Injection ferrite preparation process and injection ferrite magnet
By using ferrite magnetic powder and nylon-6 to mix and granulate in the injection molded ferrite preparation process, and pre-burn powder with iron scales and strontium carbonate, the environmental protection problem of thermosetting resin adhesive is solved and improved Magnetic performance and easy installation, achieving efficient and environmentally friendly injection molded ferrite preparation.
Patent Information
- Application Number
- CN202410597524.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-14
AI Technical Summary
The use of thermosetting resin adhesives in the existing injection molded ferrite preparation process contains toxic substances, which affects environmental protection and lacks magnetic properties.
The magnets are prepared by mixing ferrite magnetic powder and nylon-6 in a granulator to reduce the use of thermosetting resins. The clinker pre-burned powder of iron scales and strontium carbonate is used as raw materials, and the installation ring, moving block and extrusion are provided. Structures such as pressing screws improve magnetic performance and facilitate installation.
The environmentally friendly preparation of injection molded ferrite is achieved, which improves the residual magnetism, intrinsic coercive force and maximum magnetic energy production, enhances the comprehensive performance of injection molded ferrite, and simplifies the installation process.
Smart Images

Figure CN118335508B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ferrite, in particular to an injection-molded ferrite preparation process and an injection-molded ferrite magnet. Background Art
[0002] Ferrite is a metal oxide with ferromagnetism, which can be generally divided into three types: permanent ferrite, soft ferrite and gyromagnetic ferrite. In terms of electrical properties, the resistivity of ferrite is much greater than that of metal and alloy magnetic materials, and it also has higher dielectric properties. The magnetic properties of ferrite are also manifested in its higher magnetic permeability at high frequencies. Therefore, ferrite has become a widely used non-metallic magnetic material in the field of high-frequency weak electricity.
[0003] For example, an injection-molded permanent magnet ferrite material, an injection-molded magnet and a preparation method thereof with announcement number CN11292788U and announcement date 2021.06.08 are characterized in that they are mainly prepared from the following raw materials, by weight: 82 to 92 parts of ferrite powder, 6 to 16 parts of polymer matrix, 0.4 to 1 part of auxiliary agent, 0.1 to 2 parts of coupling agent, and 0.1 to 1 part of lubricant; wherein the polymer matrix is at least one of acrylonitrile-styrene-acrylic rubber resin and acrylonitrile-ethylene propylene diene monomer rubber-styrene resin; the auxiliary agent is at least one of 2-(2-hydroxy-5-methylphenyl) benzotriazole, hindered amines and benzotriazoles.
[0004] The above-mentioned and prior art injection molded ferrites are usually prepared using thermosetting resin adhesives. The use of thermosetting resin adhesives requires curing treatment during the preparation of injection molded ferrites. The curing agent is mostly toxic and will cause harm to the atmosphere and the surrounding environment, which is not environmentally friendly. Therefore, it is urgent to design an injection molded ferrite preparation process and an injection molded ferrite magnet to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide an injection molded ferrite preparation process and an injection molded ferrite magnet to solve the above-mentioned deficiencies in the prior art.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A process for preparing injection-molded ferrite comprises the following steps:
[0008] Iron scale powder: 20-40 parts; strontium carbonate powder: 10-60 parts; water: 23-53 parts; red iron oxide: 10-40 parts; barium carbonate: 3-11 parts; silane coupling agent: 1-7 parts; dispersant: 1-6 parts; nylon-6: 10-20 parts; toughening and reinforcing agent: 1-7 parts; defoaming agent: 1-7 parts; lubricant: 1-9 parts;
[0009] S1. Preparation of ferrite magnetic powder:
[0010] a: uniformly mixing iron scale powder and strontium carbonate powder to obtain an added mixed material;
[0011] b: the mixed material in a is mixed with water to form a ball, and then pre-burned to obtain a clinker pre-burned material, and then the pre-burned material is crushed to obtain a clinker pre-burned powder;
[0012] c: Mix red iron oxide and barium carbonate according to the molar ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture;
[0013] d: then the clinker pre-burned powder in b is mixed with the raw material mixture added in c to obtain ferrite raw material, and then the ferrite raw material is pre-burned to obtain ferrite raw material;
[0014] e: crushing and grinding the ferrite raw material, and then sieving to obtain ferrite magnetic powder;
[0015] S2, adding ferrite magnetic powder, silane coupling agent and dispersant into the interior of a mixing device for powder mixing;
[0016] S3, adding nylon-6 to the mixed powder obtained in S2, and continuing to mix;
[0017] S4, adding a toughening agent, a defoaming agent and a lubricant to the mixture obtained in S3, and heating and mixing;
[0018] S5, injecting the mixed material obtained in S4 into the interior of a granulator for granulation;
[0019] S6. The obtained pellets are placed in an injection molding machine and heated to melt to give them good fluidity. The pellets are injected into a metal mold with a magnetic field in a molten state while flowing. The metal mold is cooled to form the required magnet body.
[0020] Furthermore, the dispersant is sodium metaphosphate, sodium phosphate or sodium tripolyphosphate, and the toughening and reinforcing agent is one of a silicon-based toughening agent, an acrylic impact modifier, and a thermoplastic elastomer TPE, and the lubricant is zinc stearate, calcium stearate, EBS or silicone oil.
[0021] Furthermore, in b of S1, the ratio of water to mixed material is 1.6:1.
[0022] Furthermore, in step b of S1, the pre-burning temperature is 1200-1280°C, and the pre-burning time is 50-60 min.
[0023] Furthermore, in said S1 e, the particle size of the obtained ferrite magnetic powder is 1.6-1.7 μm.
[0024] Furthermore, the mixing conditions in S2 are: the temperature is 100-120°C, and the mixing time is 20-30 minutes. After adding nylon-6 in S3, the mixing is continued at a temperature of 100-120°C for 20-30 minutes.
[0025] Furthermore, in S4, the specific steps of heating and mixing are: first continue mixing at a temperature of 100-120°C for 15-20 minutes, then increase the temperature to 140-160°C and continue mixing.
[0026] An injection molded ferrite magnet includes the injection molded ferrite preparation process, a magnet body and a seesaw, a mounting ring is provided on the inner wall of the magnet body, and a moving block 1 and a moving block 2 are respectively slidably connected inside the mounting ring, plug blocks are provided on the outer walls of the moving block 1 and the moving block 2, and a triangular block is integrally connected to the outer wall of the moving block 1, an extrusion screw is threadedly inserted into the top of the mounting ring, and an extrusion block is provided at the bottom end of the extrusion screw, the extrusion block is in contact with the triangular block, a center rod is provided on the inner walls of the bottom and top of the mounting ring, and the seesaw is rotatably sleeved on the outside of the center rod, and both ends of the moving block 1 are in contact with the seesaw.
[0027] Furthermore, a guide rod is provided on the inner wall of the mounting ring, and the moving block 1 and the moving block 2 are both slidably sleeved on the outside of the guide rod. Springs connected to the moving block 1 and the moving block 2 are respectively provided on the inner wall of the mounting ring, and the springs are sleeved on the outside of the guide rod.
[0028] Furthermore, a limiting rod is arranged on the inner wall of the mounting ring, and the second moving block is slidably sleeved on the outside of the limiting rod.
[0029] In the above technical scheme, the injection molded ferrite preparation process and the injection molded ferrite magnet provided by the present invention, (1) by using ferrite magnetic powder and nylon-6 in a granulator to mix and granulate the magnet, no thermosetting resin is used, thereby reducing the use of curing agent, and no large amount of toxic substances are released, which is more environmentally friendly to the atmosphere and the surrounding environment; (2) the injection molded ferrite uses iron scale and strontium carbonate clinker pre-sintered powder as raw materials, so that the prepared injection molded ferrite has high remanence, intrinsic coercive force and maximum magnetic energy product, effectively improving the comprehensive performance of the injection molded ferrite; ( 3) By setting the mounting ring, moving block 1, plug-in block, triangular block, extrusion screw and extrusion block, rotating the extrusion screw can drive the extrusion block to squeeze the triangular block, the triangular block will push the moving block 1 to move, the moving block 1 will squeeze one end of the seesaw, and the other end of the seesaw will push the moving block 2 to move, so that the plug-in blocks on the moving block 1 and the moving block 2 can be moved out from the inside of the mounting ring and can be plugged into the mounting rod that needs to be installed, thereby realizing the function of easy installation, and the guide rod can guide the moving block 1 and the moving block 2, and can prevent the moving block 1 and the moving block 2 from offset when moving. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.
[0031] Figure 1 A schematic diagram of the preparation process structure of the injection molded ferrite preparation process and the injection molded ferrite magnet embodiment of the present invention.
[0032] Figure 2 A schematic diagram of the three-dimensional structure of a magnet body provided for the injection molded ferrite preparation process and the injection molded ferrite magnet embodiment of the present invention.
[0033] Figure 3 A schematic diagram of the internal structure of a magnet body provided by the injection molded ferrite preparation process and the injection molded ferrite magnet embodiment of the present invention.
[0034] Figure 4 The present invention is a front view schematic diagram of the internal structure of the magnet body provided by the injection molded ferrite preparation process and the injection molded ferrite magnet embodiment of the present invention.
[0035] Description of reference numerals:
[0036] 1. Magnet body; 2. Mounting ring; 3. Moving block 1; 4. Insert block; 5. Triangular block; 6. Extrusion screw; 7. Extrusion block; 8. Guide rod; 9. Spring; 10. Center rod; 11. Rocker; 12. Moving block 2; 13. Limit rod. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.
[0038] like Figure 1-4 As shown, the injection molded ferrite preparation process provided by the embodiment of the present invention includes the following preparation steps:
[0039] Iron scale powder: 22 parts; strontium carbonate powder: 11 parts; water: 25 parts; red iron oxide: 12 parts; barium carbonate: 5 parts; silane coupling agent: 1 part; dispersant: 6 parts; nylon-6: 11 parts; toughening and reinforcing agent: 2 parts; defoaming agent: 2 parts; lubricant: 3 parts;
[0040] S1. Preparation of ferrite magnetic powder:
[0041] a: uniformly mixing iron scale powder and strontium carbonate powder to obtain an added mixed material;
[0042] b: The mixture in a is mixed with water to form a ball, the ratio of water to the mixture is 1.6:1, and then pre-burned to obtain a clinker pre-burned material, the pre-burning temperature is: 1200°C, the pre-burning time is 50min, and then the pre-burned material is crushed to obtain a clinker pre-burned powder;
[0043] c: Mix red iron oxide and barium carbonate according to the molar ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture;
[0044] d: then the clinker pre-burned powder in b is mixed with the raw material mixture added in c to obtain ferrite raw material, and then the ferrite raw material is pre-burned to obtain ferrite raw material;
[0045] e: crushing and grinding the ferrite raw material, and then sieving to obtain ferrite magnetic powder, the particle size of the ferrite magnetic powder is 1.6 μm;
[0046] S2, adding ferrite magnetic powder, silane coupling agent and dispersant into the interior of a mixing device for mixing, the temperature is 100°C, and the mixing time is 20min;
[0047] S3, adding nylon-6 to the mixed powder obtained in S2, and continuing to mix at a temperature of 100° C. for 20 min;
[0048] S4, adding a toughening agent, a defoaming agent and a lubricant to the mixture obtained in S3, heating and mixing, first continuing to mix at a temperature of 100° C. for 15 min, then raising the temperature to 140° C. and continuing to mix for 15 min;
[0049] S5, injecting the mixed material obtained in S4 into the interior of a granulator for granulation;
[0050] S6. The obtained pellets are placed in an injection molding machine and heated to melt to give them good fluidity. The pellets are injected into a metal mold having a magnetic field in a molten state while flowing. The metal mold is cooled to form the required magnet body 1.
[0051] The injection molded ferrite preparation process provided by the present invention comprises the following preparation steps:
[0052] Iron scale powder: 21 parts; strontium carbonate powder: 21 parts; water: 23 parts; red iron oxide: 13 parts; barium carbonate: 3 parts; silane coupling agent: 1 part; dispersant: 2 parts; nylon-6: 10 parts; toughening and reinforcing agent: 2 parts; defoaming agent: 2 parts; lubricant: 2 parts;
[0053] S1. Preparation of ferrite magnetic powder:
[0054] a: uniformly mixing iron scale powder and strontium carbonate powder to obtain an added mixed material;
[0055] b: The mixture in a is mixed with water to form a ball, the ratio of water to the mixture is 1.6:1, and then pre-burned to obtain a clinker pre-burned material, the pre-burning temperature is: 1200°C, the pre-burning time is 50min, and then the pre-burned material is crushed to obtain a clinker pre-burned powder;
[0056] c: Mix red iron oxide and barium carbonate according to the molar ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture;
[0057] d: then the clinker pre-burned powder in b is mixed with the raw material mixture added in c to obtain ferrite raw material, and then the ferrite raw material is pre-burned to obtain ferrite raw material;
[0058] e: crushing and grinding the ferrite raw material, and then sieving to obtain ferrite magnetic powder, the particle size of the ferrite magnetic powder is 1.6 μm;
[0059] S2, adding ferrite magnetic powder, silane coupling agent and dispersant into the interior of a mixing device for mixing, the temperature is 100°C, and the mixing time is 20-30min;
[0060] S3, adding nylon-6 to the mixed powder obtained in S2, and continuing to mix at a temperature of 100° C. for 20 min;
[0061] S4, adding a toughening agent, a defoaming agent and a lubricant to the mixture obtained in S3, heating and mixing, first continuing to mix at a temperature of 100° C. for 15 min, then raising the temperature to 140° C. and continuing to mix for 15 min;
[0062] S5, injecting the mixed material obtained in S4 into the interior of a granulator for granulation;
[0063] S6. The obtained pellets are placed in an injection molding machine and heated to melt to give them good fluidity. The pellets are injected into a metal mold having a magnetic field in a molten state while flowing. The metal mold is cooled to form the required magnet body 1.
[0064] In one embodiment provided by the present invention, the dispersant is sodium metaphosphate, sodium phosphate or sodium tripolyphosphate, and the toughening and reinforcing agent is one of a silicone toughening agent, an acrylic impact modifier, and a thermoplastic elastomer TPE, and the lubricant is zinc stearate, calcium stearate, EBS or silicone oil.
[0065] The injection molded ferrite magnet includes the injection molded ferrite preparation process, and also includes a magnet body 1 and a seesaw 11. A mounting ring 2 is arranged on the inner wall of the magnet body 1, and the interior of the mounting ring 2 is respectively slidably connected with a moving block 1 3 and a moving block 2 12, and an insert block 4 is arranged on the outer wall of the moving block 1 3 and the moving block 2 12, and a triangular block 5 is integrally connected to the outer wall of the moving block 1 3, and an extrusion screw 6 is inserted into the top thread of the mounting ring 2, and an extrusion block 7 is arranged at the bottom end of the extrusion screw 6, and the extrusion block 7 is in contact with the triangular block 5, and the bottom of the mounting ring 2 is in contact with the top A center rod 10 is provided on the inner wall, and a seesaw 11 is rotatably sleeved on the outside of the center rod 10, both ends of the moving block 3 are in contact with the seesaw 11, and rotating the extrusion screw 6 can drive the extrusion block 7 to squeeze the triangular block 5, and the triangular block 5 will push the moving block 3 to move, and the moving block 13 will squeeze one end of the seesaw 11, and the other end of the seesaw 11 will push the moving block 2 12 to move, so that the moving block 13 and the plug-in block 4 on the moving block 2 12 can be moved out from the inside of the mounting ring 2, and can be plugged into the mounting rod that needs to be installed, thereby realizing the function of easy installation.
[0066] In an embodiment provided by the present invention, a guide rod 8 is provided on the inner wall of the mounting ring 2, and the moving block 1 3 and the moving block 2 12 are both slidably sleeved on the outside of the guide rod 8, and springs 9 connected to the moving block 1 3 and the moving block 2 12 are respectively provided on the inner wall of the mounting ring 2, and the springs 9 are sleeved on the outside of the guide rod 8, and the tension of the springs 9 can pull the moving block 1 3 and the moving block 2 12 to move.
[0067] In another embodiment provided by the present invention, a limiting rod 13 is provided on the inner wall of the mounting ring 2 , and the second moving block 12 is slidably sleeved on the outside of the limiting rod 13 , and the limiting rod 13 can limit and guide the second moving block 12 .
[0068] Embodiment 1
[0069] The injection molding ferrite preparation process includes the following preparation steps:
[0070] Iron scale powder: 21 parts; strontium carbonate powder: 21 parts; water: 23 parts; red iron oxide: 13 parts; barium carbonate: 3 parts; silane coupling agent: 1 part; dispersant: 2 parts; nylon-6: 10 parts; toughening and reinforcing agent: 2 parts; defoaming agent: 2 parts; lubricant: 2 parts;
[0071] S1. Preparation of ferrite magnetic powder:
[0072] a: uniformly mixing iron scale powder and strontium carbonate powder to obtain an added mixed material;
[0073] b: The mixture in a is mixed with water to form a ball, the ratio of water to the mixture is 1.6:1, and then pre-burned to obtain a clinker pre-burned material, the pre-burning temperature is: 1230°C, the pre-burning time is 53min, and then the pre-burned material is crushed to obtain a clinker pre-burned powder;
[0074] c: Mix red iron oxide and barium carbonate according to the molar ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture;
[0075] d: then the clinker pre-burned powder in b is mixed with the raw material mixture added in c to obtain ferrite raw material, and then the ferrite raw material is pre-burned to obtain ferrite raw material;
[0076] e: crushing and grinding the ferrite raw material, and then sieving to obtain ferrite magnetic powder, the particle size of the ferrite magnetic powder is 1.6 μm;
[0077] S2, adding ferrite magnetic powder, silane coupling agent and dispersant into the interior of a mixing device for mixing, the temperature is 110°C, and the mixing time is 23min;
[0078] S3, adding nylon-6 to the mixed powder obtained in S2, and continuing to mix at a temperature of 110° C. for 23 min;
[0079] S4, adding a toughening agent, a defoaming agent and a lubricant to the mixture obtained in S3, heating and mixing, first continuing to mix at a temperature of 110° C. for 16 min, then raising the temperature to 150° C. and continuing to mix for 17 min;
[0080] S5, injecting the mixed material obtained in S4 into the interior of a granulator for granulation;
[0081] S6. The obtained pellets are placed in an injection molding machine and heated to melt to give them good fluidity. The pellets are injected into a metal mold having a magnetic field in a molten state while flowing. The metal mold is cooled to form the required magnet body 1.
[0082] In one embodiment provided by the present invention, the dispersant is sodium metaphosphate, sodium phosphate or sodium tripolyphosphate, and the toughening and reinforcing agent is one of a silicone toughening agent, an acrylic impact modifier, and a thermoplastic elastomer TPE, and the lubricant is zinc stearate, calcium stearate, EBS or silicone oil.
[0083] The injection molded ferrite magnet includes the injection molded ferrite preparation process, and also includes a magnet body 1 and a seesaw 11. A mounting ring 2 is arranged on the inner wall of the magnet body 1, and the interior of the mounting ring 2 is respectively slidably connected with a moving block 1 3 and a moving block 2 12, and an insert block 4 is arranged on the outer wall of the moving block 1 3 and the moving block 2 12, and a triangular block 5 is integrally connected to the outer wall of the moving block 1 3, and an extrusion screw 6 is inserted into the top thread of the mounting ring 2, and an extrusion block 7 is arranged at the bottom end of the extrusion screw 6, and the extrusion block 7 is in contact with the triangular block 5, and the bottom of the mounting ring 2 is in contact with the top A center rod 10 is provided on the inner wall, and a seesaw 11 is rotatably sleeved on the outside of the center rod 10, both ends of the moving block 3 are in contact with the seesaw 11, and rotating the extrusion screw 6 can drive the extrusion block 7 to squeeze the triangular block 5, and the triangular block 5 will push the moving block 3 to move, and the moving block 13 will squeeze one end of the seesaw 11, and the other end of the seesaw 11 will push the moving block 2 12 to move, so that the moving block 13 and the plug-in block 4 on the moving block 2 12 can be moved out from the inside of the mounting ring 2, and can be plugged into the mounting rod that needs to be installed, thereby realizing the function of easy installation.
[0084] In an embodiment provided by the present invention, a guide rod 8 is provided on the inner wall of the mounting ring 2, and the moving block 1 3 and the moving block 2 12 are both slidably sleeved on the outside of the guide rod 8, and springs 9 connected to the moving block 1 3 and the moving block 2 12 are respectively provided on the inner wall of the mounting ring 2, and the springs 9 are sleeved on the outside of the guide rod 8, and the tension of the springs 9 can pull the moving block 1 3 and the moving block 2 12 to move.
[0085] In another embodiment provided by the present invention, a limiting rod 13 is provided on the inner wall of the mounting ring 2 , and the second moving block 12 is slidably sleeved on the outside of the limiting rod 13 , and the limiting rod 13 can limit and guide the second moving block 12 .
[0086] Embodiment 2
[0087] The injection molding ferrite preparation process includes the following preparation steps:
[0088] Iron scale powder: 20 parts; strontium carbonate powder: 18 parts; water: 24 parts; red iron oxide: 14 parts; barium carbonate: 4 parts; silane coupling agent: 1 part; dispersant: 2 parts; nylon-6: 13 parts; toughening and reinforcing agent: 1 part; defoaming agent: 2 parts; lubricant: 1 part;
[0089] S1. Preparation of ferrite magnetic powder:
[0090] a: uniformly mixing iron scale powder and strontium carbonate powder to obtain an added mixed material;
[0091] b: The mixture in a is mixed with water to form a ball, the ratio of water to the mixture is 1.6:1, and then pre-burned to obtain a clinker pre-burned material, the pre-burning temperature is: 1270°C, the pre-burning time is 56 minutes, and then the pre-burned material is crushed to obtain a clinker pre-burned powder;
[0092] c: Mix red iron oxide and barium carbonate according to the molar ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture;
[0093] d: then the clinker pre-burned powder in b is mixed with the raw material mixture added in c to obtain ferrite raw material, and then the ferrite raw material is pre-burned to obtain ferrite raw material;
[0094] e: crushing and grinding the ferrite raw material, and then sieving to obtain ferrite magnetic powder, the particle size of the ferrite magnetic powder is 1.7 μm;
[0095] S2, adding ferrite magnetic powder, silane coupling agent and dispersant into the interior of a mixing device for mixing, the temperature is 115 ° C, and the mixing time is 26 minutes;
[0096] S3, adding nylon-6 to the mixed powder obtained in S2, and continuing to mix at a temperature of 115° C. for 26 minutes;
[0097] S4, adding a toughening agent, a defoaming agent and a lubricant to the mixture obtained in S3, heating and mixing, first continuing to mix at a temperature of 115° C. for 18 min, then raising the temperature to 150° C. and continuing to mix for 19 min;
[0098] S5, injecting the mixed material obtained in S4 into the interior of a granulator for granulation;
[0099] S6. The obtained pellets are placed in an injection molding machine and heated to melt to give them good fluidity. The pellets are injected into a metal mold having a magnetic field in a molten state while flowing. The metal mold is cooled to form the required magnet body 1.
[0100] In one embodiment provided by the present invention, the dispersant is sodium metaphosphate, sodium phosphate or sodium tripolyphosphate, and the toughening and reinforcing agent is one of a silicone toughening agent, an acrylic impact modifier, and a thermoplastic elastomer TPE, and the lubricant is zinc stearate, calcium stearate, EBS or silicone oil.
[0101] The injection molded ferrite magnet comprises a magnet body 1 and a seesaw 11, a mounting ring 2 is arranged on the inner wall of the magnet body 1, and a moving block 3 and a moving block 12 are respectively slidably connected inside the mounting ring 2, an insert block 4 is arranged on the outer wall of the moving block 3 and the moving block 12, and a triangular block 5 is integrally connected to the outer wall of the moving block 3, an extrusion screw 6 is threadedly inserted at the top of the mounting ring 2, and an extrusion block 7 is arranged at the bottom end of the extrusion screw 6, and the extrusion block 7 is in contact with the triangular block 5, and a middle screw is arranged on the inner wall of the bottom and top of the mounting ring 2 The core rod 10, and the seesaw 11 are rotatably sleeved on the outside of the center rod 10, both ends of the moving block 3 are in contact with the seesaw 11, and rotating the extrusion screw 6 can drive the extrusion block 7 to squeeze the triangular block 5, and the triangular block 5 will push the moving block 3 to move, and the moving block 13 will squeeze one end of the seesaw 11, and the other end of the seesaw 11 will push the moving block 2 12 to move, so that the moving block 13 and the plug-in block 4 on the moving block 2 12 can be moved out from the inside of the mounting ring 2, and can be plugged into the mounting rod that needs to be installed, thereby realizing the function of easy installation.
[0102] In an embodiment provided by the present invention, a guide rod 8 is provided on the inner wall of the mounting ring 2, and the moving block 1 3 and the moving block 2 12 are both slidably sleeved on the outside of the guide rod 8, and springs 9 connected to the moving block 1 3 and the moving block 2 12 are respectively provided on the inner wall of the mounting ring 2, and the springs 9 are sleeved on the outside of the guide rod 8, and the tension of the springs 9 can pull the moving block 1 3 and the moving block 2 12 to move.
[0103] In another embodiment provided by the present invention, a limiting rod 13 is provided on the inner wall of the mounting ring 2 , and the second moving block 12 is slidably sleeved on the outside of the limiting rod 13 , and the limiting rod 13 can limit and guide the second moving block 12 .
[0104] Embodiment 3
[0105] The injection molding ferrite preparation process includes the following preparation steps:
[0106] Iron scale powder: 26 parts; strontium carbonate powder: 11 parts; water: 23 parts; red iron oxide: 12 parts; barium carbonate: 7 parts; silane coupling agent: 2 parts; dispersant: 1 part; nylon-6: 12 parts; toughening and reinforcing agent: 1 part; defoaming agent: 2 parts; lubricant: 3 parts;
[0107] S1. Preparation of ferrite magnetic powder:
[0108] a: uniformly mixing iron scale powder and strontium carbonate powder to obtain an added mixed material;
[0109] b: The mixture in a is mixed with water to form a ball, the ratio of water to the mixture is 1.6:1, and then pre-burned to obtain a clinker pre-burned material, the pre-burning temperature is: 1280°C, the pre-burning time is 60min, and then the pre-burned material is crushed to obtain a clinker pre-burned powder;
[0110] c: Mix red iron oxide and barium carbonate according to the molar ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture;
[0111] d: then the clinker pre-burned powder in b is mixed with the raw material mixture added in c to obtain ferrite raw material, and then the ferrite raw material is pre-burned to obtain ferrite raw material;
[0112] e: crushing and grinding the ferrite raw material, and then sieving to obtain ferrite magnetic powder, the particle size of the ferrite magnetic powder is 1.7 μm;
[0113] S2, adding ferrite magnetic powder, silane coupling agent and dispersant into the interior of a mixing device for mixing, the temperature is 120 ° C, and the mixing time is 30 minutes;
[0114] S3, adding nylon-6 to the mixed powder obtained in S2, and continuing to mix at a temperature of 120° C. for 30 min;
[0115] S4, adding a toughening agent, a defoaming agent and a lubricant to the mixture obtained in S3, heating and mixing, first continuing to mix at a temperature of 120° C. for 20 min, then raising the temperature to 160° C. and continuing to mix for 20 min;
[0116] S5, injecting the mixed material obtained in S4 into the interior of a granulator for granulation;
[0117] S6. The obtained pellets are placed in an injection molding machine and heated to melt to give them good fluidity. The pellets are injected into a metal mold having a magnetic field in a molten state while flowing. The metal mold is cooled to form the required magnet body 1.
[0118] In one embodiment provided by the present invention, the dispersant is sodium metaphosphate, sodium phosphate or sodium tripolyphosphate, and the toughening and reinforcing agent is one of a silicone toughening agent, an acrylic impact modifier, and a thermoplastic elastomer TPE, and the lubricant is zinc stearate, calcium stearate, EBS or silicone oil.
[0119] The injection molded ferrite magnet includes the injection molded ferrite preparation process, and also includes a magnet body 1 and a seesaw 11. A mounting ring 2 is arranged on the inner wall of the magnet body 1, and the interior of the mounting ring 2 is respectively slidably connected with a moving block 1 3 and a moving block 2 12, and an insert block 4 is arranged on the outer wall of the moving block 1 3 and the moving block 2 12, and a triangular block 5 is integrally connected to the outer wall of the moving block 1 3, and an extrusion screw 6 is inserted into the top thread of the mounting ring 2, and an extrusion block 7 is arranged at the bottom end of the extrusion screw 6, and the extrusion block 7 is in contact with the triangular block 5, and the bottom of the mounting ring 2 is in contact with the top A center rod 10 is provided on the inner wall, and a seesaw 11 is rotatably sleeved on the outside of the center rod 10, both ends of the moving block 3 are in contact with the seesaw 11, and rotating the extrusion screw 6 can drive the extrusion block 7 to squeeze the triangular block 5, and the triangular block 5 will push the moving block 3 to move, and the moving block 13 will squeeze one end of the seesaw 11, and the other end of the seesaw 11 will push the moving block 2 12 to move, so that the moving block 13 and the plug-in block 4 on the moving block 2 12 can be moved out from the inside of the mounting ring 2, and can be plugged into the mounting rod that needs to be installed, thereby realizing the function of easy installation.
[0120] In an embodiment provided by the present invention, a guide rod 8 is provided on the inner wall of the mounting ring 2, and the moving block 1 3 and the moving block 2 12 are both slidably sleeved on the outside of the guide rod 8, and springs 9 connected to the moving block 1 3 and the moving block 2 12 are respectively provided on the inner wall of the mounting ring 2, and the springs 9 are sleeved on the outside of the guide rod 8, and the tension of the springs 9 can pull the moving block 1 3 and the moving block 2 12 to move.
[0121] In another embodiment provided by the present invention, a limiting rod 13 is provided on the inner wall of the mounting ring 2 , and the second moving block 12 is slidably sleeved on the outside of the limiting rod 13 , and the limiting rod 13 can limit and guide the second moving block 12 .
[0122] Working principle: S1. Preparation of ferrite magnetic powder: a. Mix iron scale powder and strontium carbonate powder evenly to obtain an added mixture; b. Add water to the mixture in a to form a ball, the ratio of water to the mixture is 1.6:1, and then pre-burn to obtain a clinker pre-burned material, the pre-burning temperature is: 1200~1280°C, the pre-burning time is 50-60min, and then the pre-burned material is crushed to obtain a clinker pre-burned powder; c. Mix red iron oxide and barium carbonate according to a mol ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture; d: then the clinker pre-burned powder in b is mixed with the raw material mixture added to c to obtain a ferrite raw material, and then the ferrite raw material is pre-burned to obtain a ferrite raw material; e: the ferrite raw material is crushed and ground, and then sieved to obtain ferrite magnetic powder, the particle size of the ferrite magnetic powder is 1.6-1.7μm; S2, ferrite magnetic powder, silane coupling agent and dispersant are added to the inside of a mixing device for powder mixing, the temperature is 100-120°C, and the mixing time is 20-30min; S3, nylon-6 is added to the mixed powder obtained in S2, and mixing is continued, and mixing is carried out at a temperature of 100-120°C for 20-30min; S4, toughening and reinforcing agent, defoaming agent and lubricant are added to the mixture obtained in S3, and the temperature is increased and mixed, and mixing is continued at a temperature of 100-120°C. Mix for 15-20min, then increase the temperature to 140-160°C, and continue mixing for 15-20min; S5, inject the mixture obtained in S4 into the interior of the granulator for granulation; S6, put the obtained granules into the interior of the injection molding machine, heat and melt them to make them have good fluidity, and inject them into the interior of the metal mold with a magnetic field in a molten state while flowing, cool the metal mold, and form the required magnet body 1 after cooling. When it is necessary to install the injection molded ferrite magnet, rotating the extrusion screw 6 can drive the extrusion block 7 to extrude the triangular block 5, the triangular block 5 will push the moving block 1 3 to move, the moving block 1 3 will squeeze one end of the seesaw 11, and the other end of the seesaw 11 will push the moving block 2 12 to move, so that the moving block 1 3 and the plug-in block 4 on the moving block 2 12 can be removed from the interior of the mounting ring 2, and can be plugged into the mounting rod that needs to be installed, thereby realizing the function of easy installation.
[0123] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.
Claims
1. Injection molded ferrite magnet, characterized in that, The invention comprises a magnet body (1) and a seesaw (11), wherein a mounting ring (2) is arranged on the inner wall of the magnet body (1), and a moving block 1 (3) and a moving block 2 (12) are slidably connected inside the mounting ring (2), an insert block (4) is arranged on the outer wall of one side of the moving block 1 (3) and the moving block 2 (12), and a triangular block (5) is integrally connected to the outer wall of one side of the moving block 1 (3), an extrusion screw (6) is threadedly inserted at the top of the mounting ring (2), and an extrusion block (7) is arranged at the bottom end of the extrusion screw (6), and the extrusion block (7) is in contact with the triangular block (5), a center rod (10) is arranged on the inner wall of the bottom and top of the mounting ring (2), and the seesaw (11) is rotatably sleeved on the outside of the center rod (10), and both ends of the moving block 1 (3) are in contact with the seesaw (11); The magnet body (1) is prepared by the following preparation process, which includes the following preparation steps: Iron scale powder: 20-40 parts; Strontium carbonate powder: 10-60 parts; Water: 23-53 parts; Red iron oxide: 10-40 parts; Barium carbonate: 3-11 parts; Silane coupling agent: 1-7 parts; Dispersant: 1-6 parts; Nylon-6: 10-20 parts; Toughening and reinforcing agent: 1-7 parts; Defoaming agent: 1-7 parts; Lubricant: 1-9 parts; S1. Preparation of ferrite magnetic powder: a: uniformly mixing iron scale powder and strontium carbonate powder to obtain an added mixed material; b: the mixed material in a is mixed with water to form a ball, and then pre-burned to obtain a clinker pre-burned material, and then the pre-burned material is crushed to obtain a clinker pre-burned powder; c: Mix red iron oxide and barium carbonate according to the molar ratio : BaCO3 is 5.5-6.2 and mixed to obtain a raw material mixture; d: then the clinker pre-burned powder in b is mixed with the raw material mixture added in c to obtain ferrite raw material, and then the ferrite raw material is pre-burned to obtain ferrite raw material; e: crushing and grinding the ferrite raw material, and then sieving to obtain ferrite magnetic powder; S2, adding ferrite magnetic powder, silane coupling agent and dispersant into the interior of a mixing device for powder mixing; S3, adding nylon-6 to the mixed powder obtained in S2, and continuing to mix; S4, adding a toughening agent, a defoaming agent and a lubricant to the mixture obtained in S3, and heating and mixing; S5, injecting the mixed material obtained in S4 into the interior of a granulator for granulation; S6. The obtained pellets are placed in an injection molding machine and heated to melt to give them good fluidity. The pellets are injected into a metal mold having a magnetic field in a molten state while flowing. The metal mold is cooled to form the desired magnet body (1).
2. The injection molded ferrite magnet according to claim 1, characterized in that: The dispersant is sodium metaphosphate, sodium phosphate or sodium tripolyphosphate, the toughening and reinforcing agent is one of a silicon toughening agent, an acrylic impact modifier, and a thermoplastic elastomer TPE, and the lubricant is zinc stearate, calcium stearate, EBS or silicone oil.
3. The injection molded ferrite magnet according to claim 1, characterized in that: In b of S1, the ratio of water to mixed material is 1.6:
1.
4. The injection molded ferrite magnet according to claim 1, characterized in that: In b of S1, the pre-burning temperature is 1200-1280° C., and the pre-burning time is 50-60 min.
5. The injection molded ferrite magnet according to claim 1, characterized in that: In the step e of S1, the particle size of the obtained ferrite magnetic powder is 1.6-1.7 μm.
6. The injection molded ferrite magnet according to claim 1, characterized in that: The mixing conditions in S2 are: the temperature is 100-120°C, and the mixing time is 20-30 minutes. After adding nylon-6 in S3, the mixing is continued at a temperature of 100-120°C for 20-30 minutes.
7. The injection molded ferrite magnet according to claim 1, characterized in that: In S4, the specific steps of heating and mixing are: first continue mixing at a temperature of 100-120° C. for 15-20 minutes, then increase the temperature to 140-160° C. and continue mixing.
8. The injection molded ferrite magnet according to claim 7, characterized in that: A guide rod (8) is arranged on the inner wall of the mounting ring (2), and the first moving block (3) and the second moving block (12) are both slidably sleeved on the outside of the guide rod (8). Springs (9) connected to the first moving block (3) and the second moving block (12) are respectively arranged on the inner wall of the mounting ring (2), and the springs (9) are sleeved on the outside of the guide rod (8).
9. The injection molded ferrite magnet according to claim 8, characterized in that: A limiting rod (13) is provided on the inner wall of the mounting ring (2), and the second moving block (12) is slidably sleeved on the outside of the limiting rod (13).