cells. It treats the overhaul slag harmlessly, fundamentally eliminates the potential pollution risks, and achieves multiple goals such as turning waste into treasure and protecting the environment.
[0038] References herein to "various embodiments", "some embodiments", "one embodiment", or "an embodiment" refer to specific features, structures, or properties described in conjunction with the embodiments being included in at least one embodiment. Therefore, the phrases "in various embodiments", "in some embodiments", "in one embodiment", or "in an embodiment" appearing throughout the present invention do not necessarily refer to the same embodiment. In addition, specific features, structures, or properties may be combined in any suitable manner in one or more embodiments. Therefore, specific features, structures, or properties shown or described in conjunction with one embodiment may be combined in whole or in part with features, structures, or properties of one or more other embodiments without restriction, as long as the combination is not illogical or inoperable. Expressions similar to "according to A", "based on A", "through A", or "using A" appearing herein are intended to be non-exclusive, that is, "according to A" may include "according to A only" or "according to A and B", unless it is specifically stated that its meaning is "according to A only". In this application, for the sake of clarity, some exemplary operating steps are described in a certain order, but those skilled in the art will understand that each of these operating steps is not essential, and some of the steps may be omitted or replaced by other steps. These operation steps do not have to be executed sequentially in the manner shown; on the contrary, some of these operation steps can be executed in different orders or in parallel according to actual needs, as long as the new execution manner is not illogical or inoperable.
[0039] Having thus described several aspects of at least one embodiment of the present invention, it will be appreciated that various changes, modifications and improvements will readily occur to those skilled in the art. Such changes, modifications and improvements are intended to be within the spirit and scope of the present invention. Although the present invention has been described by way of some embodiments, the present invention is not limited to the embodiments described herein, and also includes various changes and variations made without departing from the scope of the present invention.
Claims
1. A method for producing a steelmaking slag accelerator, comprising: Sorting of aluminum electrolytic cell overhaul slag to separate silicon nitride-bonded silicon carbide side blocks, spent cathode steel rods and spent cathodes; After the sorting process, the remaining materials in the aluminum electrolytic cell overhaul slag are crushed to obtain crushed materials, wherein the remaining materials include anti-seepage materials, pastes, ceramic fiber boards, calcium silicate boards, refractory bricks, and high-strength castables; Adding additives to the crushed material, wherein the additives include a scab material containing aluminum oxide or aluminum hydroxide, wherein the aluminum content of the material obtained after adding the additives is required to be 10-30% in terms of the percentage of the mass of aluminum oxide; and The material obtained after mixing the additives is sintered to obtain a steelmaking slag-making accelerator, wherein the steelmaking slag-making accelerator includes the following components in weight percentage: fluoride 13-30%; Al2O3 8-26%; SiO2 0.5-3%; MgO 1.5-26%; CaO 0.5-12%.
2. The method according to claim 1, wherein: The particle size of the crushed material obtained after the crushing process is less than 30 mm.
3. The method according to claim 1, wherein: The sintering of the material obtained after mixing the additives comprises: The material obtained after mixing the additives is sintered using a rotary kiln, wherein the sintering temperature range of the rotary kiln is 700-900°C.
4. A steelmaking slag accelerator produced by the method according to any one of claims 1 to 3, characterized in that: It includes the following components in percentage by weight: fluoride 13-30%; Al2O3 8-26%; SiO2 0.5-3%; MgO 1.5-26%; CaO 0.5-12%.
5. The steelmaking slag-forming accelerator according to claim 4, further comprising the following components in weight percentage: 0%<C<2%; 0%<N<0.5%; 0%<S<0.3%.