A cold-rolled high-strength steel for enamel and its manufacturing method
By adding a small amount of titanium and rare earth elements to enamel steel and optimizing the alloy element ratio, the problems of water inlet blockage and poor enamel wettability caused by high Ti content have been solved, resulting in low-cost, high-strength enamel steel suitable for electric water heater inner tanks.
Patent Information
- Application Number
- CN202310032928.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-01-10
AI Technical Summary
The high Ti content in existing enamel steels leads to nozzle blockage and poor enamel wettability. The expensive alloying elements increase costs and affect welding performance, and there is also a problem with insufficient enamel adhesion.
Using low-carbon steel as the base, a small amount of titanium and rare earth elements are added, supplemented with copper, chromium, nickel, etc., and the proportion of alloying elements is controlled to form a diffusely distributed second phase particle, optimize the morphology of inclusions, and improve the anti-scaling and adhesion properties of the steel plate.
It achieves low-cost, high-strength enamel steel with good formability and anti-scaling properties, ensuring stable steel plate strength after high-temperature enamel firing, and is suitable for thin-gauge electric water heater inner tanks.
Smart Images

Figure CN118326242B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a metallic material and its manufacturing method, and more particularly to a steel for enamel and its manufacturing method. Background Technology
[0002] Enameled products are a composite material formed by coating a layer of inorganic vitreous ceramic enamel onto the surface of a molded steel plate and then sintering it at high temperatures. They possess excellent structural strength, corrosion resistance, wear resistance, and high-temperature resistance, and are widely used in light industry, home appliances, building decoration, environmental protection, petrochemicals, and pharmaceuticals. Mechanical strength, molding performance, and coating performance are the most critical technical indicators in the production of enamel products.
[0003] Driven by economic costs, energy conservation, environmental protection, and high safety performance, cold-rolled high-strength steel for enamel is receiving increasing attention and importance from the enamel industry. On the one hand, the application of high-strength steel can reduce the thickness of the steel plate, thereby reducing the weight of the product and achieving the goals of reducing material costs and saving enamel firing energy. On the other hand, the steel plate maintains a high yield strength after high-temperature enamel firing at 830-890℃, which can avoid the risk of surface enamel peeling due to large elastic or plastic deformation caused by compressive stress, thus improving the safety performance and service life of the product.
[0004] Chinese patent document CN112941418 A, entitled "A Cold-Rolled High-Strength Steel for Enamel and Its Preparation Method," discloses an enamel steel with the following elemental composition (wt%): C: 0.005-0.03%, Si≤0.03%, Mn: 0.2-0.5%, S≤0.006%, P≤0.012%, Alt≤0.05%, Nb: 0.01-0.03%, Ti: 0.05-0.20%, N: 0.005-0.012%; wherein Ti≥3.42N+4C, and the balance is iron and unavoidable impurities. It mainly employs a Nb and Ti composite microalloying method to improve both the strength and anti-scaling properties of the steel plate. However, the Ti content in this enamel steel is as high as 0.05-0.20%. On the one hand, Ti oxides continuously deposit on the inner wall of the nozzle during casting, forming nodules that easily cause nozzle blockage and reduce the number of consecutive casting furnaces. On the other hand, the higher the Ti content, the easier it is to form TiO2 at high temperatures. This oxide adheres to the surface of the steel plate, hindering the wetting and erosion of the steel plate by the enamel during high-temperature firing, and reducing the adhesion strength of the enamel plate.
[0005] Chinese patent document CN111945060A, entitled "Manufacturing Method of Cold-Rolled High-Strength Heat-Resistant Enamel Steel," discloses a method for manufacturing cold-rolled high-strength heat-resistant enamel steel. The elemental composition (wt%) of this enamel steel is: C: 0.04-0.07%, Si≤0.03%, Mn: 0.40-0.80%, P≤0.025%, S≤0.020%, Alt≤0.030%, Cr: 0.15-0.40%, Mo: 0.05-0.15%, N: 0.004-0.010%, with the balance being Fe and unavoidable trace elements. To improve the strength of the steel plate, a high content of precious alloying elements such as Cr and Mo is added. This not only increases the cost of the steel plate but also increases crack susceptibility, negatively impacting weldability. Furthermore, it easily forms a dense oxide film on the steel plate surface, affecting the adhesion of the enamel. Summary of the Invention
[0006] One of the objectives of this invention is to provide a low-carbon, rare-earth-enameled cold-rolled steel for enamel, which is inexpensive and has certain strength, resistance to high-temperature enameling softening, good formability, anti-scaling properties, and adhesion properties, making it suitable for producing thin-gauge electric water heater inner tanks.
[0007] To achieve the above objectives, the present invention provides a cold-rolled high-strength steel for enamel, which contains Fe and unavoidable impurities, and further contains the following chemical elements in the following mass percentages:
[0008] C: 0.03-0.08%, Si: 0.01-0.04%, Mn: 0.15-0.35%, S: 0.002-0.012%, Al: 0.015-0.055%, N≤0.006%, Ti: 0.02-0.05%, RE: 0.005-0.015%, 0<Ca≤0.008%, 0<Zr≤0.008%, and containing at least one of Cu: 0.01-0.06%, Cr: 0.01-0.05%, and Ni: 0.005-0.05%; the cold-rolled high-strength steel for enamel does not contain Nb and B elements.
[0009] Accordingly, the present invention also provides a cold-rolled high-strength steel for enamel, wherein the mass percentage of each chemical element is as follows:
[0010] C: 0.03-0.08%, Si: 0.01-0.04%, Mn: 0.15-0.35%, S: 0.002-0.012%, Al: 0.015-0.055%, N≤0.006%, Ti: 0.02-0.05%, RE: 0.005-0.015%, 0<Ca≤0.008%, 0<Zr≤0.008%, and containing at least one of Cu: 0.01-0.06%, Cr: 0.01-0.05% and Ni: 0.005-0.05%; the balance being Fe and other unavoidable impurities.
[0011] This invention presents a low-alloy, high-strength cold-rolled enamel steel that differs from existing technologies that primarily employ Nb and B alloying. Instead, it adds small amounts of titanium and rare earth elements to a low-carbon steel base, along with copper, chromium, and nickel to enhance enamel density, and trace amounts of calcium and zirconium to improve the steel's plasticity. The addition of small amounts of titanium primarily forms dispersed second-phase particles with carbon, nitrogen, and sulfur. These particles act as effective hydrogen traps, improving the steel's resistance to scabbing. Furthermore, they dissolve into the matrix during high-temperature scabbing and precipitate as finer, more dispersed particles during subsequent cooling, maintaining a high yield strength after high-temperature sintering. Rare earth elements mainly combine with sulfur to form rare earth sulfides, which not only improve the morphology of sulfides and enhance the steel's transverse properties but also further improve its resistance to scabbing. This invention, through reasonable alloy element design and process control, obtains a microstructure of fine and uniform ferrite with a small amount of pearlite, achieves a dispersed distribution of precipitates, ensures that the steel plate has high strength and plasticity, and at the same time has sufficient hydrogen trapping, good adhesion and anti-pinhole properties.
[0012] Specifically, the composition design principle of the cold-rolled high-strength steel for enamel used in this invention is as follows:
[0013] Carbon: C is the most basic strengthening element in steel. The higher the content, the higher the strength of the steel plate, but the lower the plasticity and toughness. For enamel steel, in addition to affecting mechanical properties, C is directly related to the steel plate's resistance to blistering and pinhole defects. Dispersed cementite and carbides in the steel plate are beneficial to its resistance to blistering. However, if the cementite content is too high, it will decompose into a large amount of CO gas during high-temperature enameling. The excessively large bubble diameter easily forms pinhole defects on the surface of the enamel layer, affecting the surface quality and corrosion resistance of the product. Therefore, this invention limits the C content in cold-rolled enamel steel to 0.03-0.08%.
[0014] Silicon (Si) plays a role in solid solution strengthening in steel. As a reactive element, a certain thickness of SiO2 oxide film inevitably forms on the surface of steel plates in the air. An appropriate amount of SiO2 oxide film promotes adhesion between the steel plate and the enamel, but an excessively thick SiO2 oxide film hinders the exchange of iron ions with enamel ions. Therefore, this invention limits the Si content in cold-rolled enamel steel to 0.01-0.04%.
[0015] Manganese (Mn) is also a common steel strengthening element, playing a role in solid solution strengthening. Mn is also a good deoxidizer and desulfurizer; however, the resulting MnS inclusions are easily elongated into a spindle shape at high temperatures, causing significant anisotropy in the steel's properties. In this technical solution, the addition of appropriate amounts of rare earth elements (RE) and titanium elements forms a composite sulfide of rare earth and titanium with strong resistance to plastic deformation, which can significantly improve the transverse mechanical properties of the steel. Excessive Mn content can also affect the formability and adhesion properties of the steel. Therefore, this invention limits the Mn content in cold-rolled enamel steel to 0.15-0.35%.
[0016] Sulfur: S is a harmful element in general-purpose steel, usually existing as MnS, but this inclusion affects the steel's transverse properties. In this technical solution, appropriate amounts of strong sulfide-forming elements such as Ti and RE are added. By controlling the proportions, sulfides with suitable morphology and size are formed, while simultaneously improving the toughness and anti-scaling properties of the steel plate. Therefore, this invention limits the S content in cold-rolled enamel steel to 0.002-0.012%.
[0017] Aluminum (Al) is added to steel as a deoxidizer, reacting with oxygen (O) to form Al₂O₃. This removes oxygen from the steel during oxygen blowing smelting, preventing the formation of numerous other oxide inclusions, which helps refine the grains and improve the steel's workability. Al also fixes nitrogen (N) in the steel, reducing the aging of the steel plate. If the Al content is too high, the steel plate is prone to blistering defects and decreased adhesion strength after enamel coating. Therefore, this invention limits the Al content in cold-rolled enamel steel to 0.015-0.055%.
[0018] Nitrogen: Nitrogen dissolved in steel can cause aging and reduce the elongation at break of the steel plate. Therefore, in this technical solution, adding an appropriate amount of Ti can fix all the N into TiN particles, which not only improves the anti-scaling performance of the steel plate but also avoids the aging caused by dissolved N. Therefore, the N content must be strictly controlled. This invention limits the N content in cold-rolled enamel steel to ≤0.006%.
[0019] Titanium (Ti) is a reactive element in steel, forming compounds with O, N, S, and C in that order of affinity. These compounds exert their effects through formation, dissolution, and precipitation within the steel. In this technical solution, to fully utilize the promoting effects of Ti-containing compounds on the strength, anti-scaling properties, and adhesion of the steel plate, the Ti content must be strictly controlled. This is because: at high temperatures, Ti initially forms TiO2 with O, but excessive TiO2 precipitates should be avoided. On the one hand, this worsens the castability of the molten steel and causes severe nozzle blockage; on the other hand, excessive TiO2 hinders the wetting of the enamel onto the steel plate during high-temperature enameling, reducing adhesion strength. Furthermore, Ti in steel forms dispersed TiN, TiS, and TiC particles. On one hand, these particles themselves have a certain adsorption effect on hydrogen atoms, and after cold deformation, tiny pores are formed around the particles, which can store hydrogen generated during pickling and enameling. On the other hand, these particles play a role in precipitation strengthening, improving the yield strength and resistance to high-temperature softening of the steel plate. In addition, these particles can also prevent the coarsening of austenite grains in the overheated zone under welding thermal cycling, improving the mechanical strength of the welded joint. However, excessive Ti content leads to the formation of coarse TiN, TiS, and TiC particles, which not only impairs the formability of the steel plate but also has limited improvement on the strength, anti-scaling properties, and weldability of the steel plate. Therefore, this invention limits the Ti content in cold-rolled enamel steel to 0.02-0.05%.
[0020] Rare earth elements (RE) are an element added in this technical solution, serving three beneficial purposes: First, RE has a strong affinity for sulfur (S), reducing the amount and further deformation of harmful inclusions (MnS), thus achieving a spheroidizing effect and significantly weakening the anisotropy of the steel plate. Second, the addition of rare earth elements increases the number of inclusions per unit volume without increasing the total amount of inclusions, meaning it refines inclusions and improves their dispersion. The finer and more dispersed the inclusions, the more pronounced the precipitation strengthening effect, while also strongly inhibiting hydrogen diffusion, effectively improving the steel plate's resistance to blistering. Third, the addition of rare earth elements can also refine grains, while simultaneously improving the strength and plasticity of the steel plate. Therefore, this invention limits the RE content in cold-rolled enamel steel to 0.005-0.015%.
[0021] Calcium: Trace amounts of calcium (Ca) form stable high-melting-point inclusions (CaO and CaS) in steel, generally distributed in circular or polygonal shapes. Sulfides such as MnS attach to these inclusions, nucleating and growing in a similar morphology. Therefore, Ca plays a role in improving the morphology of inclusions, thereby enhancing the mechanical properties of the steel plate. Improper control of the Ca content not only fails to achieve the desired metallurgical effect but also damages the steel's casting properties. Therefore, this invention limits the Ca content in cold-rolled enamel steel to 0 < Ca ≤ 0.008%.
[0022] Zirconium: Trace amounts of Zr also play a role in steel by transforming elongated MnS into nearly ductile spherical sulfides, thus improving the plasticity and toughness of the steel sheet. This invention limits the Zr content in cold-rolled enamel steel to 0 < Zr ≤ 0.008%.
[0023] Copper, chromium, and nickel: When the content of these elements is properly controlled, they can all promote the chemical reaction and interdiffusion of iron ions and enamel ions in the steel plate, improving the adhesion between the steel plate and the enamel layer. In addition, Ni can also inhibit hydrogen diffusion and improve anti-scaling performance. If the content is too high, it will increase the cost of the alloy and be detrimental to the adhesion performance. Therefore, this invention limits the content of Cu, Cr, and Ni in cold-rolled enamel steel to 0.01-0.06%, 0.01-0.05%, and 0.005-0.05%, respectively.
[0024] Furthermore, in the cold-rolled high-strength steel for enamel described in this invention, the mass percentage content of RE and S also satisfies: RE / S = 1-3.
[0025] In this invention, the mass percentage of rare earth elements (RE / S) is important for the formability of steel. When RE / S < 1, S mainly exists in the form of elongated strip-shaped MnS, which seriously impairs the transverse properties of the steel plate. When RE / S > 3, excessive rare earth elements will lead to an increase in the total amount of inclusions or excessive size, thus limiting the improvement of the plasticity and anti-scaling properties of the steel plate. Therefore, controlling RE / S between 1 and 3 plays a role in controlling the transformation of MnS morphology, reducing the number of elongated strip-shaped MnS inclusions in the steel, generating beneficial rare earth composite sulfides, and reducing the anisotropy of the steel plate.
[0026] Furthermore, in the cold-rolled high-strength steel for enamel described in this invention, it also satisfies: 6×Ti / (3.43×N+1.5×S-0.32×RE+4×C)≤1; where each chemical element is represented by the value before the percentage sign of its mass percentage content.
[0027] This formula is designed to further ensure that the titanium compounds are distributed in a fine and dispersed state, thereby improving the steel plate's resistance to blistering, strength, and plasticity.
[0028] Furthermore, in the cold-rolled high-strength steel for enamel described in this invention, among the unavoidable impurities, P ≤ 0.03% and O ≤ 0.005%.
[0029] The unavoidable impurities in this invention are mainly P and O. Specifically:
[0030] Phosphorus: P increases the cold brittleness of steel, especially at low temperatures. Cold brittleness worsens processing and welding properties, so the lower the P content, the better. Therefore, this invention limits the P content in cold-rolled enamel steel to ≤0.03%.
[0031] Oxygen: During smelting, oxygen blowing mainly serves to decarburize. Therefore, a certain amount of oxygen inevitably remains in the molten steel. If the O content is higher, the number and size of titanium and rare earth oxide inclusions formed will be larger, which will seriously impair the formability of the steel plate. Moreover, these oxides accumulate on the surface of the steel plate, changing the surface properties of the steel plate and thus affecting the enameling performance of the steel plate. Therefore, this invention limits the O content in cold-rolled enamel steel to ≤0.005%.
[0032] Furthermore, the microstructure of the cold-rolled high-strength steel for enamel described in this invention is ferrite + a small amount of pearlite, wherein the volume ratio of pearlite is less than 6%, and the pearlite is distributed at the triple grain boundaries of ferrite. The ferrite matrix is also distributed with composite sulfides of Ti and RE and Ti precipitates.
[0033] Furthermore, the composite sulfides of Ti and RE are spherical or elliptical (Ti,Mn)S and (RE,Mn)S with dimensions of 2-20 μm and a transverse / longitudinal dimension ratio of 0.8-2.
[0034] Furthermore, the Ti precipitates include Ti(C,N), TiC, and Ti4C2S2, with sizes ranging from 1 to 300 nm.
[0035] Furthermore, the ferrite grain size is 9-10.
[0036] Furthermore, the cold-rolled high-strength steel for enamel used in this invention meets the following performance requirements: yield strength ≥ 280 MPa, tensile strength ≥ 340 MPa, elongation at break of 30-40% at a gauge length of 50 mm, anisotropy index Δr ≤ 0.45, and hydrogen penetration value TH2 ≥ 7.0 min / mm. 2 .
[0037] Furthermore, after being fired at 850℃ for 10 minutes, its yield strength can still be maintained above 270MPa.
[0038] Another object of the present invention is to provide a method for manufacturing cold-rolled high-strength steel for enamel as described above.
[0039] To achieve the above objectives, the present invention provides a method for manufacturing cold-rolled high-strength steel for enamel, comprising the following steps:
[0040] (1) Smelting, refining and continuous casting;
[0041] (2) Hot charging and hot delivery into the insulation pit to reduce billet heating time and energy consumption, simplify the production process and improve the production pace;
[0042] (3) Heating of the billet;
[0043] (4) Hot rolling and coiling;
[0044] (5) Pickling;
[0045] (6) Cold rolling: Control the cold rolling reduction rate to 60-80%;
[0046] (7) Continuous annealing: the soaking temperature is 750-860℃, the soaking time is 100-300s, the over-aging temperature is 300-420℃, and the over-aging time is 200-400s;
[0047] (8) Flat.
[0048] This invention controls the cold rolling reduction rate between 60-80% because the cold rolling reduction rate affects the size of recrystallized grains. The higher the reduction rate, the more nucleation sites there are for ferrite recrystallization, making it easier to form fine, uniform equiaxed ferrite. If the reduction is too low, the above objective will not be achieved; if it is too high, the degree of microstructure hardening will be high, increasing the load on the cold rolling equipment.
[0049] Furthermore, the present invention employs a reasonable annealing process to: 1) ensure the recrystallization and growth of ferrite grains, resulting in uniform and fine ferrite grains, while simultaneously improving the strength and plasticity of the steel plate; 2) guarantee the full development of the {111} recrystallization texture to enhance the stamping performance of the steel plate; and 3) allow titanium compounds such as TiC and TiS particles to partially dissolve and precipitate during annealing, which serves as precipitation strengthening and also improves resistance to scale breakage.
[0050] Furthermore, in step (3) of the manufacturing method described in this invention, the heating temperature is 1120-1200℃ and the holding time is ≥240min.
[0051] The setting of heating temperature and holding time for continuously cast billets is to ensure that the alloy composition and carbonitrides in the billets are fully dissolved and diffused, resulting in a uniform and fine austenitic structure. If the temperature is too low or the holding time is too short, the austenitic composition inhomogeneity will be inherited to the finished product structure, leading to severe segregation and impaired mechanical properties. If the temperature is too high or the holding time is too long, the continuously cast billets will undergo decarburization or oxidation, resulting in coarse austenitic grains, wasting energy and materials, and negatively impacting the performance of the finished steel plate.
[0052] Furthermore, in step (4) of the manufacturing method described in this invention, the final rolling temperature of hot rolling is controlled to be 780-920°C, and the coiling temperature is controlled to be 620-700°C.
[0053] The final rolling temperature of hot rolling is controlled between 780-920℃ in order to obtain sufficient deformation in the austenite before it crystallizes, in order to prepare for grain refinement, and at the same time to avoid rolling in the two-phase region to form a mixed-grain structure, which would result in uneven mechanical properties of the hot-rolled plate.
[0054] In addition, after hot rolling, the steel sheet is cooled to between 620-700°C by a laminar flow cooling system before being coiled, in order to ensure the formability of the steel sheet and the full release of the second phase particles.
[0055] Furthermore, in step (8) of the manufacturing method described in this invention, the leveling reduction rate is controlled to be 0.8-2.0%.
[0056] This invention controls the flattening reduction rate to 0.8-2.0%. On the one hand, it can slow down or eliminate the yield plateau of low alloy steel and improve the stamping performance of the steel plate. On the other hand, it can control the surface roughness of the steel plate and increase the bonding between the steel plate and the enamel.
[0057] The cold-rolled high-strength steel for enamel as described in this invention has the following characteristics and beneficial effects:
[0058] The cold-rolled high-strength steel for enamel described in this invention adopts a low-cost alloy design and a simple and easy-to-control manufacturing process, resulting in enamel steel with excellent formability, superior anti-scaling performance, and good adhesion. It also solves the problem of low strength of steel plates used in enamel inner tanks of electric water heaters, and meets the requirement of high rigidity for enamel inner tanks.
[0059] The cold-rolled high-strength steel for enamel described in this invention optimizes the morphology and distribution of harmful inclusions MnS by adding a small amount of rare earth elements and controlling the RE / S ratio and the contents of Ca and Zr. This significantly improves the formability of the enamel steel and enhances its resistance to scale breakage, while reducing the amount of Ti microalloying element, which plays a crucial role in resisting scale breakage. The Ti mass percentage is controlled at 0.02-0.05%, which reduces problems such as poor castability and poor adhesion of steel plates caused by excessive Ti content, and also lowers alloy costs.
[0060] This invention fully utilizes the formation, dissolution, and precipitation characteristics of Ti compounds during high-temperature heating, high-temperature winding, and continuous high-temperature rapid annealing processes. Ultimately, it achieves the uniform precipitation of fine, dispersed Ti(C,N), TiC, and Ti4C2S2 on a ferrite matrix. This not only plays a crucial role in counteracting scaling by acting as a hydrogen storage trap, but also strengthens the steel by precipitation and inhibits grain growth during enamel firing. This improves the yield strength and resistance to high-temperature softening of the steel plate, resulting in minimal strength change after high-temperature enamel firing. It is suitable for preparing large-volume enamel liners with high fatigue resistance requirements.
[0061] Based on this, the present invention can achieve: yield strength ≥280MPa, tensile strength ≥340MPa, elongation at break of 30-40% with a gauge length of 50mm, anisotropy index Δr ≤0.45, and hydrogen penetration value TH2 ≥7.0min / mm. 2Furthermore, after being fired at 850℃ for 10 minutes, its yield strength can still be maintained above 270MPa. Attached Figure Description
[0062] Figure 1 The metallographic microstructure of the cold-rolled high-strength steel for enamel in Example A1.
[0063] Figure 2 The metallographic microstructure of the cold-rolled high-strength steel for enamel in Example A1 after simulated high-temperature enamel firing is shown. Detailed Implementation
[0064] The following will further explain and illustrate the cold-rolled high-strength steel for enamel and its manufacturing method according to the present invention with reference to specific embodiments and accompanying drawings. However, this explanation and illustration do not constitute an undue limitation on the technical solution of the present invention.
[0065] Examples A1-A6 and Comparative Examples B1-B2
[0066] Table 1 lists the mass percentage of each chemical element in the cold-rolled high-strength steel for enamel in Examples A1-A6 and Comparative Examples B1-B2.
[0067] Table 1. (wt%, balance Fe and other unavoidable impurities besides O and P)
[0068]
[0069] Note: In Table 1, I = 6 × Ti / (3.43 × N + 1.5 × S - 0.32 × RE + 4 × C) ≤ 1; each chemical element in the formula should be replaced with the value before the percentage sign of its mass percentage content.
[0070] The cold-rolled high-strength steel for enamel in Embodiments A1-A6 and the steel plates in Comparative Examples B1-B2 of the present invention were obtained by the following steps:
[0071] 1) Hot metal pretreatment;
[0072] 2) Converter smelting: Through top and bottom combined blowing, carbon reduction, dephosphorization, removal of harmful gases and inclusions are achieved, and the basic composition of molten steel is adjusted.
[0073] 3) RH refining: Under vacuum conditions, deep decarburization, deoxidation, and desulfurization are carried out to further remove inclusions and harmful gases such as hydrogen and nitrogen from the molten steel, so as to achieve precise control of the mass percentage of each chemical element in Table 1 and to achieve morphological control of inclusions.
[0074] 4) Continuous casting: The molten steel is made into a 230mm thick continuous casting billet;
[0075] 5) The continuously cast billet is directly hot-charged and hot-transported to the heat preservation pit using roller conveyors;
[0076] 6) Billet heating: The billet heating temperature is 1120-1200℃, the holding time is more than 240 minutes, and the uniform temperature of the continuously cast billet after exiting the furnace is ≤20℃;
[0077] 7) Hot rolling: The final rolling temperature is 780-920℃. The steel plate is cooled to the coiling temperature by a laminar flow cooling system and then coiled. The coiling temperature is 620-700℃.
[0078] 8) Pickling to remove iron oxide scale from the surface of the steel plate.
[0079] 9) Cold rolling: The cold rolling reduction rate is 60-80%.
[0080] 10) Continuous annealing: The soaking temperature is 750-860℃, the soaking time is 100-300s, the over-aging temperature is 300-420℃, and the over-aging time is 200-400s.
[0081] 11) Smoothing: Smoothing elongation rate is 0.8-2.0%.
[0082] Tables 2-1 and 2-2 list the specific process parameters for the cold-rolled high-strength steel for enamel in Examples A1-A6 and the steel plates in Comparative Examples B1-B2.
[0083] Table 2-1.
[0084]
[0085]
[0086] Table 2-2.
[0087]
[0088] It should be noted that the over-aging temperature changes during actual operation and is not stable at a fixed value. Instead, the temperature gradually decreases during the over-aging period. Therefore, the over-aging temperatures in Table 2-2 are presented as a range of values rather than point values in each embodiment and comparative example.
[0089] The cold-rolled high-strength steel for enamel application in Examples A1-A6 and the steel plates in Comparative Examples B1-B2 underwent various performance tests, which are listed in Table 3. The transverse mechanical properties at room temperature for Examples A1-A6 and Comparative Examples B1-B2 include the yield strength R. eL Tensile strength R m Elongation at break A 50mm And the anisotropy index Δr.
[0090] In addition, Table 3 lists the hydrogen penetration time of steel plates measured by the electrochemical method specified in BS EN10209, and then converted into the hydrogen permeability value TH2 corresponding to a 1 mm thick steel plate.
[0091] Examples A1-A6 and Comparative Examples B1-B2 were placed in a resistance heating furnace at 850°C and held for 10 minutes to simulate a high-temperature sintering test. They were then removed and air-cooled to room temperature. The yield strength of the samples after high-temperature sintering was tested, and the results are listed in Table 3.
[0092] Table 3.
[0093]
[0094]
[0095] As can be seen from Tables 1 and 3, the transverse yield strength of Examples A1-A6 at room temperature is between 283-346 MPa, the tensile strength is between 347-306 MPa, the elongation at break is between 31.3-38.9%, the anisotropy index is controlled below 0.42, and the hydrogen penetration value TH2 ≥ 7 min / mm 2 After being fired at 850℃ for 10 minutes, the yield strength remained above 270MPa, and the decrease in yield strength was controlled within 15MPa.
[0096] This demonstrates that the cold-rolled enamel steel described in this invention has low anisotropy, which is beneficial for improving the stamping uniformity of the steel sheet and reducing the material loss rate. Furthermore, it possesses excellent hydrogen storage performance, ensuring that no scaling or cracking occurs after double-sided or single-sided enamel coating; and it maintains a high yield strength even after high-temperature simulated enamel firing, which is highly beneficial for improving the fatigue resistance and service life of the enamel liner.
[0097] In contrast, the comparative examples B1-B2 exhibited low transverse tensile strength, significant anisotropy, and a marked decrease in yield strength after enameling. Furthermore, the hydrogen storage capacity of the comparative examples was also insufficient.
[0098] Figure 1 The metallographic microstructure of Example A1 is shown. It can be seen that the microstructure of the steel plate is uniform ferrite grains with a small amount of pearlite. The pearlite is located at the three-pronged grain boundaries of the ferrite grains. The ferrite matrix is also distributed with composite sulfides of Ti and RE and Ti precipitates.
[0099] In various embodiments of the present invention, the ferrite is fine, and the ferrite grain size is 9-10.
[0100] In various embodiments of the present invention, the composite sulfides of Ti and RE are circular or elliptical (Ti,Mn)S and (RE,Mn)S with dimensions of 2-20 μm and a cross-sectional area ratio of 0.8-2. The Ti precipitates include Ti(C,N), TiC, and Ti4C2S2, with dimensions between 1-300 nm.
[0101] Figure 2 The metallographic microstructure of Example A1 after simulated high-temperature sintering is shown. It can be seen that the ferrite grains grew uniformly, with the average grain size increasing from 12.0 μm to 14.0 μm, and no abnormal growth occurred.
[0102] It should be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made thereto are those that can be directly derived or easily conceived by those skilled in the art from the content disclosed in the present invention, and should all fall within the protection scope of the present invention.
Claims
1. A cold-rolled high-strength steel for enamel, characterized in that, Its mass percentage of each chemical element is as follows: C: 0.03-0.08%, Si: 0.01-0.04%, Mn: 0.15-0.35%, S: 0.002-0.012%, Al: 0.015-0.055%, N≤0.006%, Ti: 0.02-0.05%, RE: 0.005-0.015%, 0<Ca≤0.008%, 0<Zr≤0.008%, and containing at least one of Cu: 0.01-0.06%, Cr: 0.01-0.05%, and Ni: 0.005-0.05%; the balance being Fe and other unavoidable impurities. The mass percentages of RE and S also satisfy: RE / S = 1 - 3; It also satisfies: 6×Ti / (3.43×N+1.5×S-0.32×RE+4×C)≤1; where each chemical element is represented by the value before the percentage sign of its mass percentage content.
2. The cold-rolled high-strength steel for enamel as described in claim 1, characterized in that, In unavoidable impurities, P ≤ 0.03% and O ≤ 0.005%.
3. The cold-rolled high-strength steel for enamel as described in claim 1, characterized in that, Its microstructure consists of ferrite and pearlite, with the volume ratio of pearlite being less than 6%. Pearlite is distributed at the three-pronged grain boundaries of ferrite. The ferrite matrix also contains composite sulfides of Ti and RE, as well as Ti precipitates.
4. The cold-rolled high-strength steel for enamel as described in claim 3, characterized in that, The Ti and RE complex sulfides are spherical or elliptical (Ti,Mn)S and (RE,Mn)S, with sizes ranging from 2 to 20 mm. m, with a width / width ratio of 0.8-2.
5. The cold-rolled high-strength steel for enamel as described in claim 3, characterized in that, Ti precipitates include Ti(C,N), TiC, and Ti4C2S2, with sizes ranging from 1 to 300 nm.
6. The cold-rolled high-strength steel for enamel as described in claim 3, characterized in that, The ferrite grain size is 9-10.
7. The cold-rolled high-strength steel for enamel as described in claim 1, characterized in that, Its performance meets the following requirements: yield strength ≥ 280 MPa, tensile strength ≥ 340 MPa, elongation at break of 30-40% with a gauge length of 50 mm, and anisotropy index. ≤0.45, hydrogen penetration value TH2≥7.0min / mm 2 .
8. A method for manufacturing cold-rolled high-strength steel for enamel as described in any one of claims 1-7, characterized in that, Including the following steps: (1) Smelting, refining and continuous casting; (2) Hot loading and hot delivery into the insulation pit; (3) Heating of the billet; (4) Hot rolling and coiling; (5) Pickling; (6) Cold rolling: Control the cold rolling reduction rate to 60-80%; (7) Continuous annealing: the soaking temperature is 750-860℃, the soaking time is 100-300s, the over-aging temperature is 300-420℃, and the over-aging time is 200-400s; (8) Flat.
9. The manufacturing method as described in claim 8, characterized in that, In step (3), the heating temperature is 1120-1200℃ and the holding time is ≥240min.
10. The manufacturing method as described in claim 8, characterized in that, In step (4), the final rolling temperature of hot rolling is controlled at 780-920℃, and the coiling temperature is controlled at 620-700℃.
11. The manufacturing method as described in claim 8, characterized in that, In step (8), the leveling reduction rate is controlled to be 0.8-2.0%.
Citation Information
Patent Citations
Manufacturing method for cold-rolled high-strength heat-resistant enameled steel
CN111945060A
High-strength steel for cold-rolled enamel and preparation method of high-strength steel
CN112941418A
Hot rolling high strength steel plate for two-sided porcelain enamel and manufacturing method thereof
CN101353758A
High strength steel plate used for enamel liners and manufacturing method thereof
CN103510011A