Composite negative electrode material and preparation method thereof, secondary battery and electronic device

By attaching silicon-containing materials to the porous carbon support and optimizing process conditions, composite negative electrode materials are prepared, which solves the performance problems caused by volume expansion of silicon-based negative electrode materials, and achieves high cycle stability and rate performance of lithium-ion batteries, satisfying the satisfaction of Large-scale application requirements.

CN118335946BActive Publication Date: 2024-11-22SHANGHAI NANOMET TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410459664.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-11-22
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

The silicon-based anode material has poor circulation performance, low first-time efficiency and poor rate performance in lithium-ion batteries due to volume expansion, which cannot meet the needs of large-scale applications.

Method used

Using composite negative electrode material, the silicon-containing material is attached to the porous carbon support, and the flow rate, concentration of the silicon source gas, pressure, temperature and time in the reaction chamber can be controlled to achieve uniform distribution and surface coating of the silicon-containing material and the carbon framework. , optimize the ratio of powder compaction density to specific surface area of ​​composite materials, reduce the amount of internal closed pores, and improve particle strength and surface activity.

Benefits of technology

It significantly improves the cycle stability and rate performance of lithium-ion batteries, improves the battery's energy density and first-time efficiency, and extends the retention rate of battery capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118335946B_ABST
    Figure CN118335946B_ABST
Patent Text Reader

Abstract

The present invention provides a composite negative electrode material and a preparation method thereof, as well as a secondary battery and an electronic device. The 8T powder compaction density PD of the composite negative electrode material of the present application is g / cm 3 , and specific surface area B, in cm 3 / g, the ratio satisfies the following relationship: 0.01≤PD / B≤6; the composite negative electrode material provided by the present invention has low internal closed pores, and the cross-sectional SEM statistics show that the closed pore area accounts for less than 20% of the pore diameter greater than 100nm; the composite negative electrode material comprises a porous carbon carrier and a silicon-containing material attached to the porous carbon carrier; the composite negative electrode material has a high first efficiency of 80%-98% and a high theoretical capacity (500-2600mAh / g); the capacity ratio of the first lithium removal to 0.8V of the composite negative electrode material to the first lithium removal to 2.0V is Cap, wherein 80%≤Cap≤98%. This composite negative electrode material greatly improves the cycle stability and rate performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, in particular to the field of lithium-ion battery technology, and specifically to a composite negative electrode material and a preparation method thereof, as well as a secondary battery and an electronic device. Background Art

[0002] As the power of electrical equipment such as mobile phones, computers, electric vehicles, and energy storage power stations continues to increase, people's requirements for the energy density of lithium batteries are also increasing.

[0003] At present, silicon as the negative electrode material of lithium-ion batteries has a theoretical gram capacity of up to 4200mAh / g, which is much higher than the theoretical gram capacity of graphite, a commercial negative electrode material, 372mAh / g. Therefore, it is considered to be the next generation of negative electrode materials; the industry has begun to add silicon-based negative electrode materials to the negative electrode, which can significantly improve the energy density of the battery. However, silicon-based negative electrodes will undergo a huge volume expansion (300-400%) during the lithium insertion process, which greatly limits the promotion and popularization of this silicon-based negative electrode material. To solve this problem, silicon-carbon negative electrodes are the most promising materials in silicon-based negative electrodes; the current method is to deposit nano-silicon inside porous carbon and use the reserved gaps inside the porous carbon to reduce the expansion rate of the silicon negative electrode. However, during the charge and discharge process, the material particles are constantly expanding and contracting, resulting in the appearance of new electrolyte / active material interfaces on the particle surface. In particular, nano-silicon and the electrolyte have higher reactivity, which will continuously consume the electrolyte to form an unstable solid electrolyte membrane (SEI membrane), which can easily cause irreversible lithium consumption and deterioration of the conductive network, leading to rapid attenuation of battery capacity and deterioration of rate performance.

[0004] Existing technologies for improving silicon-carbon negative electrodes mainly focus on adjusting process parameters to reduce specific surface area, increase silicon content and initial efficiency, and cannot significantly improve battery cycle and rate performance; the present invention has found that the ratio of compaction density to specific surface area of ​​silicon-carbon negative electrode material powder and the internal pores of the particles are critical, and are closely related to particle structure strength and surface activity. Particle strength and surface activity have a great influence on electrolyte consumption and battery cycle and rate performance; the present invention has found that the gram capacity of 0.8V is critical, and this potential corresponds to the actual operating voltage and capacity of the full battery, which has a great influence on cycle performance, energy density and rate performance. Summary of the invention

[0005] Problems solved by the present invention: Although silicon material has high specific capacity, which is 10 times that of graphite, due to the large volume expansion of silicon, it leads to problems such as poor cycle performance, low initial efficiency, and poor rate performance, and currently cannot meet large-scale application needs. The present invention provides a composite negative electrode material with good cycle stability and excellent rate performance.

[0006] The invention provides a method for preparing a composite negative electrode material, which has a simple process and is suitable for industrial production.

[0007] The invention provides a lithium ion battery with excellent cycle and rate performance.

[0008] The invention provides an electronic device.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] The first aspect of the present invention provides a composite negative electrode material, which comprises a porous carbon carrier and a silicon-containing material attached to the porous carbon carrier, wherein the 8T powder compaction density of the composite negative electrode material is PD, in units of g / cm 3 , and specific surface area B, unit m 2 / g, the ratio satisfies the following relationship: 0.01≤PD / B≤6;

[0011] The composite negative electrode material provided by the present invention has low internal closed pores, and the area of ​​closed pores with a diameter greater than 100 nm in the SEM-CP photograph accounts for less than 20%. It has a high first efficiency of 80%-98%, a high theoretical capacity (500-2600mAh / g), and a high 0.8V capacity ratio.

[0012] In some embodiments, the 8T powder compaction density of the composite negative electrode material is PD, in g / cm 3 The specific surface area of ​​the composite negative electrode material after 8T powder compaction is B, unit m 2 / g, where 0.01≤PD / B≤6.

[0013] In some embodiments, a more preferred range is 0.1≤PD / B≤2.5; the greater the compaction density of the composite negative electrode material 8T, the smaller the specific surface area, and the greater the ratio of compaction density to specific surface area, indicating that the energy density of the composite material is higher. At the same time, the lower the specific surface area and the lower the reaction activity of the electrolyte, the higher the first efficiency and the better the cycle performance.

[0014] In some embodiments, the 8T powder compaction density of the composite negative electrode material is 0.6 g / cm 3 ≤PD g / cm 3 ≤1.5g / cm 3 When the compaction density of the composite negative electrode material is too high, it will affect its electrical performance at a high rate. When the compaction density of the composite negative electrode material is low, it is not conducive to improving the energy density of the secondary battery.

[0015] In some embodiments, the specific surface area of ​​the composite negative electrode material is 0.2 m 2 / g to 160m 2 / g.

[0016] The specific surface area of ​​the composite negative electrode material after compaction of 8T powder is 0.5m 2 / g to 180m 2 / g.

[0017] When the specific surface area BET of the composite negative electrode material is too high, the storage performance of the secondary battery may be at risk of deterioration. When the BET is too small, the kinetic performance of the secondary battery may be at risk of deterioration.

[0018] In some embodiments, the internal closed pore area of ​​the composite negative electrode material accounts for C, C≤20%, and the cross-section after ion cutting is observed by SEM. The closed pore area with a pore diameter greater than 100 nm in the particles on the cross-section accounts for C, C≤20%, C=(P / A)*100%, and the closed pore area is P, where P is the sum of the pore areas within the 100 nearest neighboring particles with a pore diameter d1>100 nm, and A is the sum of the areas of the 100 nearest neighboring particles; if C is too large, the particle strength is reduced, and the particles are easily broken during cold pressing and charging and discharging, thereby increasing the consumption of the electrolyte and posing a risk of deterioration in the cycle performance of the secondary battery.

[0019] In some embodiments, the mass proportion of silicon in the composite negative electrode material is X, and the range of X is: 10% ≤ X ≤ 60%. Increasing the mass content of silicon is conducive to improving the gram capacity and the first efficiency, thereby helping to improve the energy density of the secondary battery. However, when the silicon content is too high, there is a risk of reduced cycle performance and rate performance of the secondary battery. When the silicon content is too low, although it is conducive to improving the cycle and rate performance of the secondary battery, it is not conducive to improving the gram capacity and the first efficiency, and improving the energy density of the secondary battery.

[0020] In some embodiments, the mass proportion of carbon in the composite negative electrode material is Y, and the range of Y is: 30% ≤ Y ≤ 80%. The reduction in the mass content of carbon is conducive to the improvement of gram capacity and first efficiency, thereby helping to improve the energy density of the secondary battery. However, when the carbon content is too low, there is a risk of reduced cycle performance and rate performance of the secondary battery. When the carbon content is too high, although it is conducive to the improvement of the cycle and rate performance of the secondary battery, it is not conducive to the improvement of gram capacity and first efficiency, and the improvement of the energy density of the secondary battery.

[0021] In some embodiments, carbon-rich particles are present in the composite negative electrode material, and the carbon-rich particles refer to the carbon content data of the EDS analysis of the approximately 0.5 μm×0.5 μm area of ​​the particles selected when observing the cross section after ion cutting by SEM, which is higher than 50% of the carbon content test data; the carbon content test method is described later (Testing and Characterization of Powder and Pole Performance 8). Carbon-rich particles are beneficial to improving the conductivity of the composite negative electrode material. At the same time, since the high BET of carbon-rich particles is conducive to adsorbing excess electrolyte, it is also beneficial to increase ionic conductivity, which is beneficial to improving the battery cycle performance and rate performance of the composite negative electrode material;

[0022] In some embodiments, the Dv50 of the composite negative electrode material is 3 μm to 15 μm.

[0023] In some embodiments, the Dv99 of the composite negative electrode material is 6 μm to 30 μm.

[0024] In some embodiments, Dn10 of the composite negative electrode material is 0.5 μm to 5 μm.

[0025] If the particle size of the composite negative electrode material is too small, there is a risk that the BET of the composite negative electrode material will increase, thereby increasing the side reaction between the composite negative electrode material and the electrolyte, which is not conducive to the cycle performance of the secondary battery; if the particle size is too large, it will be not conducive to the rate performance of the secondary battery.

[0026] In some embodiments, the gram capacity of the composite negative electrode material is 600-2500 mAh / g, and the first efficiency is 80%-96%. High gram capacity and first efficiency are conducive to improving the energy density of the secondary battery;

[0027] In some embodiments, the ratio of the capacity of the composite negative electrode material at the first delithiation to 0.8V to the capacity at the first delithiation to 2.0V is Cap, wherein 80%≤Cap≤98%. Since the delithiation of 0.8V corresponds to a full battery discharge cut-off potential of 3.0V, the higher the capacity ratio of 0.8V, the higher the capacity of the full battery at 3.0V, which is more conducive to improving the energy density of the secondary battery in practical applications.

[0028] In some embodiments, the carbon Raman peak Id / Ig ratio of the composite negative electrode material is 0.05 to 1.3, and the silicon Raman peak Id / Ig ratio is 0.5 to 1.2. Too high or too low Raman peak ratios are not conducive to improving energy density or the cycle performance of secondary batteries.

[0029] In some embodiments, the porous carbon support of the composite negative electrode material has a BET of 200-4000 m 2 / g, pore volume is 0.1cc / g-2.0cc / g, and the pore volume corresponding to the pore size of 0.3-2nm accounts for more than 50%. Too low BET and pore volume can load less silicon-containing materials, and the improvement of gram capacity is not obvious, and the improvement of secondary battery energy density is not obvious. Too high BET and pore volume can load more silicon-containing materials, but there is a risk of reduced strength of particles, and there is a risk of rupture during the cold pressing process of the pole piece, which is not conducive to the improvement of secondary battery cycle performance. Too low 0.3-2nm pore size ratio is not conducive to the entry of silicon-containing materials into the pores, and silicon-containing materials are easily enriched on the surface, so there is a risk of reduced secondary battery cycle performance.

[0030] In some embodiments, the proportion of carbon in the porous carbon carrier of the composite negative electrode material is 85%-100%, the proportion of silicon is less than 5%, and the proportion of oxygen is 0.1%-15%. The appropriate proportion of silicon and oxygen in the carbon carrier is conducive to the entry of silicon-containing materials into the carbon carrier. Excessive proportions of silicon and oxygen are not conducive to improving the conductivity of the composite negative electrode material and have the risk of reducing rate performance.

[0031] In some embodiments, the porous carbon carrier testing method of the composite negative electrode material is to select particles with a cross-sectional diameter close to D50 when observing the cross-section after ion cutting with SEM, and select 5 EDS analysis carbon content data of approximately 0.5 μm×0.5 μm areas on the cross-section of the observed particles, and take the ratio of the maximum carbon content to the minimum carbon content as L, and the range of L is L<1.2; when the carbon content ratio L is in this range, it is the porous carbon carrier described in the present invention; the larger the L value, the worse the uniformity of the carbon distribution, which is not conducive to the stability of the particle structure and the improvement of electrical performance.

[0032] A second aspect of the present invention provides a method for preparing a composite negative electrode material, which comprises the following steps:

[0033] First, the silicon-containing material is attached to the porous carbon carrier, and then the carbon-containing material is coated. By controlling the flow rate, concentration, pressure, temperature and reaction time of the silicon source gas, the silicon-containing material and the carbon skeleton are evenly distributed, and the surface is effectively coated. This method is environmentally friendly, simple in process, and is conducive to the large-scale production of high-performance composite negative electrode materials;

[0034] P1: The reactor 1 equipped with the porous carbon carrier is heated to T1 and an inert gas is introduced, wherein T1 ranges from 390-650°C, and after being kept warm for 0h-4h, a silicon source gas and a diluent gas are introduced into the reaction chamber equipped with the porous carbon carrier to perform vapor deposition 1, wherein the deposition time is t1, and the range of t1 is 2h-36h, to obtain a composite negative electrode material intermediate 1 of deposited silicon material; the surface pressure 1 of the reaction chamber is 0.5kPa to 200kPa;

[0035] P2: Then, the reactor 1 is heated to T2, T2 ranges from 200°C to 750°C, and after being kept warm for ≤4h, a carbon source gas and a dilution gas are introduced into the reaction chamber of P1 to perform vapor deposition 2, and the deposition time is t2, t2 ranges from 0.5h to 24h, to obtain the composite negative electrode material intermediate 2; the surface pressure 2 of the reaction chamber is 0.5kPa to 200kPa;

[0036] P3: Then, the composite negative electrode material intermediate 2 is transferred to the reaction chamber of the reactor 2, and the temperature is raised to T3 and an inert gas is introduced, wherein the range of T3 is 300°C-750°C. After the temperature is kept at ≤4h, a carbon source gas and a dilution gas are introduced into the reaction chamber to perform vapor deposition 3, wherein the deposition time is t3 and the range of t3 is 1h-24h to obtain the composite negative electrode material; the surface pressure 3 of the reaction chamber is 0.1kPa to 100kPa.

[0037] In some embodiments, the silicon source gas in the P1 process includes at least one of monosilane, disilane, silicon vapor, trichlorosilane, and dichlorosilane; and the diluent gas includes at least one of hydrogen, argon, and nitrogen.

[0038] In some embodiments, in the P1 process, the gauge pressure 1 is 0.5 kPa to 25 kPa, in the P2 process, the gauge pressure 2 is 0.5 kPa to 25 kPa, and in the P3 process, the gauge pressure 3 is 0.5 kPa to 25 kPa.

[0039] When the gauge pressure is too low, such as during vapor deposition1, it is not easy for silicon-containing gas to enter the pores of the porous carbon carrier, which is not conducive to the uniform distribution of silicon-containing materials on the porous carbon carrier. When the gauge pressure is too high, it approaches or exceeds the pressure limit of some equipment accessories, which is not conducive to safe production.

[0040] In some embodiments, the carbon source gas in the P2 and P3 processes includes at least one of methane, ethylene, propylene, and acetylene; and the dilution gas includes at least one of hydrogen, argon, and nitrogen.

[0041] In some embodiments, in the P1 process and the P2 process, the porous carbon material exists in a fluidized state under the action of the gas flow of the raw gas and the diluent gas, or exists in an expanded state driven by the baffle or other components inside the cavity, and the volume of the dense phase region is 1.2 to 2.5 times the volume of static accumulation. The loose particle state and the circulating movement of the particles in the cavity greatly increase the contact between the raw gas and the particles;

[0042] The P1 process is conducive to the silicon-containing material entering the porous carbon and achieving uniform distribution of silicon and porous carbon carriers, which is beneficial to the cycle performance of the secondary battery. At the same time, the P2 process is conducive to the carbon-containing material being more evenly attached to the surface of the composite negative electrode material intermediate, which is conducive to achieving more uniform coating and improving conductivity, thereby improving the rate performance of the secondary battery.

[0043] In some embodiments, in the P1 process, the flow rates of the silicon source gas and the dilution gas are determined according to the weight of the porous carbon in the reaction chamber, and the silicon source gas is introduced at a flow rate of 1L / min / kg to 50L / min / kg, and the dilution gas is introduced at a flow rate of 1L / min / kg to 50L / min / kg. Too low or too high a dilution gas is not conducive to the fluidization of the powder in the reaction chamber. The ratio of the silicon source gas to the dilution gas is D, and D is less than 1.5. Too high a silicon source gas flow rate or a silicon source gas ratio is not conducive to its full contact with the porous carbon carrier, and is not conducive to the uniform adhesion of the silicon-containing material to the porous carbon support, thereby posing a risk of deteriorating the cycle performance of the secondary battery, or leaving the reaction chamber before entering the porous carbon pores and entering the exhaust gas pipe for discharge, thereby posing a risk of reducing the utilization rate of the silicon source gas.

[0044] In some embodiments, in the P2 process, the flow rates of the carbon source gas and the dilution gas are determined based on the weight of the porous carbon in the reaction chamber, and the carbon source gas is introduced at a flow rate of 1L / min / kg to 50L / min / kg, and the dilution gas is introduced at a flow rate of 1L / min / kg to 50L / min / kg. Too low or too high a dilution gas is not conducive to the fluidization of the powder in the reaction chamber. The ratio of the carbon source gas to the dilution gas is E, E<1.5. Too high a carbon source gas flow rate or a carbon source gas ratio is not conducive to vapor deposition 2, and is not conducive to the adhesion of carbon-containing materials to the composite negative electrode material intermediate 1.

[0045] In some embodiments, during the P1 process, the range of T1 is 390°C-650°C. If the temperature is too low, the decomposition rate of the silicon source gas is low, which is not conducive to the adhesion of the silicon-containing material to the porous carbon carrier. If the temperature is too high, it is not conducive to the uniform adhesion of the silicon-containing material inside and outside the porous carbon carrier, which is not conducive to the cycle performance of the secondary battery.

[0046] In the P2 process, the range of T2 is 200℃-750℃. Too low a temperature is not conducive to the adhesion of carbon-containing materials to the composite negative electrode material intermediate 1. Too high a temperature has the risk of producing SiC phase. At the same time, there is also the risk of reducing gram capacity and initial efficiency, which is not conducive to improving the energy density of the secondary battery.

[0047] In some embodiments, the P1 process has a holding time of 0.5h-2h, the P2 process has a holding time of 0.5h-2h, and the P3 process has a holding time of ≤2h.

[0048] In some embodiments, in the P1 process, the time t1 of deposition 1 is 2.5h-30h, in the P2 process, the time t1 of deposition 2 is 2h-24h, and in the P3 process, the time t1 of deposition 3 is 2h-12h.

[0049] In some embodiments, reactor 1 and reactor 2 are at least one of a fluidized bed, a vibrating bed, and a rotary kiln.

[0050] The preparation method of the porous carbon carrier comprises carbonization and activation steps, the activation step comprises a gas activation method and an alkali activation method, and the gas activation method comprises at least one of the following steps: (the flow rates of the inert gas and the activation gas are determined according to the weight of the carbon source precursor in the reaction chamber)

[0051] G1: Carbonization step: Inert gas is introduced into the reaction chamber of the reactor 3 containing the carbon source precursor, and the inert gas flow rate is 0.2L / min / kg-5L / min / kg, and the reaction chamber is heated to TG1, the TG1 range is 400℃-1500℃, and carbonization cracking reaction is carried out, and the TG1 is kept warm for ≤24h. During this process, the surface pressure 1 of the reaction chamber is 0.5kpa-50kpa; after the cracking reaction, a porous carbon carrier intermediate is obtained;

[0052] G2: Activation step: The porous carbon carrier intermediate is transferred to the reaction chamber of the reactor 4, and the inert gas is passed and the temperature is raised to TG2, the inert gas flow rate is 0.2L / min / kg-5L / min / kg, and the TG2 range is 500℃-1100℃, and then the activation gas containing CO2 is passed into the reaction chamber, and the activation gas flow rate is 0.2L / min / kg-5L / min / kg, and the activation reaction is carried out, and the TG2 is kept warm for 0.1h-80h. During this process, the surface pressure 2 of the reaction chamber is 0.5kpa-50kpa; after the activation reaction, the porous carbon carrier is obtained.

[0053] Or G2': Activation step: The porous carbon carrier intermediate is transferred to the reaction chamber of the reactor 4', and the inert gas is passed and the temperature is raised to TG2', the inert gas flow rate is 0.2L / min / kg-5L / min / kg, and the TG2' range is 200-1300°C, and then the activation gas containing H2O is passed into the reaction chamber, and the activation gas flow rate is 0.2L / min / kg-5L / min / kg, and the activation reaction is carried out, and the TG2 is kept warm for 0.1h-50h. During this process, the surface pressure 2' of the reaction chamber is 0.5kpa-50kpa; after the activation reaction, the porous carbon carrier is obtained.

[0054] In some embodiments, the carbon source precursor in the G1 process comprises a polymer

[0055] (such as polyacrylonitrile, phenolic resin, melamine resin, epoxy resin, urea-formaldehyde resin, polyester resin, polyamide resin, polyimide resin, polycarbonate, acrylonitrile copolymer), biomass carbon source

[0056] (such as coconut shell, fruit shell, fruit core, tea shell, wood, cellulose, straw, bamboo, walnut shell, sugar, starch) and at least one of mineral carbon sources (such as asphalt, coal, petroleum).

[0057] In some embodiments, the G2 step is used for gas activation to achieve a porous carbon carrier with a good pore structure; in some embodiments, the G2' step is used for gas activation, which has a simple process, low cost, high cost performance, and is easy to scale up.

[0058] In some embodiments, the activation step includes two activation steps, G2 and G2', to achieve a high-efficiency activation effect.

[0059] In some embodiments, the inert gas is at least one of nitrogen, argon, and helium, used as a protective gas. The inert gas flow rate ranges from 0.25 L / min / kg to 4.5 L / min / kg. If the flow rate is too large, the reactants are at risk of being blown away, resulting in a reduced yield; if the flow rate is too small, it is difficult to form a good protective atmosphere, which is not conducive to the stability or safety of the carbonization process.

[0060] In some embodiments, the activation gas contains at least one of CO2 and H2O. In the process of G2 or G2', the flow rate of the activation gas ranges from 0.2L / min / kg to 5L / min / kg. If the flow rate is too large, the reactants may be blown away and there may be a risk of over-activation. If the flow rate is too small, there may be a risk of substandard activation, which is not conducive to obtaining porous carbon with a good pore structure.

[0061] In some embodiments, TG1 ranges from 500° C. to 1200° C. A too low temperature may result in insufficient carbonization, while a too high temperature may be beneficial to the ordered transformation of amorphous carbon but may be detrimental to the subsequent activation effect.

[0062] In some embodiments, the TG1 holding time is 0.2h-12h. If the time is too short, there is a risk of insufficient carbonization. If the time is too long, although it is beneficial to the ordered transformation of amorphous carbon, it is not conducive to the subsequent activation effect.

[0063] In some embodiments, TG2 is in the range of 700° C.-1000° C. If the temperature is too low, there is a risk of insufficient activation, and if the temperature is too high, there is a risk of over-activation, and the yield will be reduced.

[0064] In some embodiments, the TG2 holding time is 1h-50h. If the time is too short, there is a risk of insufficient activation and failure to obtain suitable pore volume and pore size. If the time is too long, there is a risk of over-activation, which not only results in high energy consumption and reduced yield, but is also not conducive to obtaining a porous carbon carrier with uniform pore size and high pressure resistance, which is not conducive to the cycle stability of the secondary battery.

[0065] In some embodiments, TG2' ranges from 500°C to 1000°C. Too low a temperature may result in insufficient activation, while too high a temperature may result in overactivation, which may reduce the yield and be detrimental to obtaining a porous carbon support with high compressive strength.

[0066] In some embodiments, the TG2' insulation time is 1h-40h. If the time is too short, there is a risk of insufficient activation and failure to obtain suitable pore volume and pore size. If the time is too long, there is a risk of over-activation, which not only results in high energy consumption and reduced yield, but is also not conducive to obtaining a porous carbon carrier with uniform pore size and high pressure resistance, which is not conducive to the cycle stability of the secondary battery.

[0067] In some embodiments, in the G1 process, the gauge pressure 1 is 0.5 kPa to 25 kPa, in the G2 process, the gauge pressure 2 is 0.5 kPa to 25 kPa, and in the G2' process, the gauge pressure 2' is 0.5 kPa to 25 kPa. When the gauge pressure is too low, it is not conducive to forming a good protective atmosphere, and there is a risk of air entering, which is not conducive to safe production; in the G2 and G2' processes, the activated gas is not easy to enter the porous carbon carrier intermediate, which is not conducive to the formation of a porous carbon carrier with uniform pore size. When the gauge pressure is too high, it approaches or exceeds the pressure resistance limit of some accessories of the equipment, which is not conducive to safe production.

[0068] In some embodiments, the reactor 3, the reactor 4, and the reactor 4' are at least one of a fluidized bed, a vibrating bed, a rotary kiln, a box kiln, a roller kiln, and a push plate kiln.

[0069] The preparation method of the porous carbon carrier comprises carbonization and activation steps, the activation step comprises a gas activation method and an alkali activation method, and the alkali activation method comprises the following steps: (the flow rates of the inert gas and the oxygen-containing gas are determined according to the weight of the carbon source precursor in the reaction chamber)

[0070] K1: Carbonization step: Inert gas is introduced into the reaction chamber of the reactor 5 containing the carbon source precursor, and the inert gas flow rate is 0.2L / min / kg-5L / min / kg, and the reaction chamber is heated to TK1, TK1 range is 400℃-1500℃, and carbonization cracking reaction is carried out, and TK1 is kept warm for 0-24h. During this process, the surface pressure 1 of the reaction chamber is 0.5kpa-50kpa;

[0071] K2: Activation step: After the porous carbon carrier intermediate is fully mixed with the alkaline activator in a certain proportion, it is transferred to the reaction chamber of the reactor 6, and an inert gas is introduced and the temperature is raised to TK2. The inert gas flow rate is 0.2L / min / kg-5L / min / kg, and the TK2 range is 400℃-1000℃. The activation reaction is carried out, and the TK2 is kept warm for 0.01h-12h. During this process, the surface pressure 2 of the reaction chamber is 0.5kpa-50kpa; after the activation reaction, the porous carbon carrier intermediate is obtained;

[0072] K3: Passivation step: oxygen-containing gas is introduced into the reaction chamber of the reactor 6 for passivation treatment, and the flow rate of the oxygen-containing gas is 0.2L / min / kg-5L / min / kg. The product after the passivation treatment is a porous carbon carrier intermediate 2; during this process, the surface pressure 2 of the reaction chamber is 0.5kpa-50kpa

[0073] The porous carbon intermediate is acid-washed, water-washed and dried to remove excess metal impurities and excess water, thereby obtaining a porous carbon carrier. The content of metal impurity elements in the porous carbon carrier is less than 100 ppm, and the water content is less than 2%.

[0074] In some embodiments, the inert gas contains at least one of nitrogen, argon, and helium, which is used as a protective gas.

[0075] In some embodiments, in the K1 process and the K2 process, the inert gas flow rate ranges from 0.25 L / min / kg to 4.5 L / min / kg; in the K1 process, if the flow rate is too large, the reactants are at risk of being blown away, resulting in a reduced yield; if the flow rate is too small, it is difficult to form a good protective atmosphere, which is not conducive to the stability or safety of the carbonization process. In the K2 process, if the flow rate is too large, the reactants are at risk of being blown away, resulting in a reduced yield; if the flow rate is too small, it is difficult to form a good protective atmosphere, because the intermediate byproducts such as K vapor and H2 are highly active, which is not conducive to the stability or safety of the activation process.

[0076] In some embodiments, TK1 ranges from 500° C. to 850° C. A temperature that is too low may result in insufficient carbonization, while a temperature that is too high may be beneficial to the ordered transformation of amorphous carbon but may be detrimental to the subsequent activation effect.

[0077] In some embodiments, the TK1 holding time is 0.1h-12h. If the time is too short, there is a risk of insufficient carbonization. If the time is too long, although it is beneficial to the ordered transformation of amorphous carbon, it is not conducive to the subsequent activation effect.

[0078] In some embodiments, TK2 ranges from 500°C to 850°C. Too low a temperature may result in insufficient activation, while too high a temperature may result in overactivation, a reduced yield, and the risk of potassium vapor appearing, which is detrimental to the stability or safety of the activation process.

[0079] In some embodiments, the TK2 insulation time is 0.1h-10h. If the time is too short, there is a risk of insufficient activation and failure to obtain suitable pore volume and pore size. If the time is too long, there is a risk of over-activation, which not only results in high energy consumption and reduced yield, but is also not conducive to obtaining a porous carbon carrier with uniform pore size and high pressure resistance, which is not conducive to the cycle stability of the secondary battery.

[0080] In some embodiments, in the K2 process, the alkaline activator contains KOH. The molar ratio of the porous carbon carrier intermediate to the alkaline activator is in the range of 0.2-2. If the molar ratio is too low, there is a risk of failing to achieve the activation effect, failing to obtain a high pore volume, and after depositing the silicon-containing material, it is not conducive to obtaining a composite negative electrode material with a high gram capacity and first efficiency, which is not conducive to improving the energy density of the secondary battery; if the molar ratio is too high, there is a risk of overactivation, resulting in a reduced yield, increased costs, and not conducive to forming a porous carbon carrier with a uniform pore structure, thereby not being conducive to obtaining a composite negative electrode material with good cycle performance.

[0081] In some embodiments, in the K3 process, the oxygen-containing gas contains at least one of CO2, H2O, and O2. In the K3 process, the highly active components containing K element or hydrogen in the passivation process 2 are unstable when exposed to air, which is conducive to safe discharge and safe production.

[0082] In some embodiments, in the K1 process, the gauge pressure 1 is 0.5 kPa to 25 kPa, in the K2 process, the gauge pressure 2 is 0.5 kPa to 25 kPa, and in the K3 process, the gauge pressure 3 is 0.5 kPa to 25 kPa. When the gauge pressure is too low, it is not conducive to forming a good protective atmosphere, and there is a risk of air entering, which is not conducive to safe production. When the gauge pressure is too high, it approaches or exceeds the pressure resistance limit of some equipment accessories, which is not conducive to safe production.

[0083] In some embodiments, the reactor 5 and the reactor 6 are at least one of a fluidized bed, a vibrating bed, a rotary kiln, a box furnace, a roller kiln, and a push plate kiln.

[0084] The third aspect of the present invention provides a secondary battery electrochemical device, comprising a negative electrode, a positive electrode, an electrolyte and a separator. The negative electrode comprises a negative electrode material layer, the negative electrode material layer comprises a negative electrode active material, and the negative electrode active material comprises the composite negative electrode material of the first aspect or the composite negative electrode material prepared by the preparation method of the second aspect.

[0085] In some embodiments, the electrochemical device of the present invention is a high energy density fast-charge lithium ion battery, which comprises a negative electrode, a positive electrode, an electrolyte, and a separator.

[0086] In some embodiments, the electrochemical device of the present invention is a lithium ion battery, the negative electrode of the lithium ion battery includes a negative electrode current collector and a negative electrode material layer coated on the negative electrode current collector, the negative electrode material layer includes a negative electrode active material, and the positive electrode of the lithium ion battery includes a positive electrode current collector and a positive electrode material layer coated on the positive electrode current collector, the positive electrode material layer includes a positive electrode active material.

[0087] In some embodiments, based on the mass of the negative electrode active material, the mass content of the composite negative electrode material of the present invention is 0.1% to 100%. In some embodiments, the mass content of the composite negative electrode material is 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100% or a range consisting of any two of these values.

[0088] In some embodiments, the negative electrode active material further includes a carbon material, and the carbon material includes at least one of natural graphite, artificial graphite, hard carbon, and soft carbon.

[0089] In some embodiments, the negative electrode material layer further comprises a conductive agent and a binder. The mass content of the conductive agent in the negative electrode material layer is preferably 0.01% to 15%, more preferably 0.02% to 10%.

[0090] The mass content of the binder in the negative electrode material layer is preferably 0.1% to 15%, and more preferably 0.3% to 10%.

[0091] In some embodiments, the negative electrode conductive agent includes, but is not limited to: at least one of carbon-based materials, metal-based materials, conductive polymers, conductive oxides, conductive nitrides, etc. In some embodiments, the carbon-based material includes at least one of conductive carbon black, carbon nanotubes, acetylene black, graphene, carbon fiber, flake graphite, Ketjen black, natural graphite, artificial graphite, etc. The carbon nanotube may include, but is not limited to, at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes. In some embodiments, the metal-based material includes at least one of copper, nickel, aluminum, or silver.

[0092] In some embodiments, the conductive polymer is at least one of polyaniline, polythiophene, polyacetylene, polypyrrole, and polyphenylene derivatives.

[0093] In some embodiments, the negative electrode binder includes, but is not limited to: at least one of copolymer-based materials and polymer-based materials; the copolymer-based binder includes at least one of styrene-butadiene copolymer, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, acrylonitrile, and (meth)acrylic acid copolymer obtained by copolymerization of unsaturated carboxylic acids; some groups of the copolymer are substituted by one or more of Na, K, and Li. The polymer-based binder includes at least one of polyurethane, polyacrylonitrile, polyimide, polyamide-imide, polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, and polyphosphazene;

[0094] In some embodiments, the binder and a viscosity-adjusting thickener may be used together. The mass content of the thickener in the negative electrode material layer is preferably 0.1% to 10%, more preferably 0.2% to 8%. The thickener includes at least one of carboxymethyl cellulose (sodium), hydroxymethyl cellulose, methyl cellulose, ethyl cellulose, polyvinyl alcohol, polyacrylic acid (ester), oxidized starch, phosphorus oxidized starch, casein, etc.

[0095] In some embodiments, the negative electrode further includes a negative electrode current collector, which includes at least one of: copper foil, copper foil coated with a conductive agent, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, and a polymer substrate coated with a conductive metal.

[0096] In some embodiments, the positive electrode active material includes at least one of lithium iron phosphate, lithium cobalt oxide, lithium nickel manganese cobalt oxide, lithium nickel manganese aluminum oxide, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, and spinel lithium nickel manganese oxide.

[0097] In some embodiments, the positive electrode material layer further comprises a conductive agent and a binder. The mass content of the conductive agent in the positive electrode material layer is preferably 0.01% to 10%. The mass content of the binder in the positive electrode material layer is preferably 0.1% to 10%.

[0098] In some embodiments, the positive electrode conductive agent includes, but is not limited to: at least one of carbon-based materials, metal-based materials, conductive polymers, conductive oxides, conductive nitrides, etc. In some embodiments, the carbon-based material includes at least one of conductive carbon black, carbon nanotubes, acetylene black, graphene, carbon fiber, flake graphite, Ketjen black, natural graphite, artificial graphite, etc. The carbon nanotube may include, but is not limited to, at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes. In some embodiments, the metal-based material includes at least one of copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer is at least one of polyaniline, polythiophene, polyacetylene, polypyrrole, and polyphenylene derivatives.

[0099] In some embodiments, the positive electrode binder includes, but is not limited to: at least one of polyvinylidene fluoride, modified polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified SBR rubber or polyurethane.

[0100] In some embodiments, the positive electrode further includes a positive electrode current collector, which includes at least one of aluminum foil, aluminum foil coated with a conductive agent, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, and a polymer substrate coated with a conductive metal.

[0101] The secondary battery provided by the present invention further comprises an electrolyte. The electrolyte is at least one of a solid electrolyte, a gel electrolyte, and an electrolyte, and the electrolyte comprises a lithium salt, a non-aqueous solvent, and an additive. The electrolyte of the present invention may be an electrolyte known in the prior art.

[0102] In some embodiments, the lithium salt includes inorganic lithium salts such as LiClO4, LiPF6, LiAsF6, LiBF4, LiAlCl4, LiSCN, and organic lithium salts such as LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, lithium bis(difluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), organic borate lithium salts such as lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), and organic lithium phosphate salts. The concentration of the lithium salt in the electrolyte is 0.5 mol / L to 2 mol / L.

[0103] In some embodiments, the non-aqueous solvent may be at least one of a carbonate compound, a carboxylate compound, an ether compound, and other organic solvents.

[0104] The carbonate compound may be at least one of a cyclic carbonate compound, a chain carbonate compound, and a fluorinated carbonate compound. Examples of cyclic carbonate compounds are at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), and vinylene carbonate (VC). Chain carbonate compounds are at least one of diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), dimethyl carbonate (DMC), and dipropyl carbonate (DPC). The fluorinated carbonate compound is at least one of fluoroethylene carbonate (FEC), 1,1-difluoroethylene carbonate, 1,2-difluoroethylene carbonate (DFEC), 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, and trifluoromethylethylene carbonate.

[0105] The carboxylate compound is at least one of methyl formate (MF), methyl acetate (MA), ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate (EP), propyl propionate, methyl butyrate (MB), γ-butyrolactone, decanoic acid lactone, valerolactone, mevalonolactone, and caprolactone.

[0106] The ether compound is at least one of tetrahydrofuran (THF), 2-methyltetrahydrofuran (2Me-THF), 1,3-dioxolane (DOL), dimethoxymethane (DMM), 1,2-dimethoxyethane (DME), 1,2-diethoxyethane, ethoxymethoxyethane, dibutyl ether, tetraethylene glycol dimethyl ether, and diethylene glycol dimethyl ether (DG).

[0107] The non-aqueous solvent is a sulfur-containing solvent including ethyl methyl sulfone (EMS), dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, ethylene sulfite (ES), propylene sulfite (PS), diethyl sulfite (DES), dimethyl sulfite (DMS), a nitrogen-containing solvent including 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, and a P-containing solvent including at least one of trimethyl phosphate, triethyl phosphate, trioctyl phosphate and phosphate.

[0108] In some embodiments, the additive accounts for 0.02% to 30% of the electrolyte mass. The above non-aqueous solvent and lithium salt can be used as additives. The additive of the present invention can be an additive known in the prior art.

[0109] The secondary battery provided by the present invention also includes a separator. The separator may include at least one of a substrate layer and a coating treatment layer. In some embodiments, the material of the substrate layer is at least one of polyethylene, polypropylene, polyethylene terephthalate, polyimide, polyphenylene sulfide (PPS), and cellulose, and the substrate layer is a non-woven fabric, film, or composite film with a porous structure, including at least one of a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric, and a polypropylene-polyethylene-polypropylene porous composite film.

[0110] In some embodiments, at least one surface of the substrate layer has a coating layer, and the coating layer is at least one of a polymer layer and an inorganic layer. The inorganic layer includes inorganic particles and a binder, and the inorganic particles are at least one of oxides (e.g., aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, zirconium oxide, magnesium oxide, titanium oxide), nitrides (e.g., boron nitride, silicon nitride, aluminum nitride), silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate.

[0111] The binder is at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride and hexafluoropropylene, styrene-butadiene rubber, polyamide, polyacrylonitrile, polyacrylic acid (e.g., polybutyl acrylate, polyethyl acrylate, polybutyl methacrylate, polymethyl methacrylate, polyacrylate, polyacrylic acid, polyacrylate), polyvinylpyrrolidone, polyethylene alkoxide, polytetrafluoroethylene and polyhexafluoropropylene.

[0112] The polymer layer contains a polymer, and the material of the polymer is at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyoxyethylene alkylphenol ether, polyoxyethylene fatty alcohol ether, polyoxyethylene polyoxypropylene block copolymer, siloxane, polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, and polyvinyl pyrrolidone.

[0113] A fourth aspect of the present invention provides an electronic device comprising the secondary battery electrochemical device of the third aspect.

[0114] The electronic device of the present invention is not particularly limited and can be used for any purpose known in the prior art.

[0115] In some embodiments, the electronic devices of the present invention include, but are not limited to, automobiles, motorcycles, laptop computers, portable phones, headphones, cameras, video recorders, LCD televisions, portable cleaners, household batteries, power tools, backup power supplies, motors, lighting fixtures, toys, game consoles, clocks, etc.

[0116] Compared with the prior art, the present invention has at least the following beneficial effects:

[0117] The present application provides a negative electrode material, a secondary battery and an electronic device. The secondary battery includes a negative electrode plate, and the negative electrode plate includes a composite negative electrode material. The composite negative electrode material of the present application includes elemental carbon and elemental silicon. The 8T powder compaction density PD of the composite negative electrode material is g / cm 3 , specific surface area B, unit: cm 3 / g, (methyl) satisfies 0.01≤PD / B≤6;

[0118] The composite negative electrode material provided by the present invention has low internal closed pores (CP diameter is greater than 100nm and the closed pore area accounts for less than 20%), high first efficiency and high theoretical capacity; the composite negative electrode material includes a porous carbon carrier and a silicon element filled inside and outside the porous carbon carrier;

[0119] The silicon element accounts for 10wt%-60wt% in the composite negative electrode material.

[0120] The composite negative electrode material in the secondary battery provided by the present invention greatly improves the capacity and energy density of the secondary battery, and at the same time, significantly improves the cycle performance and rate performance of the secondary battery.

[0121] Of course, any product or method of the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0122] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0123] Figure 1 A powder compaction density curve of a composite negative electrode material provided by an embodiment of the present invention;

[0124] Figure 2 It is a cross-sectional SEM of the composite negative electrode material of the present invention and a photograph of the position of the closed pores with a diameter of 100 nm. The arrows indicate the closed pores of the present invention.

[0125] Figure 3-1 It is a charge-discharge curve diagram of the composite negative electrode material of the present invention.

[0126] Figure 3-2 It is a DQ / DV curve diagram of the composite negative electrode material of the present invention.

[0127] Figure 4-1 It is a cumulative distribution diagram of pore size and pore volume of the porous carbon carrier of the composite negative electrode material of the present invention.

[0128] Figure 4-2 The figure is a distribution diagram of the pore size-pore volume increment change of the porous carbon carrier of the composite negative electrode material of the present invention.

[0129] Figure 5 This is a cross-sectional SEM-EDS analysis result diagram of the composite negative electrode material of the present invention;

[0130] Figure 6 Schematic diagram of the minimum circumscribed circle used for calculating the closed pore ratio of the composite negative electrode material of the present invention. DETAILED DESCRIPTION

[0131] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0132] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0133] In the detailed description and claims, a list of items connected by the terms "at least one of", "at least one of", "at least one of" or other similar terms may mean any combination of the listed items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" may represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c may be single or multiple.

[0134] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0135] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0136] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0137] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0138] The term "PET" is the abbreviation of "Polyethyleneterephthalate", which means polyethylene terephthalate; the term "PU" is the abbreviation of "polyurethane", which means polyurethane material and is the abbreviation of polyurethane...

[0139] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0140] The present invention is not limited to the following examples. In addition, unless otherwise specified, "parts" and "%" are by mass. The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or purchased directly from the market.

[0141] Embodiment 1:

[0142] This embodiment provides a composite negative electrode material. The 8T powder compaction density PD of the composite negative electrode material of this embodiment is 1.0, in g / cm 3 , the specific surface area B is 7.6, unit m 2 / g, the ratio of PD to B is 0.13;

[0143] The composite negative electrode material provided in this embodiment has low internal closed pores. According to the cross-section particle SEM photos, the internal closed pores with diameters greater than 100 nm account for 3% of the closed pore area. The composite negative electrode material comprises a porous carbon carrier and a silicon-containing material filled inside and outside the porous carbon carrier. The composite negative electrode material has a high first efficiency of 87% and a high theoretical capacity of 1565 mAh / g.

[0144] The ratio of the capacity of the composite negative electrode material in this embodiment after the first delithiation to 0.8V to the capacity of the composite negative electrode material after the first delithiation to 2.0V is Cap, and the value of Cap is 86%.

[0145] The composite negative electrode material provided in this embodiment greatly improves the cycle stability and rate performance of the battery. The composite negative electrode material provided in this embodiment is mainly prepared by the following steps:

[0146] Preparation of porous carbon support:

[0147] First, weigh 200g of phenolic resin (carbon source precursor) and grind it into 200μm by ball milling, put it into a crucible and place it in a box furnace.

[0148] 1G1: Carbonization step: Inert gas nitrogen is introduced into the reaction chamber of the box furnace containing the carbon source precursor, and the flow rate of inert gas nitrogen is 1.5L / min / kg, i.e. 0.3L / min, and the reaction chamber is heated to 300°C for polymerization for 2h, and then the reaction chamber is heated to 1TG1, 1TG1 is 900°C, and carbonization cracking reaction is carried out, and 1TG1 is kept warm for 4h. During this process, the surface pressure of the reaction chamber is 0.1kpa-20kpa; after the cracking reaction, a porous carbon carrier intermediate is obtained;

[0149] 1G2: Activation step: The nitrogen introduced into the reaction chamber of the box furnace reactor is switched to CO2 activation gas, and the activation gas flow rate is 1.5L / min / kg, i.e. 0.3L / min, to further activate and form pores for the pyrolytic carbon. The temperature of the reaction chamber 1TG2 remains unchanged, and 1TG2 is kept at 980°C for 8h. During this process, the surface pressure of the reaction chamber is 0.1kpa-20kpa; after 8h of activation, the carbon dioxide is switched to nitrogen, and the nitrogen flow rate is 1.5L / min / kg, i.e. 0.3L / min, and the heating is stopped. When the sample cools to room temperature, 18.4g of porous carbon carrier is obtained after weighing; the porous carbon carrier is ball-milled and crushed. After crushing, the particle size Dv50 of the porous carbon carrier is tested to be 6.7 microns, and the specific surface area is 1890m 2 / g, the pores smaller than 50nm accounted for 99%, the pores smaller than 3nm accounted for 94%, and the pore volume tested by nitrogen adsorption and desorption was 0.91cm 3 / g.

[0150] Preparation of composite negative electrode materials:

[0151] 1P1: Take 10g of the porous carbon carrier obtained above and put it into a tubular rotary furnace, introduce nitrogen into the tubular rotary furnace equipped with the porous carbon carrier, set the speed to 1 rpm, the nitrogen flow rate to 10L / min / kg, i.e. 0.1L / min, and heat it to 1T1, 1T1 is 440℃, keep it warm for 1h, stop introducing nitrogen, introduce a mixed gas of monosilane and diluent nitrogen into the reaction chamber equipped with the porous carbon carrier, the volume ratio of monosilane gas to nitrogen is 1:20, and introduce it into the tubular furnace at a flow rate of 10L / min / kg, i.e. 0.1L / min, for silicon deposition for 10h, then switch the mixed gas of monosilane and nitrogen back to nitrogen, with a flow rate of 0.25L / min / kg. Obtain a composite negative electrode material intermediate of deposited silicon material; the surface pressure of the reaction chamber is 0.1kPa to 20kPa;

[0152] 1P2: Then, the temperature of the 1P1 tubular rotary kiln reaction chamber is raised to 1T2, 1T2 is 500°C, and after keeping warm for 1h, the introduction of nitrogen is stopped, and a mixed gas of acetylene and nitrogen is introduced into the reaction chamber of 1P1, the volume ratio of acetylene gas to nitrogen is 1:1, and the flow rate is 10L / min / kg, i.e. 0.1L / min, for vapor deposition of carbon, the deposition time is t2, t2 is 5h; then the introduction of the mixed gas of acetylene and nitrogen is stopped, and switched to nitrogen gas introduction, with a flow rate of 10L / min / kg, i.e. 0.1L / min, until the reaction product is cooled to room temperature, 17g of composite negative electrode material is obtained, and the surface pressure of the reaction chamber is 0.1kPa to 20kPa.

[0153] The obtained composite negative electrode material was subjected to powder testing, electrochemical testing, full battery assembly and testing. The test results are shown in Table 1.

[0154] Example 2: The difference between this example and Example 1 is that, when preparing the composite negative electrode material, the step of introducing carbon source acetylene gas is not performed; the preparation method and its step parameters refer to Example 1.

[0155] Example 3: The difference between this example and Example 1 is that, when preparing the porous carbon carrier of the composite negative electrode material, the carbon source precursor is commercially available phenolic resin balls, the activation step adopts alkaline activation, and the raw material is commercially available KOH reagent, as follows; for the rest of the preparation method and its step parameters, refer to Example 1.

[0156] Commercially available phenolic resin balls have a Dv50 of 6.7 microns and a Dn10 of 1.2 microns. First, 200 g of phenolic resin ball carbon source precursor is weighed, loaded into a dry pot and placed in a box furnace. The carbonization step is similar to Example 1, and 110 g of a porous carbon carrier intermediate is obtained;

[0157] 3K2: Activation step: After 100g of the porous carbon carrier intermediate is fully mixed with the alkaline activator KOH reagent (KOH purity 85%) at a mass ratio of 1:3, it is placed in a crucible and transferred to the reaction chamber of a box furnace reactor, inert gas nitrogen is introduced and the temperature is raised to 3TK2, the nitrogen flow rate is 3L / min / kg, i.e. 0.3L / min, 3TK2 is 750℃, activation reaction is carried out, and 3TK2 is kept warm for 0.75h. During this process, the surface pressure of the reaction chamber is 0.1kpa-20kpa; after the activation reaction, the porous carbon carrier intermediate 2 is obtained;

[0158] 3K3: Passivation step: The gas introduced into the reaction chamber of the box furnace is switched to a CO2-containing gas for passivation treatment for 2 hours, and the CO2-containing gas flow rate is 3L / min / kg, i.e. 0.3L / min. After the passivation treatment for 2 hours, it is switched to nitrogen for cooling, and the obtained product is a porous carbon support intermediate 3; during this process, the surface pressure 2 of the reaction chamber is 0.1kpa-20kpa;

[0159] The porous carbon intermediate was acid-washed, water-washed, and dried to remove excess metal impurities and excess water, thereby obtaining a porous carbon carrier. The metal impurity element content in the porous carbon carrier was 50 ppm, and the water content was 0.2%. The specific surface area of ​​the porous carbon carrier was 2003 m 2 / g, and the pore volume tested by nitrogen adsorption and desorption is 0.75cm 3 / g;

[0160] After obtaining the porous carbon support, continue preparing the composite negative electrode material, referring to Example 1.

[0161] Example 4: The difference between this example and Example 1 is that a porous carbon carrier using commercially available coconut shell as a carbon source is selected as the porous carbon carrier, and a fluidized bed reactor is selected to prepare the composite negative electrode material, as follows; the rest of the preparation method and its step parameters refer to Example 1.

[0162] 4P1: 1000 g of porous carbon support with coconut shell as carbon source, Dv50 of the porous carbon support is 6.3 μm, BET is 1380, and pore volume is 0.73 cm 3 / g, put it into the reaction chamber of the fluidized bed reactor, set the stirring blade speed to 100 rpm, pass nitrogen at a flow rate of 10L / min / kg, i.e. 10L / min, so that the porous carbon reaches a stable fluidized state (when stable fluidization, the height of the solid phase dense phase region is 1.5-2.5 times the initial stacking height), and heat the fluidized bed reaction chamber to 4T1, 4T1 is 500°C. Keep warm for 2h, and then pass monosilane at a flow rate of 2L / min / kg, i.e. 2L / min, after the temperature stabilizes, pass monosilane for 6h, and control the pressure of the fluidized bed reaction chamber to a slightly positive pressure (gauge pressure is 0-20kPa).

[0163] 4P2: Subsequently, the introduction of silane was stopped. After 10 minutes, acetylene gas was introduced at a flow rate of 6 L / min / kg, i.e. 6 L / min. The acetylene flow time was 5 hours, and the pressure of the fluidized bed reaction chamber was controlled to be slightly positive (gauge pressure was 0-10 kPa).

[0164] Subsequently, the introduction of acetylene was stopped, and the temperature was lowered to room temperature under a nitrogen atmosphere before the material was discharged to obtain 1.8 kg of a composite negative electrode material.

[0165] Example 5: The difference between this example and Example 4 is that a porous carbon carrier using a commercially available resin as a carbon source is selected as the porous carbon carrier, the temperature for introducing silane gas for deposition is changed to 450°C, and the nitrogen preheating temperature is adjusted to 400°C. The composite negative electrode material prepared by the fluidized bed reactor is transferred to a rotary kiln for further carbon coating deposition, as follows; the rest of the preparation method and its step parameters refer to Example 4;

[0166] 5P3: Carbon coating: As described above, 1 kg of the composite negative electrode material prepared in the fluidized bed reactor was transferred to the rotary kiln cavity, the rotary kiln speed was set to 1 rpm, nitrogen was introduced into the rotary kiln cavity, and the nitrogen flow rate was 1 L / min / kg, i.e. 1 L / min, and the rotary kiln reaction cavity was heated to 500°C. After keeping warm for 8 hours, the nitrogen introduction was stopped, and acetylene was introduced into the reaction cavity at an acetylene flow rate of 1 L / min / kg, i.e. 1 L / min, and carbon was vapor deposited for 5 hours; then the acetylene gas was stopped and switched to nitrogen gas at a flow rate of 1 L / min / kg, i.e. 1 L / min, until the reaction product was cooled to room temperature, and 987 g of composite negative electrode material was obtained; the surface pressure of the reaction cavity was 0.1 kPa to 20 kPa.

[0167] Example 6: The difference between this example and Example 5 is that a carbon coating deposition step is further performed in a rotary furnace, and the deposition temperature is 660°C; the rest of the preparation method and its step parameters refer to Example 5.

[0168] Example 7: The difference between this example and Example 1 is that in step 1P2, the reaction chamber temperature is 250°C; the acetylene gas introduced is replaced with H2O; the rest of the preparation method and its step parameters refer to Example 1.

[0169] Embodiment 8: The difference between this embodiment and embodiment 5 is that:

[0170] 1) The porous carbon support uses commercially available mesoporous carbon with a BET of 950 cm 2 / g, pore volume is 0.5g / cc,

[0171] 2) In step 4P1, the temperature of the reaction chamber is raised to 415° C. After keeping the temperature, monosilane gas is introduced; the rest of the preparation method and its step parameters refer to Example 5.

[0172] Embodiment 9: The difference between this embodiment and embodiment 1 is that:

[0173] 1) The 1G2 activation step was not performed;

[0174] 2) The time for passing the silicon source gas is 250 minutes; the rest of the preparation method and its step parameters refer to Example 1.

[0175] Example 10: The difference between this example and Example 3 is that 1) in the carbonization step, the carbonization temperature is 500°C; 2) the time for passing the silicon source gas is 650 minutes; the rest of the preparation method and its step parameters refer to Example 3.

[0176] Comparative Example 1: The difference between this comparative example and Example 1 is that the 1P2 step is performed first to pass the carbon source gas, and then the 1P1 step is performed; the rest of the preparation method and its step parameters refer to Example 1.

[0177] Comparative Example 2: The difference between this comparative example and Example 5 is that the temperature of the carbon source gas cracking deposition in step 5P3 is set to 1200°C; the rest of the preparation method and its step parameters refer to Example 1.

[0178] Comparative Example 3: The difference between this comparative example and Example 5 is that the porous carbon carrier uses commercially available porous graphene; the rest of the preparation method and its step parameters refer to Example 1.

[0179] Comparative Example 4: The difference between this comparative example and Example 5 is that a commercially available molecular sieve is selected as the porous carbon carrier; the rest of the preparation method and its step parameters refer to Example 1.

[0180] Comparative Example 5: The difference between this comparative example and Example 1 is that the rotation speed of the tube furnace in step 1P1 is adjusted to 0 rpm; the rest of the preparation method and its step parameters refer to Example 1.

[0181] Comparative Example 6: Commercially available ground silicon carbon was used to test powder and battery performance, referring to Example 1.

[0182] By comparing Examples 1-2, it can be seen that in the preparation process of the composite negative electrode material, no carbon source deposition is performed, the BET of the 8T powder after compaction is higher, and the PD / B value is lower, thereby reducing the 0.8V capacity share and the first efficiency of the composite negative electrode material, which will also affect the design of the full battery; this is because the carbon deposition layer reduces the BET of the material, reduces the interfacial side reactions with the electrolyte, is conducive to the improvement of the first efficiency and the 0.8V capacity, and can also increase the conductivity of the material, which is conducive to the formation of a more complete conductive network, and is conducive to better cycle stability and rate performance. Compared with Example 1, Example 3 is a spherical resin precursor, which is etched by alkaline method to obtain a porous carbon carrier with higher microporosity. After the same preparation process, a suitable PD / B can be obtained, with a pore area share greater than 100nm, a 0.8V capacity share, and better electrochemical performance; high microporosity, more uniform distribution of silicon on the carrier, lower stress concentration during lithium extraction, and spherical morphology are all conducive to improving particle strength, thereby stabilizing the interface, reducing electrolyte consumption, and improving cycle performance;

[0183] Example 4 uses coconut shell carbon as a porous carbon carrier and adopts a silicon and carbon deposition strategy in a fluidized bed reactor to obtain a suitable PD / B, a capacity ratio of 0.8V and a pore area ratio greater than 100nm, and also obtains a composite negative electrode material with excellent electrochemical performance, cycle and rate performance.

[0184] Compared with Example 4, Example 5 uses a porous carbon carrier using a commercially available resin as a carbon source, adjusts the temperature for deposition by passing silane gas, and adds a rotary kiln carbon deposition step to obtain a composite negative electrode material. Although the gram capacity is reduced due to the increase in deposited carbon, the proportion of pores larger than 100 nm is significantly reduced, the mechanical strength of the particles is improved, and the side reactions caused by particle rupture and failure and the consumption of electrolyte are reduced. Therefore, the composite negative electrode material prepared by this method has better cycle and rate performance.

[0185] Compared with Example 5, the temperature of the rotary kiln carbon deposition step in Example 6 is higher. After the same preparation process, a suitable PD / B can be obtained, with a pore area ratio greater than 100nm and a capacity ratio of 0.8V. The obtained composite negative electrode material has excellent cycle and rate performance; but the gram capacity tends to decrease, indicating that the silicon content that can be deintercalated and deintercalated with lithium is reduced at a higher temperature, which is not conducive to improving the battery energy density; therefore, it is necessary to control the temperature range of carbon deposition.

[0186] As can be seen from Example 7, in the process of preparing the composite material, after silicon is deposited, water vapor passivation treatment can also be used, and after treatment, a composite negative electrode material with suitable PD / B, low >100nm pore area ratio, high 0.8V capacity ratio and excellent electrochemical performance can be obtained;

[0187] It can be seen from Example 8 that a composite negative electrode material with a suitable structure and excellent electrochemical performance can be obtained by using a mesoporous carbon carrier and the conditions of the present invention.

[0188] As can be seen from Example 9, in order to reduce costs, carbonized materials are used as porous carriers. Although PD / B is improved, it is not too high. Although the pore volume is low, the gram capacity, the first efficiency and the 0.8V capacity ratio are also relatively high, and the prepared composite negative electrode material has good electrochemical performance. As can be seen from Example 10, a high specific surface area and high pore volume porous carbon carrier is used to obtain a suitable PD / B, a higher 0.8V capacity ratio, a higher gram capacity and first efficiency, and a composite negative electrode material with good cycle and rate performance.

[0189] By comparing Example 1 with Comparative Example 1, it can be seen that the method for preparing the composite negative electrode material provided by the present invention, the process of first depositing silicon and then depositing carbon has obvious advantages for the electrochemical performance of the material. Compared with Example 5, Comparative Example 2 changes the temperature of the rotary kiln. It can be seen that in the preparation process of the composite negative electrode material, the carbon deposition temperature is too high, resulting in too high PD / B, and the 0.8V capacity ratio is too low, which has a very adverse effect on the electrochemical performance. Compared with Example 5, Comparative Example 3 replaces other carbon carriers, and the composite negative electrode material prepared by this carrier has too high a pore area greater than 100nm, resulting in a significant deterioration in the cycle and rate performance. Similarly, compared with Example 5, Comparative Example 4 is a molecular sieve carrier with a low specific surface area, and the electrochemical performance is significantly deteriorated. Compared with Example 1, after the deposition equipment of Comparative Example 5 was replaced with a static equipment, the cycle and rate performance of the prepared composite negative electrode material were significantly deteriorated. Comparative Example 6 is commercially available grinding method silicon carbon, and its cycle and rate performance are significantly worse than the material of the present invention. By comparing Examples 1-10 with Comparative Examples 1-6, it can be seen that the capacity retention rate and rate performance of the battery of the composite negative electrode material prepared by the composite negative electrode material preparation method provided by the present invention have very significant advantages.

[0190] The materials obtained in Examples 1-10 and Comparative Examples 1-5 were tested and characterized for powder and pole piece performance:

[0191] 1) PD / B test: Take 5g of the above-mentioned composite negative electrode material and test it with a powder compaction density meter (model: Tianjin Bojun BJ-24); first, place a metal disc at the bottom of a special mold, then put 5g of powder into the special mold, and then place a metal disc on the powder so that the powder is located between the two metal discs, place the mold on the powder compaction density instrument, and place a metal cylinder on the top disc of the mold. Set the pressure parameter to 8T, the pressure displacement rate parameter to 20mm / min, the holding time to 60s, and the pressure relief displacement rate parameter to 20mm / min. Record and calculate the thickness of the sample after pressure relief, and calculate the volume of the powder after pressure relief.

[0192] Finally, the 8T powder compaction density PD is calculated according to the density formula. The powder compaction density curve is as follows: Figure 1 As shown; the specific surface area of ​​the powder after pressure relief is tested to obtain the specific surface area B of 8T powder after compaction; PD / B=8T powder compaction density PD / 8T powder specific surface area B after compaction is calculated.

[0193] 2) Test of the proportion of closed pores larger than 100 nm: The above composite negative electrode material and binder polyvinylidene fluoride (PVDF) were dissolved in N-methylpyrrolidone solvent at a mass ratio of 93:7 to prepare a slurry. The slurry was stirred and mixed and coated on the copper foil current collector. The loading amount of the composite negative electrode material was 10 mg / cm 2 The coated electrode is placed in a vacuum oven and dried at 90°C for 12 hours to obtain a negative electrode; the electrode is placed on an argon ion polisher and a high-speed inert ion source is used to cut the electrode section and ion polish it. Use SEM to observe the section after ion cutting, and count the total area A of the composite negative electrode material particles, and the total area P of the closed pores with a diameter greater than 100nm in the composite particles. The area ratio of pores greater than 100nm = (P / A)*100%; Calculation of the area of ​​composite negative electrode material particles: select a particle, take the minimum circumscribed circle diameter on the particle section as the particle diameter D1, the area A1 of this particle = 3.14×(D1 / 2)^2, and so on, calculate the 100 nearest neighbor particles The area of ​​the particles is calculated and the total area A of the composite negative electrode material particles is obtained; a particle with a closed pore is selected, and the minimum circumscribed circle diameter of the pore on the particle section is recorded as the pore diameter d1. The area of ​​this pore P1 = 3.14×(d1 / 2)^2, and so on, the pore areas of the 100 nearest neighboring particles with pore diameter d1>100nm are calculated and the total area P of the pores in the composite negative electrode material particles is calculated; a closed pore is defined as a pore edge line on the particle ion polishing section that is closed; a closed pore SEM-CP is as follows Figure 2 As shown; the minimum circumscribed circle diameter is Figure 6 As shown, refer to the national standard GB_T1182-2018.

[0194] 3) Silicon content test: The test was conducted using inductively coupled plasma optical emission spectroscopy.

[0195] Weigh 0.1g of the above composite material sample and 1.5g of KOH, mix them and heat them in a muffle furnace at 400℃ for 1h. Transfer the treated mixture to a beaker and soak it in 98℃ deionized water for 2h. Filter the soaked solution to remove the residue and transfer it to a volumetric flask. Add deionized water to make it 100mL. Add the fixed solution to the atomization chamber and pump it at a speed of 1.3L / min for testing.

[0196] 4) Particle size test: The particle size distribution of the powder was tested by laser diffraction method, with specific reference to the national standard GB / T19077-2016. 0.2g of the above composite negative electrode material was placed in a beaker, 20mL of deionized water and 5 drops of surfactant were added, and the mixture was transferred to an ultrasonic cleaner for ultrasonic dispersion for 5 minutes to obtain a dispersion. The dispersion was tested using MasterSizer3000 to obtain the sample size.

[0197] Particle size distribution diagram, and volume distribution parameters Dv10, Dv50, Dv90, Dv99 and number distribution parameters Dn10, Dn50, Dn90, Dn99. Dv50 means that 50% of the total sample volume has a particle diameter smaller than this value. And so on. Dv99 means that 90% of the total sample volume has a particle diameter smaller than this value. Dn10 means that 10% of the total sample particle number has a particle diameter smaller than this value. And so on. Dn99 means that 90% of the total sample particle number has a particle diameter smaller than this value.

[0198] 5) BET test: The specific surface area of ​​the above-mentioned composite negative electrode material is tested by nitrogen adsorption and desorption method, with specific reference to the national standard GB / T19587-2017. Weigh 2g of the above-mentioned composite negative electrode material powder into the test sample tube and degas at 200℃ for 2h. After degassing, the sample tube is transferred to the test bench for testing. The adsorbent is high-purity nitrogen, and adsorption and desorption are performed at liquid nitrogen temperature and data are collected; the specific surface area is calculated by the multi-point BET method.

[0199] 6) Porous carbon BET, pore volume, and micro-mesopore ratio test: A high-precision adsorption instrument (Lihanke) was used to perform adsorption-desorption curve test. The adsorption-desorption gas was Ar gas, and the P / P0 measurement range was 0.00000001-0.99. Weigh 0.1g of the above porous carbon material powder into the test sample tube and degas at 200°C for 2h. After degassing, the sample tube was transferred to the test bench for testing. The collected adsorption-desorption curve data was used to calculate the BET and pore volume using the IporeDFT software. The micropore ratio and mesopore ratio were calculated using the pore size and pore volume data. Micropore ratio = (pore volume of 2nm / total pore volume) * 100%; mesopore ratio = (pore volume of 2-50nm / total pore volume) * 100%;

[0200] A porous carbon carrier of a composite negative electrode material provided by an embodiment Figure 4-1 Mesopore size-pore volume cumulative distribution diagram and Figure 4-2 Mesopore diameter-pore volume increment change distribution diagram. In order to obtain a smoother pore diameter-pore volume increment change distribution curve, the pore volume increment change value can be taken at fixed intervals.

[0201] For example, the first, second, third, fourth, fifth, sixth, ... to the nth pore volume increase data are PV1, PV2, PV3, PV4, PV5, PV6, ... to PVn, and the first, second, third, fourth, fifth, sixth, ... to the nth pore volume increase data are (PV5-PV1), (PV6-PV2), (PV7-PV3), (PV8-PV4), (PV9-PV5), (PV10-PV6), ... to (PVn+4-PVn)

[0202] 7) Raman test: The test equipment is Horiba Jobin-Yvon LabRAM HR800 spectrometer, the light source is 532nm, and the test wavelength range is 0cm -1 ~4000cm -1 .

[0203] Take a small amount of powder and spread it evenly on the sample stage, adjust the equipment parameters, analyze the sample area of ​​100μm*100μm, and obtain the Raman spectrum. From the Raman spectrum of the composite negative electrode material, calculate the carbon material at ~1340cm -1 and ~1600cm -1 The intensity ratio of the peak at . The intensity ratios of 100 regions are counted and the average is calculated to obtain the ID / IG of carbon. This intensity ratio reflects the degree of disorder of the carbon material. A higher ratio represents the presence of higher disordered carbon, which is beneficial to improve the strength of the porous carbon support and thus improve the stability of the composite negative electrode material in the cycle.

[0204] The same method was used to calculate the location of silicon materials at 125 cm -1 and ~465cm -1 The intensity ratio of the peak at is used to obtain the ID / IG of the silicon material.

[0205] 8) Carbon content test: Use a high-frequency infrared carbon-sulfur analyzer (Shanghai Dekai HCS-140) to test the sample. Its working principle is to use the characteristics of CO2 and SO2 having strong characteristic absorption bands at 4.26μm and 7.4μm respectively. By measuring the gas absorption light intensity and analyzing the CO2 and SO2 content, the percentage of carbon and sulfur elements in the tested sample can be indirectly determined. Take 0.5g of the above composite negative electrode material sample and input it into the computer, then heat the sample in a high-frequency furnace under oxygen-rich conditions until it burns, so that carbon is oxidized into CO2 gas. The carbon content in the sample can be obtained by analysis and calculation.

[0206] 9) Oxygen content test: Analytical equipment PerkinElmer 2400 Series II CHNS / O elemental analysis. Weigh 0.1g of composite negative electrode material sample and perform parallel measurements twice or more in accordance with the measurement procedure until the two adjacent results meet the analytical error requirements. Then measure the mass percentage of oxygen element in the standard material sample to obtain the calibration factor for the day; the mass percentage of oxygen element = (absolute mass of hydrogen element in the sample obtained from the calibration curve / weighed mass of the sample) * calibration factor of oxygen element for the day * 100%.

[0207] 10) EDS test: In the above-mentioned test method for the proportion of closed pore area > 100 nm, when observing the cross section after ion cutting with SEM, select particles with a cross-sectional diameter close to D50, and select an area of ​​about 0.5 μm × 0.5 μm on the cross section of the observed particles, such as Figure 5 As shown in Table 1, based on the selected carbon, silicon and oxygen elements, the element content in the sample is scanned and analyzed.

[0208] Table 1 SEM-EDS analysis results of the internal structure of the cross-section particles of the composite negative electrode material

[0209] EDS C content, % O content, % Si content, % EDS1 90 8 2 EDS2 77 13 10 EDS3 86 10 4 EDS4 83 9 8 EDS5 55 6 39 EDS6 47 9 44 EDS7 54 9 37 EDS8 55 9 35

[0210] 11) Porous carbon carrier test: first perform SEM-EDS analysis of the cross section. Specifically, in the above-mentioned test method for the proportion of closed pore area greater than 100 nm, when observing the cross section after ion cutting with SEM, select particles with a cross-sectional diameter close to D50. On the cross section of the observed particles, select 3 areas of approximately 0.5μm×1μm, and scan and analyze the carbon content in the sample based on the selected carbon, silicon, and oxygen elements.

[0211] The ratio of the maximum carbon content to the minimum carbon content obtained by EDS analysis is taken as L, and the carrier of the composite negative electrode material whose L ranges from 1 to 1.2 is the porous carbon carrier described in the present invention.

[0212] The electrochemical properties of the materials obtained in Examples 1-10 and Comparative Examples 1-5 were tested and characterized:

[0213] 1) The first efficiency test of composite negative electrode material gram capacity

[0214] Preparation of pole piece: the above-mentioned composite negative electrode material, carbon nanotubes, lithium carboxymethyl cellulose and lithium polyacrylate are mixed in a mass ratio of 93.2:0.4:1.4:5 to prepare a slurry, and after mixing, an appropriate amount of solvent deionized water is added, and a negative electrode slurry is obtained under the action of a homogenizer, wherein the solid content of the negative electrode slurry is 25wt%; the slurry after stirring and mixing is coated on a copper foil current collector, and the coated pole piece is placed in a vacuum oven, and dried under vacuum conditions at 90°C for 12 hours to obtain a negative electrode pole piece; the loading amount of the composite negative electrode material is 6.1mg / cm 2 .

[0215] Preparation of electrolyte: In an argon atmosphere glove box, the water content is less than 10ppm, and the lithium salt LiPF6 and the non-aqueous organic solvent, ethylene carbonate (EC): diethyl carbonate (DEC): propylene carbonate (PC): propyl propionate (PP): fluoroethylene carbonate (FEC) = 20:30:20:25:5, the mass ratio of which is 8:92 to prepare the electrolyte.

[0216] Preparation of isolation membrane: A commercially available polyethylene (PE) porous polymer film with a thickness of 7 μm was used as the isolation membrane, and was punched into 10 mm small discs.

[0217] Battery assembly: The above-mentioned pole pieces are punched into circular pole pieces with a diameter of 10 mm; the metal lithium sheet is used as the counter electrode, and is also punched into small round pieces of 10 mm. They are assembled in a glove box with an argon atmosphere. The assembly order is negative electrode shell → steel sheet → lithium sheet → isolation membrane → electrolyte → negative electrode sheet → steel sheet → spring → positive electrode shell → sealing. They are assembled into button batteries. To ensure sufficient infiltration of the electrolyte, the button battery is left to stand for 6 hours after assembly, and then a blue-electricity test is performed.

[0218] Battery test: The charge and discharge cut-off voltages are 2V and 0.005V respectively. The test process is 0.1C discharge to 0.005V, 0.05C discharge to 0.005V, stand for 10min, 0.01C discharge to 0.005V, stand for 10min, record the first discharge capacity; 0.05C charge to 2.0V, stand for 10min, record the first charge capacity. The test process is repeated for 2 cycles. The first discharge specific capacity = the first discharge capacity / the mass of the composite negative electrode material, the first charge specific capacity = the first charge capacity / the mass of the composite negative electrode material; the first efficiency of the composite negative electrode material = (the first charge specific capacity / the first discharge specific capacity) × 100%; the gram capacity of the composite negative electrode material is the first charge specific capacity.

[0219] The test results are shown in Table 2 and Table 3.

[0220] 2) 0.8V capacity ratio test of composite negative electrode material: 0.8V capacity ratio = (specific capacity when charged to 0.8V for the first time / specific capacity when charged for the first time) × 100%.

[0221] 3) DQ / DV primary and secondary peak intensity ratio test

[0222] The first charge and discharge curve of the composite negative electrode material is obtained by blue electric test, such as Figure 3-1 As shown, the charge-discharge specific capacity is the horizontal axis and the voltage is the vertical axis;

[0223] The first cycle charge capacity is recorded as Q and the voltage is recorded as V. The data obtained by differential calculation is used as the horizontal axis and the voltage V is used as the vertical axis to obtain the DQ / DV-V differential capacity curve, as shown in Figure 3-2 As shown; to obtain a smoother curve, the interval difference method can be selected, for example, the first point of DQDV = (Q10-Q1) / (V10-V1), the second point of DQDV = (Q11-Q2) / (V11-V2), the third point of DQDV = (Q12-Q3) / (V12-V3), and so on. Among them, Q1, Q2, Q3, Q10, Q11, Q12 are the abscissa specific capacity values ​​of the first point, the second point, the third point, the tenth point, the eleventh point, and the twelfth point of the first cycle charge specific capacity-voltage curve, and V1, Q2, Q3, Q10, Q11, Q12 are the ordinate voltage values ​​of the first point, the second point, the third point, the tenth point, the eleventh point, and the twelfth point of the first cycle charge specific capacity-voltage curve.

[0224] From the figure, we can see that the characteristic peak at 0.24V-0.35V is the main peak, the highest peak intensity in this voltage range is recorded as I1, and the characteristic peak at 0.38V-0.45V is the secondary peak, the highest peak intensity in this voltage range is recorded as I2, and the lowest peak intensity between 0.24V and 0.45V is recorded as I3. The DQ / DV main and secondary peak intensity ratio = (I2-I3) / (I1-I3); from the publicly available data, different characteristic peaks correspond to different electrochemical reactions. The characteristic peak of I1 represents the highest value of the delithiation reaction of amorphous LixSi, and the characteristic peak of I2 represents the highest value of the delithiation reaction of crystalline Li15Si4. The more delithiation reactions there are, the higher the corresponding peak intensity. Since the formation of Li15Si4 has a very large expansion ratio for the Si lattice, it is not conducive to the stability of the lattice and the stability of the electrolyte. The DQ / DV major and minor peak intensity ratio needs to be controlled within a certain range, with the preferred range being 1. A low major and minor peak intensity ratio is beneficial to the improvement of the cycle performance of the composite negative electrode material.

[0225] 4) Full battery cycle performance test and rate performance test

[0226] Preparation of negative electrode sheet: The above composite negative electrode material is mixed with commercially available artificial graphite in a certain proportion to obtain a mixed negative electrode active material with a specific capacity of 450mAh / g. The mixed negative electrode active material, carbon nanotubes, lithium carboxymethyl cellulose, and lithium polyacrylate are mixed in a mass ratio of 93.2:0.4:1.4:5 to prepare a slurry. After mixing, an appropriate amount of solvent deionized water is added to obtain a negative electrode slurry under the action of a Ross mixer. The solid content of the negative electrode slurry is 41wt%, and the viscosity is 1500-5000mpa*S; the stirred and mixed slurry is transferred to the silo of the coating machine, and the slurry is coated on the copper foil current collector with a transfer coating machine. The parameters of the coating machine and the series-connected drying machine are adjusted to obtain a mixed negative electrode active material with a loading of 8.1mg / cm 2 Double-sided coated electrode; the electrode is transferred to a vacuum oven and dried under vacuum conditions at 90°C for 12 hours; then it is transferred to a cold press to obtain a cold-pressed electrode with a compaction density of 1.7g / cc, and the cold-pressed electrode is transferred to a slitting machine for slitting, and finally a negative electrode with a coating area width of 70mm × length of 360mm is obtained; then the electrode ear welding and glue pasting processes are carried out.

[0227] Preparation of positive electrode sheet: The positive electrode material is 4.5V lithium cobalt oxide with a gram capacity of 180 mAh / g. The positive electrode active material lithium cobalt oxide, conductive carbon (SuperP) and binder polyvinylidene fluoride (PVDF) are dissolved in an N-methylpyrrolidone solvent system at a mass ratio of 96:2:2. The amount of solvent added is appropriately adjusted to obtain a positive electrode slurry under the action of a stirrer. The solid content of the positive electrode slurry is 65% and the viscosity is 4000-10000 mpa.s. The stirred and mixed slurry is transferred to the hopper of the coating machine, and the slurry is coated on the aluminum foil current collector with a transfer coating machine. In order to achieve a designed excess capacity of 0.08 of the negative electrode to the positive electrode, the parameters of the coating machine and the drying machine are adjusted to obtain a loading amount of 18.2 mg / cm of lithium cobalt oxide material. 2 Double-sided coated electrode; the electrode is transferred to a vacuum oven and dried under vacuum conditions at 90°C for 12 hours; then it is transferred to a cold press to obtain a cold-pressed electrode with a compaction density of 4.2g / cc, and the cold-pressed electrode is transferred to a slitting machine for slitting, and finally a positive electrode with a coating area width of 65mm × length of 355mm is obtained; then the electrode ear welding and glue pasting processes are carried out.

[0228] Preparation of electrolyte: lithium salt LiPF6 and non-aqueous solvent (ethylene carbonate (EC): diethyl carbonate (DEC): propylene carbonate (PC): propyl propionate (PP): fluoroethylene carbonate (FEC)) = 20:30:20:25:5, mass ratio) are prepared in a mass ratio of 8:92 to prepare the electrolyte.

[0229] Preparation of isolation film: A commercially available polyethylene (PE) porous polymer film with a thickness of 7 μm is used as the substrate layer. Water, inorganic particulate aluminum oxide, and a binder are mixed in a stirrer to obtain a slurry for coating, which is evenly coated on one side of the substrate layer PE to a suitable thickness, and then placed in an oven for drying to obtain the isolation film of the present invention. After being slit according to the designed size, it enters the winding machine.

[0230] Battery assembly: The negative electrode sheet, separator, and positive electrode sheet are placed in the winding machine in order, with the separator placed between the positive and negative electrode sheets, and the electrode roll is obtained after winding. The electrode roll is placed in a punched aluminum-plastic film packaging bag, and after the top seal is completed, it is transferred to a drying oven and vacuum dried at 140°C for 12 hours; the dried top-sealed electrode roll is transferred to the liquid injection machine in the drying room, and the prepared electrolyte is injected according to the amount of 1.52g / Ah; after vacuum packaging, standing, formation, degassing, trimming and other processes, a lithium-ion secondary battery is obtained.

[0231] Battery test: Cycle capacity retention rate: At a test temperature of 25°C, take the above-prepared battery and place it on a Xinwei machine for cycle performance test; charge to 4.5V at 1C and charge to 0.05C at a constant voltage for 10 minutes, discharge to 3.0V at 1C and let stand for 10 minutes, use the discharge capacity obtained in this step as the initial capacity, and perform cycle test according to this process, with the ratio of the discharge capacity of each cycle to the initial capacity as the total coordinate, and the number of cycles as the horizontal coordinate to obtain the cycle performance curve, i.e., the cycle retention rate curve. The capacity retention rate after 400 cycles = (discharge capacity of the 400th cycle / discharge capacity of the first cycle) × 100%, and the 400-cycle cycle capacity retention rate is obtained by calculation.

[0232] Rate test: At a test temperature of 25°C, take the battery prepared as above and put it on a Xinwei tester for rate performance test; charge to 4.5V at 1C and charge to 0.05C at a constant voltage for 10 min, discharge to 3.0V at 0.2C and let stand for 10 min, and the discharge capacity obtained in this step is the initial capacity; charge to 4.5V at 1C and charge to 0.05C at a constant voltage for 10 min, discharge to 3.0V at 2C and let stand for 10 min, and the discharge capacity obtained in this step is recorded as 2C capacity; 2C discharge rate = (2C discharge capacity / initial discharge capacity) × 100%, and the 2C discharge rate is obtained by calculation.

[0233] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

[0234] The powder, pole piece and battery performance test and characterization results of the materials obtained in Examples 1-10 and Comparative Examples 1-5 are shown in Table 2 and Table 3:

[0235] Table 2 Specific implementation parameters and test results of the embodiments and comparative examples

[0236]

[0237] Table 3 Specific implementation parameters and test results of the embodiments and comparative examples

[0238]

[0239] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and the scope of protection of the present invention is defined by the attached claims, description and their equivalents.

Claims

1. A composite negative electrode material comprising a porous carbon carrier and a silicon-containing material filled inside and outside the porous carbon carrier, characterized in that: 1) The compaction density of 8T powder of composite negative electrode material is PD, in g / cm 3 The specific surface area of ​​the composite negative electrode material after 8T powder compaction is B, unit m 2 / g, where 0.01≤PD / B≤6; The specific surface area of ​​the composite negative electrode material is 0.2m 2 / g to 160m 2 / g; the specific surface area of ​​the composite negative electrode material after 8T powder compaction is 0.5m 2 / g to 180m 2 / g; 2) It has low internal closed pores. The cross section after ion cutting is observed by SEM. The closed pore area of ​​the particles with a pore diameter greater than 100 nm on the cross section is C, C≤20%, C=(P / A)*100%, and the closed pore area is P. P is the sum of the pore areas of the 100 nearest neighboring particles with a pore diameter d1>100 nm, and A is the sum of the areas of the 100 nearest neighboring particles; 3) The capacity ratio of the composite negative electrode material at the first delithiation to 0.8V to the first delithiation to 2.0V is Cap, where 80%≤Cap≤98%, the gram capacity is 600-2500mAh / g, and the first efficiency is 80%-96%.

2. The composite negative electrode material according to claim 1, characterized in that 8T powder compaction density is 0.6g / cm 3 ≤PD g / cm 3 ≤1.5g / cm 3 .

3. The composite negative electrode material according to claim 1, characterized in that The mass proportion of silicon element is 10%≤X≤60%.

4. The composite negative electrode material according to claim 1, characterized in that The mass proportion of carbon element is 30%≤X≤80%.

5. The composite negative electrode material according to claim 1, characterized in that There are carbon-rich particles, which refer to the carbon content data of the EDS analysis of a region of about 0.5 μm×0.5 μm selected from the particles when observing the cross section after ion cutting under SEM, which is higher than 50% of the carbon content test data.

6. The composite negative electrode material according to claim 1, characterized in that Dv50 is 3μm to 15μm, Dv99 is 6μm to 30μm, and Dn10 is 0.5μm to 5μm.

7. The composite negative electrode material according to claim 1, characterized in that: The carbon Raman peak Id / Ig ratio is 0.05 to 1.3, and the silicon Raman peak Id / Ig ratio is 0.5-1.

2.

8. The composite negative electrode material according to claim 1, characterized in that The specific surface area of ​​its precursor porous carbon carrier is 200-4000m 2 / g, the pore volume is 0.1-2.0cc / g, and the proportion of micropores, that is, the proportion of pores less than 2nm, is greater than 50%.

9. The composite negative electrode material according to claim 1, characterized in that: The carbon element accounts for 85%-100% of the precursor porous carbon carrier, the silicon element accounts for less than 5%, and the oxygen element accounts for 0.1%-15%.

10. The composite negative electrode material according to claim 1, characterized in that: The testing method for porous carbon carriers is to use SEM to observe the cross-section after ion cutting, select particles with a cross-section diameter close to D50, and select 5 areas of approximately 0.5μm×0.5μm on the cross-section of the observed particles for EDS analysis of carbon content data. The ratio of the maximum carbon content to the minimum carbon content is taken as L, and the range of L is L<1.

2.

11. A method for preparing the composite negative electrode material according to claim 1, comprising the following steps: First, a silicon-containing material is attached to a porous carbon carrier, and then the carbon-containing material is coated. By controlling the flow rate and concentration of the silicon source gas, the pressure, temperature and reaction time in the reaction chamber, the silicon-containing material and the carbon skeleton are evenly distributed, and effective surface coating is achieved. P1: The reactor 1 equipped with the porous carbon carrier is heated to T1 and an inert gas is introduced, wherein the range of T1 is 390-650°C, and after the temperature is kept for ≤4h, a silicon source gas and a diluent gas are introduced into the reaction chamber equipped with the porous carbon carrier to perform vapor deposition 1, wherein the deposition time is t1, and the range of t1 is 2h-36h, to obtain a composite negative electrode material intermediate 1 of deposited silicon material; the surface pressure of the first reaction chamber is 0.5kPa to 200kPa; P2: Then, the reactor 1 is heated to T2, T2 ranges from 200-750°C, and after being kept warm for ≤4h, a carbon source gas and a diluent gas are introduced into the reaction chamber of P1 to perform vapor deposition 2, the deposition time is t2, t2 ranges from 0.5h to 24h, and the composite negative electrode material intermediate 2 is obtained; the surface pressure of the second reaction chamber is 0.5kPa to 200kPa; P3: Then, the composite negative electrode material intermediate 2 is transferred to the reaction chamber of the reactor 2, and the temperature is raised to T3 and an inert gas is introduced, the T3 range is 300-750°C, and after the heat preservation time is ≤4h, a carbon source gas and a dilution gas are introduced into the reaction chamber to perform vapor deposition 3, the deposition time is t3, and the t3 range is 1h-24h to obtain the composite negative electrode material; the surface pressure of the third reaction chamber is 0.1kPa to 100kPa.

12. The method for preparing a composite negative electrode material according to claim 11, characterized in that: In the P1 process, the silicon source gas includes at least one of monosilane, disilane, silicon vapor, trichlorosilane and dichlorosilane; and the diluent gas includes at least one of hydrogen, argon and nitrogen.

13. The method for preparing a composite negative electrode material according to claim 11, characterized in that: In the P2 and P3 processes, the carbon source gas comprises at least one of methane, ethylene, propylene and acetylene; and the dilution gas comprises at least one of hydrogen, argon and nitrogen.

14. The method for preparing a composite negative electrode material according to claim 11, characterized in that: In the P1 process and the P2 process, the porous carbon carrier exists in a fluidized state under the action of the airflow of the raw gas and the dilution gas, or exists in an expanded state driven by the baffles or components inside the cavity, and the volume of the dense phase zone is 1.2 to 2.5 times the volume of static stacking.

15. The method for preparing a composite negative electrode material according to claim 11, characterized in that: In the P1 process, the flow rates of the silicon source gas and the dilution gas are determined according to the weight of the porous carbon in the reaction chamber. The silicon source gas is introduced at a flow rate of 1 L / min / kg to 50 L / min / kg, and the dilution gas is introduced at a flow rate of 1 L / min / kg to 50 L / min / kg. The ratio of the silicon source gas to the dilution gas is D, and D is less than 1.

5.

16. The method for preparing a composite negative electrode material according to claim 11, characterized in that: In the P2 process, the flow rates of the carbon source gas and the dilution gas are determined according to the weight of the porous carbon in the reaction chamber. The carbon source gas is introduced at a flow rate of 1L / min / kg to 50L / min / kg, and the dilution gas is introduced at a flow rate of 1L / min / kg to 50L / min / kg. The ratio of the carbon source gas to the dilution gas is E, and E is less than 1.

5.

17. The method for preparing a composite negative electrode material according to claim 11, characterized in that: The preparation method of the porous carbon carrier includes carbonization and activation steps, the activation includes gas activation method and alkali activation method, and the carbonization step includes the following: G1: Carbonization step: Inert gas is introduced into the reaction chamber of the reactor 3 containing the carbon source precursor, and the inert gas flow rate is 0.2L / min / kg to 5L / min / kg, and the reaction chamber is heated to TG1, and the TG1 range is 400-1500°C, and a carbonization cracking reaction is carried out, and the TG1 insulation time is less than or equal to 24h; during this process, the surface pressure 1 of the reaction chamber is 0.5kpa-50kpa; after the cracking reaction, a porous carbon carrier intermediate is obtained; The gas activation method includes at least one of the following steps: G2: Activation step: The porous carbon carrier intermediate is transferred to the reaction chamber of the reactor 4, and an inert gas is passed through and the temperature is raised to TG2, the inert gas flow rate is 0.2L / min / kg to 5L / min / kg, and the TG2 range is 500-1100°C, and then an activation gas containing CO2 is passed into the reaction chamber, and the activation gas flow rate is 0.2L / min / kg to 5L / min / kg, and an activation reaction is carried out, and TG2 is kept warm for 0.1h to 80h. During this process, the surface pressure 2 of the reaction chamber is 0.5kpa-50kpa; after the activation reaction, a porous carbon carrier is obtained; Or G2': Activation step: The porous carbon carrier intermediate is transferred to the reaction chamber of the reactor 4', and an inert gas is passed and the temperature is raised to TG2', the inert gas flow rate is 0.2L / min / kg to 5L / min / kg, and the TG2' range is 200-1300°C, and then an activation gas containing H2O is passed into the reaction chamber, and the activation gas flow rate is 0.2L / min / kg to 5L / min / kg, and an activation reaction is carried out. TG2 is kept warm for 0.1h-50h. During this process, the surface pressure 2' of the reaction chamber is 0.5kpa-50kpa; a porous carbon carrier is obtained after the activation reaction.

18. The method for preparing a composite negative electrode material according to claim 17, characterized in that: The carbon source precursor in the G1 process includes at least one of a high molecular weight polymer, a biomass carbon source and a mineral carbon source.

19. The method for preparing a composite negative electrode material according to claim 17, characterized in that: The activated gas also includes at least one of CO2 and H2O.

20. The method for preparing a composite negative electrode material according to claim 17, characterized in that: The alkaline activation method comprises the following steps: determining the flow rates of the inert gas and the oxygen-containing gas according to the weight of the carbon source precursor in the reaction chamber; K1: Carbonization step: Inert gas is introduced into the reaction chamber of the reactor 5 containing the carbon source precursor, and the inert gas flow rate is 0.2L / min / kg to 5L / min / kg, and the reaction chamber is heated to TK1, TK1 range is 400-1500°C, and carbonization and cracking reaction is carried out, and TK1 is kept warm for ≤24h; During this process, the surface pressure of the third reaction chamber is 0.5kpa-50kpa; K2: Activation step: After the porous carbon carrier intermediate and the alkaline activator are fully mixed in a certain proportion, they are transferred to the reaction chamber of the reactor 6, and an inert gas is introduced and the temperature is raised to TK2, the inert gas flow rate is 0.2L / min / kg to 5L / min / kg, and the TK2 range is 400℃-1000℃, and an activation reaction is carried out. TK2 is kept warm for 0.01h-12h. During this process, the surface pressure of the fourth reaction chamber is 0.5kpa-50kpa; after the activation reaction, a porous carbon carrier intermediate is obtained; K3: passivation step: oxygen-containing gas is introduced into the reaction chamber of reactor 6 for passivation treatment, and the flow rate of oxygen-containing gas is 0.2L / min / kg to 5L / min / kg. The product after passivation treatment is porous carbon support intermediate 2; during this process, the surface pressure of the fifth reaction chamber is 0.5kpa-50kpa; The porous carbon intermediate is acid-washed, water-washed and dried to remove excess metal impurities and excess water, thereby obtaining a porous carbon carrier. The content of metal impurity elements in the porous carbon carrier is less than 100 ppm, and the water content is less than 2%.

21. The method for preparing a composite negative electrode material according to claim 20, characterized in that: In the K2 process, the alkaline activator contains KOH; the molar ratio of the porous carbon carrier intermediate to the alkaline activator is in the range of 0.2-2.

22. The method for preparing a composite negative electrode material according to claim 20, characterized in that: In the K3 process, the oxygen-containing gas contains at least one of CO2 and H2O.

23. The method for preparing a composite negative electrode material according to claim 17 or 20, characterized in that: The inert gas contains at least one of argon and helium, and is used as a protective gas.

24. The method for preparing a composite negative electrode material according to claim 20, characterized in that: Reactor 1, reactor 2, reactor 3, reactor 4, reactor 4', reactor 5 and reactor 6 are at least one of fluidized bed, vibrating bed, rotary kiln, box furnace, roller kiln and push plate kiln.

25. A secondary battery comprising a negative electrode, wherein the negative electrode comprises a negative electrode material layer, the negative electrode material layer comprises a negative electrode active material, and the negative electrode active material comprises the composite negative electrode material according to any one of claims 1 to 10 or the composite negative electrode material prepared by the preparation method according to any one of claims 11 to 24.