A lithium iron manganese phosphate positive electrode material precursor and its preparation method and positive electrode material
By adjusting the combination and reaction pH of salt, precipitant and complexing agent in the co-precipitation method, the problems of irregular morphology and poor performance of the precursor of lithium manganese iron phosphate positive electrode material were solved, and uniform nucleation of ferromanganese and iron phosphate were achieved. The morphology control improves the specific capacity and rate performance of LMFP positive electrode material.
Patent Information
- Application Number
- CN202410726392.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-05
AI Technical Summary
The precursors of the precursors of lithium manganese iron phosphate as precipitation methods have problems such as irregular morphology, uneven particle size distribution and poor performance, making it difficult to achieve atomic or molecular level mixing of Fe and Mn metal ions, resulting in poor performance. .
By adjusting the addition method of salt, precipitant and complexing agent during co-precipitation and coordination of reaction pH, uniform nucleation and morphology control of manganese manganese are achieved, and the combination of "salt solution-complexing agent-precipitation agent" is adopted and The coordination of pH in the reaction process ensures the steady state of the precipitation reaction, and prepares a precursor with uniform distribution of Mn/Fe in the crystal lattice, regular particle morphology, and uniform particle size distribution.
The precursor of lithium manganese iron phosphate positive electrode material with excellent performance was successfully prepared, which improved the specific capacity and rate performance of LMFP positive electrode material, and was suitable for large-scale industrial production.
Smart Images

Figure CN118343848B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a lithium manganese iron phosphate positive electrode material precursor and a preparation method thereof and a positive electrode material. Background Art
[0002] The large-scale use of traditional fossil fuels has led to increasingly serious problems such as resource shortages and environmental pollution. Accelerating the transformation of the energy structure has become an important goal. Among them, developing high-efficiency, high-energy-density, and low-cost energy storage devices to assist in the electrification of automobiles is a key measure to achieve this goal.
[0003] At present, lithium iron phosphate (LFP) and lithium manganese iron phosphate (LMFP) with olivine structure have attracted widespread attention in the market due to their high safety, good electrochemical performance and relatively low cost. Among them, LMFP, as an upgraded alternative material for LFP, has a higher energy density and a higher voltage platform than LFP. In addition, the cost of raw material manganese is low, so LMFP has more advantages in terms of price. In addition, compared with another ternary material, LMFP has a long cycle life, good thermal stability, high safety and no explosion risk.
[0004] The preparation method of LMFP is similar to that of LFP. Common preparation methods include solid phase method, sol-gel method, hydrothermal method, coprecipitation method, etc. Among them, the steps of preparing LMFP by coprecipitation method are usually as follows: first, mix the manganese source, iron source, etc., add the precipitant and the coordination agent, etc. to carry out coprecipitation reaction to obtain a precipitate, then wash and dry the precipitate to obtain a precursor, and finally mix the precursor with the lithium source and calcine to obtain the LMFP positive electrode material. This method mainly includes two steps: liquid phase coprecipitation (crystal nucleation and growth) and high temperature calcination. The morphological characteristics and structural characteristics of the precursor and the positive electrode material ultimately affect the electrochemical characteristics of the positive electrode material. The advantages of this method are simple operation, low equipment requirements and short reaction time, suitable for large-scale preparation, etc., but the technical difficulty lies in: how to adjust the operating conditions in the coprecipitation preparation process to make the two metal ions of Fe and Mn reach the atomic or molecular level of mixing, and obtain a precursor with regular and uniform morphology and excellent performance, so as to obtain an excellent LMFP positive electrode material.
[0005] Therefore, there is an urgent need to provide a method for preparing a lithium manganese iron phosphate positive electrode material precursor with regular and uniform morphology and excellent performance. Summary of the invention
[0006] In view of the technical problems existing in the background technology, the present application provides a lithium iron manganese phosphate positive electrode material precursor and its preparation method and positive electrode material, aiming to solve the technical problems in the prior art of preparing lithium iron manganese phosphate positive electrode material precursor by co-precipitation method, such as irregular morphology, uneven particle size distribution and poor performance.
[0007] In a first aspect, an embodiment of the present application provides a method for preparing a lithium manganese iron phosphate positive electrode material precursor, comprising the following steps:
[0008] Prepare a first mixed solution containing ferrous salt, manganese salt and a first complexing agent, a second mixed solution containing a second complexing agent and a first precipitant, a precipitant aqueous solution containing the second precipitant, and a buffer base solution containing a third precipitant and a third complexing agent; add the first mixed solution, the second mixed solution and the precipitant aqueous solution into the buffer base solution at the same time to carry out a coprecipitation reaction, and obtain a lithium manganese iron phosphate positive electrode material precursor after aging, washing and drying; wherein the pH value is maintained at 3-6 during the coprecipitation reaction; the third complexing agent is the first complexing agent and / or the second complexing agent, and the first complexing agent is different from the second complexing agent.
[0009] In the technical scheme of the embodiment of the present application, in addition to the control of conventional reaction conditions (reaction time, reaction temperature and rotation speed), the present application focuses on the matching of "salt solution-complexing agent-precipitant" and its coordination with the pH of the reaction process. Specifically, the present application stabilizes the precipitation and crystallization process of manganese and iron elements by pre-mixing salt with complexing agent; by pre-mixing different complexing agents with precipitating agents and using them as the second mixed solution and buffer bottom solution respectively, the pH of the reaction system is quickly stabilized and has a complexing effect, and the steady state of the precipitation reaction process and the liquid phase mass transfer process is achieved, as well as good control of the precipitate morphology after the reaction, and the problems of uneven particle composition and particle morphology in the co-precipitation process are solved, and the precursor material with uniform distribution of Mn / Fe in the lattice, regular particle morphology, uniform particle size distribution and excellent performance is successfully prepared. At the same time, by washing and drying the aged material, the residual metal ions, ammonium ions and sulfate ions on the surface of the material can be removed to avoid affecting the subsequent lithium addition amount and the formation of LMFP positive electrode materials. In addition, the present invention has the advantages of simple operation, easy control of reaction conditions, low cost, etc., and is suitable for large-scale industrial production.
[0010] In some embodiments, the ferrous salt includes one or more of ferrous sulfate, ferrous nitrate, ferrous oxalate and ferrous chloride; the manganese salt includes one or more of manganese sulfate, manganese nitrate, manganese acetate, manganese oxalate and manganese chloride; the first chelating agent includes one or more of citric acid, sodium citrate, ascorbic acid, lactic acid and malic acid; the second chelating agent includes one or more of ammonia water, ethylenediaminetetraacetic acid, diisopropylaminotetraacetic acid and tris(2-aminoethyl)triacetic acid; the third chelating agent includes one or more of citric acid, sodium citrate, ammonia water, ascorbic acid, lactic acid and malic acid; the first precipitant includes one or more of phosphoric acid, diammonium hydrogen phosphate, diammonium dihydrogen phosphate and ammonium phosphate; the second precipitant includes one or more of phosphoric acid, diammonium hydrogen phosphate, diammonium dihydrogen phosphate and ammonium phosphate; the third precipitant includes one or more of phosphoric acid, diammonium hydrogen phosphate, diammonium dihydrogen phosphate and ammonium phosphate.
[0011] In this embodiment, by selecting the above-mentioned first complexing agent, ferrous ions can be preferentially complexed rather than manganese ions, thereby inhibiting the oxidation of divalent ferrous ions; by selecting the above-mentioned second complexing agent, the co-complexation of ferromanganese can be achieved; by selecting the above-mentioned third complexing agent, the ferromanganese in the system can be quickly complexed to prevent phase segregation; by selecting the above-mentioned first precipitant, second precipitant and third precipitant, the co-precipitation of ferromanganese can be achieved, and the pH of the reaction process can be stabilized to obtain a ferromanganese phosphate co-precipitation precursor.
[0012] In some embodiments, in the first mixed solution, the total concentration of manganese ions and ferrous ions is 10~120g / L, and the concentration of the first chelating agent is 2~10g / L; in the second mixed solution, the mass ratio of the second chelating agent to the first precipitant is 1:(0.2~0.6).
[0013] In this embodiment, by selecting the above-mentioned concentration range of manganese ions and ferrous ions, co-precipitation of ferromanganese can be achieved. Too high ion concentration is likely to cause partial oxidation of ferrous ions, leading to element segregation, and too low ion concentration causes reduced precipitation efficiency; by selecting the above-mentioned concentration range of the first complexing agent, ferrous ions can be effectively complexed to prevent ferrous ions from being oxidized before participating in the reaction. Too high a concentration of the first complexing agent will cause a decrease in the precipitation rate of some ferrous ions during the co-precipitation process, and too low a concentration is not conducive to protecting the ferrous ions in the first mixed solution; by controlling the ratio of the second complexing agent to the first precipitant in the second mixed solution within the above-mentioned range, the pH of the co-precipitation reaction process can be stabilized, and co-complexation and co-precipitation of ferromanganese can be achieved. Too low a ratio will cause the second mixed solution to be unable to play a role in regulating pH, and too high a ratio will easily lead to a decrease in the complexing ability of the second mixed solution for ferromanganese ions, which is not conducive to the homogeneous precipitation of the precursor.
[0014] In some embodiments, in the precipitant aqueous solution, the concentration of the second precipitant is 10-120 g / L; in the buffer base solution, the concentration of the third complexing agent is 2-10 g / L, the concentration of the third precipitant is 6-80 g / L, and the pH of the buffer base solution is 2-6.
[0015] In this embodiment, in the precipitant aqueous solution, by selecting the concentration range of the second precipitant mentioned above, uniform nucleation of manganese and iron ions can be achieved. If the concentration of the second precipitant is too high, the precursor particles will be larger, and if the concentration of the second precipitant is too low, the co-precipitation reaction rate will be reduced. By controlling the pH of the buffer base solution within the above range, the pH during the reaction can be stabilized, and at the same time, it is easy to achieve precipitation of manganese and iron in different proportions. If the pH of the buffer base solution is too high or too low, it will cause crystal phase segregation.
[0016] In some embodiments, the volume ratio of the first mixed solution, the second mixed solution, the precipitant aqueous solution and the buffer base solution is (1-3):(2-9):(2-9):1.
[0017] In this embodiment, by controlling the ratio of the buffer base solution to the first mixed solution, the second mixed solution and the precipitant aqueous solution within the range, manganese and iron co-complexation and co-precipitation can be achieved, and the pH of the reaction process can be stabilized.
[0018] In some embodiments, during the co-precipitation reaction, the temperature of the co-precipitation reaction is 50~60°C, and the pH value of the reaction system is 4~4.5; and / or, during the aging process, the aging temperature is 50~60°C, the aging time is 1~6h, and the pH value of the reaction system is 4~4.5.
[0019] In this embodiment, by controlling the pH of the co-precipitation reaction process within this range, stable co-precipitation of manganese and iron in different proportions can be achieved; if the pH is too low, it will result in more iron precipitation and too little manganese precipitation; if the pH is too high, it will result in too much manganese precipitation and too little iron precipitation; by controlling the temperature of the co-precipitation reaction process within this range, the co-precipitation reaction rate can be accelerated; if the temperature is too low, the reaction rate will be too slow and the reaction degree will be low; if the temperature is too high, the pH meter equipment will be damaged and the precursor will be oxidized.
[0020] In a second aspect, an embodiment of the present application provides a lithium iron manganese phosphate positive electrode material precursor, which is obtained by the preparation method of the lithium iron manganese phosphate positive electrode material precursor provided in the first aspect of the present application.
[0021] In the technical solution of the embodiment of the present application, the manganese and iron elements in the lithium manganese iron phosphate positive electrode material precursor of the present application are evenly distributed in the lattice, the product particles have regular morphology, uniform particle size distribution and excellent performance, and all have olivine morphology; the LMFP positive electrode material prepared from the precursor has a higher specific capacity and better rate performance.
[0022] In a third aspect, an embodiment of the present application provides a lithium iron manganese phosphate positive electrode material, which is prepared by a high-temperature solid phase method after evenly mixing the lithium iron manganese phosphate positive electrode material precursor provided by the second aspect of the present application with a lithium source.
[0023] The LMFP positive electrode material of the present application is prepared from the above-mentioned lithium manganese iron phosphate positive electrode material precursor, and thus has the advantages of high specific capacity and good rate performance.
[0024] In a fourth aspect, an embodiment of the present application provides a positive electrode plate, comprising the lithium iron manganese phosphate positive electrode material provided in the third aspect of the present application.
[0025] The positive electrode plate of the present application includes the above-mentioned LMFP positive electrode material, and thus has the advantages of high specific capacity and good rate performance.
[0026] In a fifth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate provided in the fourth aspect of the present application.
[0027] The secondary battery of the present application includes the above-mentioned positive electrode plate, and thus has the advantages of high specific capacity and good rate performance.
[0028] Compared with the prior art, the beneficial effects of this application include:
[0029] The present application stabilizes the actual precipitation reaction process by controlling the feeding method of the salt, precipitant, and complexing agent in the co-precipitation system and the pH of the reaction process, thereby achieving uniform nucleation of the product without phase separation, and the product is uniform and has a controllable morphology, all of which have a good olivine morphology; at the same time, the overall preparation process of the present application is simple, and there is no need for mixing (ball milling, sand milling, etc.) and granulation (spray drying) process flows.
[0030] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 A process flow chart of an embodiment of a method for preparing a lithium manganese iron phosphate positive electrode material precursor provided in an embodiment of the present application;
[0033] Figure 2 This is a morphology image of the lithium manganese iron phosphate positive electrode material precursor obtained in Example 1 of the present application at a magnification of 10000X;
[0034] Figure 3 This is a morphology image of the lithium manganese iron phosphate positive electrode material precursor obtained in Example 4 of the present application at a magnification of 10000X;
[0035] Figure 4 This is a morphology image of the lithium manganese iron phosphate positive electrode material precursor obtained in Comparative Example 1 of the present application at a magnification of 5000X;
[0036] Figure 5 This is a morphology image of the lithium manganese iron phosphate positive electrode material precursor obtained in Comparative Example 2 of the present application at a magnification of 10000X;
[0037] Figure 6 This is a morphology image of the lithium manganese iron phosphate positive electrode material precursor obtained in Comparative Example 3 of the present application at a magnification of 10000X;
[0038] Figure 7 This is a morphology image of the lithium manganese iron phosphate positive electrode material precursor obtained in Comparative Example 4 of the present application at a magnification of 50000X;
[0039] Figure 8 The rate performance of the LMFP positive electrode material obtained in Example 1 of the present application at 2-4.35V;
[0040] Fig. 9 The rate performance of the LMFP positive electrode material obtained in Example 4 of the present application at 2-4.35V;
[0041] Fig.10 This is the rate performance of the LMFP positive electrode material obtained in Comparative Example 1 of the present application at 2-4.35V. DETAILED DESCRIPTION
[0042] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0044] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0045] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0046] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0047] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0048] Coprecipitation is a commonly used method for preparing positive electrode materials, and this method can be used to prepare high-performance LMFP positive electrode materials. The steps for preparing LMFP by coprecipitation are usually: first mix the manganese source, iron source, etc., then add the precipitant and the ligand, etc. to carry out coprecipitation reaction, and finally wash, dry, mix and calcine the precipitate with the lithium source to obtain the LMFP material. In the process of preparing lithium manganese iron phosphate by coprecipitation, it is necessary to regulate the operating conditions in the coprecipitation preparation process so that the two metal ions of Fe and Mn can be mixed at the atomic or molecular level to obtain a precursor with regular and uniform morphology and excellent performance, thereby obtaining an excellent performance LMFP positive electrode material.
[0049] In order to solve the technical problems of uneven mixing of iron and manganese metal ions and uneven product morphology in the preparation of lithium iron manganese phosphate positive electrode material precursors by coprecipitation in the prior art, the present application provides a lithium iron manganese phosphate positive electrode material precursor and its preparation method and positive electrode material. In the preparation method of the lithium iron manganese phosphate positive electrode material precursor provided by the present application, the morphology of the precursor is regulated by adjusting the addition method of salt, precipitant and complexing agent and the reaction pH during the coprecipitation process, so that the precursor particles are uniform and have an olivine morphology; the LMFP positive electrode material prepared from the precursor has a higher specific capacity and better rate performance, and thus the specific capacity and rate performance of the positive electrode sheet and the secondary battery are also improved.
[0050] Please refer to Figure 1 In a first aspect, an embodiment of the present application provides a method for preparing a lithium manganese iron phosphate positive electrode material precursor, comprising the following steps:
[0051] S1, preparing a first mixed solution containing a ferrous salt, a manganese salt and a first complexing agent, a second mixed solution containing a second complexing agent and a first precipitant, a precipitant aqueous solution containing a second precipitant, and a buffered bottom solution containing a third precipitant and a third complexing agent;
[0052] S2, adding the first mixed solution, the second mixed solution and the precipitant aqueous solution into the buffer base solution at the same time to carry out a co-precipitation reaction, and obtaining a lithium manganese iron phosphate positive electrode material precursor after aging, washing and drying;
[0053] The pH value is maintained at 3-6 during the coprecipitation reaction; the third complexing agent is the first complexing agent and / or the second complexing agent, and the first complexing agent is different from the second complexing agent.
[0054] In addition to the control of conventional reaction conditions (reaction time, reaction temperature and rotation speed), this application focuses on the matching of "salt solution-complexing agent-precipitant" and its coordination with the pH of the reaction process. Specifically, this application stabilizes the precipitation and crystallization process of manganese and iron elements by pre-mixing salt with complexing agent; by pre-mixing different complexing agents with precipitating agents and using them as the second mixed solution and buffer base solution respectively, the pH of the reaction system is quickly stabilized and has a complexing effect, and the steady state of the precipitation reaction process and the liquid phase mass transfer process is achieved, as well as good control of the morphology of the precipitate after the reaction, and the problems of uneven particle composition and particle morphology in the co-precipitation process are solved, and the precursor material with uniform distribution of Mn / Fe in the lattice, regular particle morphology, uniform particle size distribution and excellent performance is successfully prepared. At the same time, by washing and drying the aged material, the residual metal ions, ammonium ions and sulfate ions on the surface of the material can be removed to avoid affecting the subsequent lithium addition amount and the formation of LMFP positive electrode materials. In addition, the present invention has the advantages of simple operation, easy control of reaction conditions, low cost, etc., and is suitable for large-scale industrial production.
[0055] Further, in some embodiments, in step S1, the ferrous salt includes one or more of ferrous sulfate, ferrous nitrate, ferrous oxalate and ferrous chloride; typical but non-limiting combinations include a combination of ferrous sulfate and ferrous nitrate, a combination of ferrous sulfate and ferrous oxalate, a combination of ferrous sulfate and ferrous chloride, and a combination of ferrous sulfate and ferrous nitrate, ferrous oxalate and ferrous chloride.
[0056] Further, in some embodiments, in step S1, the manganese salt includes one or more of manganese sulfate, manganese nitrate, manganese acetate, manganese oxalate and manganese chloride; typical but non-limiting combinations include a combination of manganese sulfate and manganese nitrate, a combination of manganese sulfate and manganese acetate, a combination of manganese sulfate and manganese oxalate, a combination of manganese sulfate and manganese chloride, a combination of manganese nitrate and manganese acetate, a combination of manganese nitrate and manganese oxalate, a combination of manganese nitrate and manganese chloride, a combination of manganese acetate and manganese oxalate, a combination of manganese acetate and manganese chloride, a combination of manganese oxalate and manganese chloride, a combination of manganese sulfate, manganese nitrate and manganese acetate, or a combination of manganese sulfate, manganese nitrate, manganese acetate, manganese oxalate and manganese chloride.
[0057] Further, in some embodiments, in step S1, the first complexing agent includes one or more of citric acid, sodium citrate, ascorbic acid, lactic acid and malic acid; typical but non-limiting combinations include a combination of citric acid and sodium citrate, a combination of citric acid and ascorbic acid, a combination of citric acid and lactic acid, and a combination of citric acid and malic acid.
[0058] In the technical solution of the embodiment of the present application, by selecting the above-mentioned first complexing agent, ferrous ions rather than manganese ions can be preferentially complexed, thereby inhibiting the oxidation of ferrous ions.
[0059] Further, in some embodiments, in step S1, in the first mixed solution, the total concentration of manganese ions and ferrous ions is 10-120 g / L, including but not limited to any point value of 10 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L, 100 g / L, 110 g / L or 120 g / L or the range value between any two of them.
[0060] In the technical solution of the embodiment of the present application, by selecting the above-mentioned concentration range of manganese ions and ferrous ions, the co-precipitation of manganese and iron can be achieved. Too high ion concentration can easily cause partial oxidation of ferrous ions, leading to element segregation, and too low ion concentration can reduce precipitation efficiency.
[0061] The present application does not limit the molar ratio of ferrous ions to manganese ions in the first mixed solution, and those skilled in the art may make adjustments according to the actual process. Further, in some embodiments, the molar ratio of ferrous ions to manganese ions is 1: (0.01-100), including but not limited to any point value of 1:0.01, 1:0.1, 1:1, 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100 or any range value between two of them.
[0062] Further, in some embodiments, in step S1, in the first mixed solution, the concentration of the first complexing agent is 2-10 g / L, including but not limited to any point value of 2 g / L, 3 g / L, 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L or a range value between any two of them.
[0063] In the technical solution of the embodiment of the present application, by selecting the concentration range of the above-mentioned first complexing agent, ferrous ions can be effectively complexed to prevent the ferrous ions from being oxidized before participating in the reaction. If the concentration of the first complexing agent is too high, the precipitation rate of some ferrous ions will be reduced during the co-precipitation process, and if the concentration is too low, it will not be conducive to protecting the ferrous ions in the first mixed solution.
[0064] Further, in some embodiments, in step S1, the second complexing agent includes one or more of ammonia water, ethylenediaminetetraacetic acid (EDTA), diisopropylaminotetraacetic acid (DTPA) and tris(2-aminoethyl)triacetic acid (TTHA); typical but non-limiting combinations include a combination of ammonia water and EDTA, a combination of ammonia water and DTPA, and a combination of ammonia water and TTHA.
[0065] In the technical solution of the embodiment of the present application, by selecting the above-mentioned second complexing agent, the co-complexation of manganese and iron can be achieved.
[0066] Further, in some embodiments, in step S1, in the second mixed solution, the concentration of the second complexing agent is 5-20 g / L, including but not limited to 5 g / L, 7 g / L, 9 g / L, 11 g / L, 13 g / L, 15 g / L, 17 g / L, and 20 g / L; the concentration of the precipitant is 1-12 g / L, including but not limited to any one of 1 g / L, 3 g / L, 5 g / L, 7 g / L, 9 g / L, and 12 g / L or a range between any two of them.
[0067] In the technical solution of the embodiment of the present application, by selecting the concentration range of the second complexing agent mentioned above, effective complexation of manganese and iron ions can be achieved. If the concentration of the second complexing agent is too high, the precipitation reaction rate will be reduced, and if the concentration is too low, a heterogeneous manganese and iron co-precipitation precursor will be easily formed.
[0068] Further, in some embodiments, in step S1, in the second mixed solution, the mass ratio of the second complexing agent to the first precipitant is 1:(0.2~0.6), including but not limited to any point value of 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6 or a range value between any two of them.
[0069] In the technical solution of the embodiment of the present application, by controlling the ratio of the second complexing agent to the first precipitant in the second mixed liquid within the above-mentioned range, the pH of the co-precipitation reaction process can be stabilized to achieve co-complexation and co-precipitation of manganese and iron. If the ratio is too low, the second mixed liquid will be unable to play the role of regulating pH, and if the ratio is too high, it will easily lead to a decrease in the complexing ability of the second mixed liquid for manganese and iron ions, which is not conducive to the homogeneous precipitation of the precursor.
[0070] Further, in some embodiments, in step S1, the concentration of the second precipitant in the precipitant aqueous solution is 10-120 g / L, including but not limited to any point value of 10 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L, 100 g / L, 110 g / L or 120 g / L or a range value between any two of them.
[0071] In the technical solution of the embodiment of the present application, in the precipitant aqueous solution, by selecting the concentration range of the above-mentioned second precipitant, uniform nucleation of manganese and iron ions can be achieved. If the concentration of the second precipitant is too high, the precursor particles will be larger, and if the concentration is too low, the co-precipitation reaction rate will be reduced.
[0072] Further, in some embodiments, in step S1, the third complexing agent includes one or more of citric acid, sodium citrate, ammonia water, ascorbic acid, lactic acid and malic acid; typical but non-limiting combinations include a combination of citric acid and sodium citrate, a combination of citric acid and ascorbic acid, a combination of citric acid and lactic acid, and a combination of citric acid and malic acid.
[0073] In the technical solution of the embodiment of the present application, by selecting the third complexing agent mentioned above, the manganese iron in the system can be quickly complexed to prevent phase segregation.
[0074] Further, in some embodiments, in step S1, in the buffer base solution, the concentration of the third complexing agent is 2-10 g / L, including but not limited to any one of 2 g / L, 3 g / L, 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, and 10 g / L or a range between any two of them; the concentration of the third precipitant is 6-80 g / L, including but not limited to any one of 6 g / L, 12 g / L, 18 g / L, 24 g / L, 30 g / L, 36 g / L, 42 g / L, 48 g / L, 54 g / L, 60 g / L, 66 g / L, 72 g / L, 78 g / L, and 80 g / L or a range between any two of them.
[0075] Further, in some embodiments, in step S1, the pH value of the buffer base solution is 2-6 by adjusting the ratio of the third precipitant and the third complexing agent, including but not limited to any point value of 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6 or a range value between any two of them.
[0076] In the technical solution of the embodiment of the present application, by controlling the pH of the buffer base solution within the above range, the pH during the reaction can be stabilized, and at the same time, it is convenient to achieve the precipitation of manganese iron in different proportions. Too high or too low pH of the buffer base solution will cause crystal phase segregation.
[0077] Further, in some embodiments, in step S1, in the buffer base solution, the molar ratio of the third complexing agent to the third precipitating agent is 1:(1-8), including but not limited to any one of 1:1, 1:3, 1:5, 1:7, 1:8 or a range between any two of them.
[0078] In the technical solution of the embodiment of the present application, by controlling the ratio of the third complexing agent to the third precipitant in the buffer base solution within the above-mentioned range, the pH required for the reaction can be controlled in advance within the range in which manganese iron can be precipitated. Both too high and too low ratios of the third complexing agent to the third precipitant are not conducive to the rapid stabilization of the pH during the co-precipitation reaction.
[0079] Further, in some embodiments, in step S1, the first precipitant, the second precipitant and the third precipitant all include one or more of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate; typical but non-limiting combinations include a combination of phosphoric acid and diammonium hydrogen phosphate, a combination of phosphoric acid and diammonium hydrogen phosphate, a combination of phosphoric acid and diammonium hydrogen phosphate, a combination of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate.
[0080] In the technical solution of the embodiment of the present application, by selecting the above-mentioned precipitant, the co-precipitation of manganese and iron can be achieved, and the pH of the reaction process can be stabilized to obtain a co-precipitation precursor of manganese and iron phosphate.
[0081] Further, in some embodiments, in step S1, the process of preparing a first mixed solution containing ferrous salt, manganese salt and a first complexing agent includes: dissolving the ferrous salt, manganese salt and the first complexing agent into water to prepare a first mixed solution; the process of preparing a second mixed solution containing a second complexing agent and a first precipitant includes: dissolving the second complexing agent and the first precipitant into water to prepare a second mixed solution; the process of preparing a precipitant aqueous solution containing the second precipitant includes: dissolving the second precipitant into water to prepare a precipitant aqueous solution; the process of preparing a buffer base solution containing a third precipitant and a third complexing agent includes: dissolving the third complexing agent and the third precipitant into water to prepare a buffer base solution.
[0082] Further, in some embodiments, in step S2, during the coprecipitation reaction, the pH value of the reaction system is 4-4.5, including but not limited to any point value of 4.0, 4.1, 4.2, 4.3, 4.4, 4.5 or a range value between any two of them, and the pH fluctuation range is controlled not to exceed ±0.01 during the reaction.
[0083] In the technical solution of the embodiment of the present application, by controlling the pH of the co-precipitation reaction process within this range, stable co-precipitation of manganese and iron in different proportions can be achieved; if the pH is too low, it will result in more iron precipitation and too little manganese precipitation; if the pH is too high, it will result in too much manganese precipitation and too little iron precipitation.
[0084] Further, in some embodiments, in step S2, during the coprecipitation reaction, the temperature of the reaction system is 50-60°C, including but not limited to any point value of 50°C, 52°C, 54°C, 56°C, 58°C, 60°C or a range value between any two of them.
[0085] In the technical solution of the embodiment of the present application, by controlling the temperature of the co-precipitation reaction process within this range, the co-precipitation reaction rate can be accelerated; if the temperature is too low, the reaction rate will be too slow and the reaction degree will be low; if the temperature is too high, the pH meter equipment will be damaged and the precursor will be oxidized.
[0086] In the technical solution of the embodiment of the present application, during the entire coprecipitation reaction, the temperature is maintained constant and the pH in the reactor is stable to ensure that the reaction in the solution proceeds fully.
[0087] Further, in some embodiments, in step S2, during the co-precipitation reaction, the co-precipitation reaction time is 2 to 24 hours, including but not limited to any point value of 2 hours, 6 hours, 10 hours, 14 hours, 18 hours or 24 hours or a range value between any two of them.
[0088] Furthermore, in some embodiments, in step S2, the coprecipitation reaction is carried out under stirring conditions.
[0089] The stirring speed of the coprecipitation reaction is 200-1000 rpm, including but not limited to any one of 200 rpm, 400 rpm, 600 rpm, 800 rpm, and 1000 rpm or a range between any two of them.
[0090] In the technical solution of the embodiment of the present application, by controlling the stirring speed of the co-precipitation reaction within this range, it is possible to achieve uniform particle size of the precursor. Too low a stirring speed will make it difficult for the precursor particles to grow, and too high a stirring speed will destroy the secondary particle structure of the precursor.
[0091] Furthermore, in some embodiments, in step S2, the coprecipitation reaction is carried out under an inert gas.
[0092] Furthermore, in some embodiments, the protective gas includes nitrogen, argon, etc., which is not limited in the present application.
[0093] Further, in some embodiments, in step S2, the process of simultaneously adding the first mixed liquid, the second mixed liquid and the precipitant aqueous solution to the buffer base liquid for co-precipitation reaction includes: adding the buffer base liquid to the reactor, and then injecting the first mixed liquid, the second mixed liquid and the precipitant aqueous solution into the reactor that has been preheated to the co-precipitation reaction temperature and filled with protective gas through a peristaltic pump, and constantly stirring.
[0094] Among them, parallel flow injection means that each solution starts to be injected into the reactor at the same time, and the injection time is exactly the same, ensuring that each component participates in the reaction at each moment of the reaction and ensuring the uniformity of the mixed slurry components. However, during the parallel flow injection process, the flow rates of each component can be the same or different, depending on actual needs.
[0095] In the technical solution of the embodiment of the present application, by adopting the above-mentioned injection method, the feeding rate can be more accurately controlled and the pH value in the solution can be stabilized.
[0096] Furthermore, in some embodiments, in step S2, during the co-precipitation reaction, the time of parallel flow injection is 2 to 24 hours, including but not limited to any point value of 2 hours, 6 hours, 10 hours, 14 hours, 18 hours or 24 hours or a range value between any two of them.
[0097] In the technical solution of the embodiment of the present application, by controlling the injection time within this range, element segregation can be reduced, which is beneficial to the homogenization of the precursor morphology. If the injection time is too short (i.e., the flow rate is too fast), it is difficult to achieve effective co-complexation of manganese and iron, and if the injection time is too long (i.e., the flow rate is too slow), the synthesis efficiency will be reduced.
[0098] Furthermore, in some embodiments, in step S2, during the coprecipitation reaction, the flow rate of the first mixed solution is 0.5-5 mL / min, including but not limited to any one of 0.5 mL / min, 1 mL / min, 1.5 mL / min, 2 mL / min, 2.5 mL / min, 3 mL / min, 3.5 mL / min, 4 mL / min, 4.5 mL / min or 5 mL / min or a range between any two of them; the flow rate of the second mixed solution is 1-15 mL / min, including but not limited to 1 mL / min, 2 mL / min, 3.5 mL / min, 4 mL / min, 4.5 mL / min or 5 mL / min; in, 4mL / min, 6mL / min, 8mL / min, 10mL / min, 12mL / min, 14mL / min, 15mL / min, any one of the point values or any range values between two of them; the flow rate of the precipitant aqueous solution is 1-15mL / min, including but not limited to 1mL / min, 2mL / min, 4mL / min, 6mL / min, 8mL / min, 10mL / min, 12mL / min, 14mL / min, 15mL / min, any one of the point values or any range values between two of them.
[0099] Further, in some embodiments, in step S2, during the aging process, the aging temperature is 50-60°C, including but not limited to any one of 50°C, 52°C, 54°C, 56°C, 58°C, 60°C or a range between any two of them; the aging time is 1-6h, including but not limited to any one of 1h, 2h, 3h, 4h, 5h or 6h or a range between any two of them; the pH of the reaction system is 4-4.5, including but not limited to any one of 4, 4.1, 4.2, 4.3, 4.4, 4.5 or a range between any two of them.
[0100] Furthermore, in some embodiments, the aging process is performed under stirring and inert gas conditions.
[0101] Furthermore, in some embodiments, the stirring speed of the aging process is 200-1000 rpm, including but not limited to any point value of 200 rpm, 400 rpm, 600 rpm, 800 rpm or 1000 rpm or a range value between any two of them.
[0102] In the technical solution of the embodiment of the present application, by controlling the stirring speed of the aging process within this range, the morphology of the precursor particles can be regularized and the particle size can be uniform. Too low a stirring speed is not conducive to regularizing the particle morphology, and too high a stirring speed is not conducive to the aggregation growth of the precipitated particles.
[0103] Furthermore, in some embodiments, the inert gas includes nitrogen, argon, etc., which is not limited in the present application.
[0104] Furthermore, in some embodiments, the precipitate obtained after aging is washed until the conductivity of the deionized water in the washing solution is 50-150 μS / cm.
[0105] Furthermore, in some embodiments, the drying temperature is 60-120° C., and the drying time is 6-12 hours.
[0106] Further, in some embodiments, in step S2, the volume ratio of the buffer base solution used to the first mixed solution is 1:(1-3), including but not limited to any one of 1:1, 1:1.5, 1:2, 1:2.5, 1:3 or a range value between any two of them; the volume ratio of the buffer base solution used to the second mixed solution is 1:(2-9), including but not limited to any one of 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or a range value between any two of them; the volume ratio of the buffer base solution used to the precipitant aqueous solution is 1:(2-9), including but not limited to 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9.
[0107] In a second aspect, an embodiment of the present application provides a lithium iron manganese phosphate positive electrode material precursor, and the lithium iron manganese phosphate positive electrode material precursor is obtained by the preparation method of the lithium iron manganese phosphate positive electrode material precursor provided in the first aspect of the present application.
[0108] The manganese and iron elements in the lithium manganese iron phosphate positive electrode material precursor of the present application are evenly distributed in the lattice, the product particles have regular morphology, uniform particle size distribution and excellent performance, and all have olivine morphology; the LMFP positive electrode material prepared from the precursor has a higher specific capacity and better rate performance.
[0109] In a third aspect, an embodiment of the present application provides a lithium iron manganese phosphate positive electrode material, which is prepared by a high-temperature solid phase method after evenly mixing the lithium iron manganese phosphate positive electrode material precursor provided by the second aspect of the present application with a lithium source.
[0110] The LMFP positive electrode material of the present application is prepared from the above-mentioned lithium manganese iron phosphate positive electrode material precursor, and thus has the advantages of high specific capacity and good rate performance.
[0111] Furthermore, in some embodiments, the molar ratio of the lithium manganese iron phosphate positive electrode material precursor to the lithium source is 1: (1-1.03).
[0112] Further, in some embodiments, the lithium source is lithium carbonate.
[0113] Furthermore, in some embodiments, a carbon source is added to the lithium manganese iron phosphate positive electrode material precursor and the lithium source after they are evenly mixed.
[0114] Furthermore, in some embodiments, the molar ratio of the lithium manganese iron phosphate positive electrode material precursor to the carbon source is 1: (0.01~0.2).
[0115] Furthermore, in some embodiments, the carbon source is selected from one or more of glucose, sucrose, fructose, cellulose, starch, citric acid, polyacrylic acid, polyethylene glycol and dopamine.
[0116] Furthermore, in some embodiments, the lithium manganese iron phosphate positive electrode material precursor and the lithium source are mixed evenly by grinding.
[0117] Furthermore, in some embodiments, the high temperature solid phase method is high temperature gradient calcination.
[0118] Furthermore, in some embodiments, during the high temperature gradient calcination process, the calcination temperature of the first stage is 350-450°C, including but not limited to any one of 350°C, 370°C, 390°C, 410°C, 430°C, 450°C or any range between two thereof; the holding time of the first stage is 2-6h, including but not limited to any one of 2h, 3h, 4h, 5h, 6h or any range between two thereof; the calcination temperature of the second stage is 760-790°C, including but not limited to any one of 760°C, 770°C, 780°C, 790°C or any range between two thereof. value; the holding time of the second stage is 2~6h, including but not limited to any one of 2h, 3h, 4h, 5h, 6h or the range between any two of them; the calcination temperature of the third stage is 600~700℃, including but not limited to any one of 600℃, 620℃, 640℃, 660℃, 680℃, 700℃ or the range between any two of them; the holding time of the third stage is 2~6h, including but not limited to any one of 2h, 3h, 4h, 5h, 6h or the range between any two of them; the heating rate and cooling rate of each stage in the material calcination process are 3~5℃ / min.
[0119] Furthermore, in some embodiments, the high temperature gradient calcination is performed under an inert gas.
[0120] Furthermore, in some embodiments, the inert gas includes nitrogen, argon, etc.
[0121] Furthermore, in some embodiments, after the high temperature gradient calcination is completed, the method further includes: cooling the calcined product and then grinding and sieving it thoroughly.
[0122] In a fourth aspect, an embodiment of the present application provides a positive electrode plate, comprising the lithium iron manganese phosphate positive electrode material provided in the third aspect of the present application.
[0123] The positive electrode plate of the present application includes the above-mentioned lithium iron manganese phosphate positive electrode material, and thus has the advantages of high specific capacity and good rate performance.
[0124] In a fifth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate provided in the fourth aspect of the present application.
[0125] The secondary battery of the present application includes the above-mentioned positive electrode plate, and thus has the advantages of high specific capacity and good rate performance.
[0126] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0127] Preparation method
[0128] 1. Preparation method
[0129] Example 1
[0130] (1) Manganese sulfate, ferrous sulfate and a first chelating agent (citric acid) were dissolved in deionized water to prepare a first mixed solution, wherein the total concentration of iron and manganese metal ions in the first mixed solution was 80 g / L, the molar ratio of manganese to iron was 6:4, and the concentration of citric acid was 4 g / L; a precipitant (ammonium dihydrogen phosphate) and a second chelating agent (ammonia water) were dissolved in deionized water to prepare a second mixed solution, wherein the concentration of ammonium dihydrogen phosphate in the second mixed solution was 3.2 g / L and the concentration of ammonia water was 8 g / L; a precipitant (the molar ratio of phosphoric acid to diammonium hydrogen phosphate was 1:1) was dissolved in water to prepare a precipitant aqueous solution with a concentration of 80 g / L; a third chelating agent (citric acid) and a precipitant (ammonium dihydrogen phosphate) were dissolved in water to prepare a buffer base solution with a pH of 4, wherein the molar ratio of citric acid to diammonium dihydrogen phosphate was 1:3, and the concentration of diammonium dihydrogen phosphate was 6 g / L.
[0131] (2) In order to ensure uniform stirring at the beginning of the reaction, 500 mL of buffer solution is added to the double-layer glass reactor, and a water bath is used to control the temperature during the reaction to be constant at 50°C; a peristaltic pump is used to slowly pump the first mixed solution, the second mixed solution and the precipitant aqueous solution into the reactor at the same time. The volumes of the first mixed solution, the second mixed solution and the precipitant aqueous solution are 500 mL, 1 L and 1 L respectively. The pH value is maintained at 4 during the reaction by adjusting the feeding rate of the second mixed solution; the stirring speed during the dropwise addition of the three solutions is 800 rpm, and nitrogen is continuously introduced for protection. The reaction is carried out for 6 hours. After the reaction is completed, the precursor slurry is aged at 50°C for 1 hour to obtain a precursor slurry; the precursor slurry is washed with deionized water to remove impurities until the conductivity of the washed deionized water is 120 μS / cm. The washed precursor is placed in a 110°C forced air oven and dried for 10 hours to remove moisture to obtain an olivine-type lithium manganese iron phosphate positive electrode material precursor.
[0132] (3) The above-mentioned olivine-type lithium manganese iron phosphate positive electrode material precursor (measured Mn:Fe=58:42) was ground with lithium carbonate and glucose in a mortar according to a molar ratio of 1:1.03:0.09, mixed evenly and loaded into a crucible; the crucible was sent into a tubular furnace for sintering, and high-purity nitrogen gas was required to be introduced into the furnace in advance. When the oxygen content in the furnace was 8ppm, the calcination program was started, and the first calcination temperature was set to 400℃, the sintering time was 5h, the temperature was increased to the second calcination temperature of 760℃, the sintering time was 5h, and then the temperature was reduced to the third calcination temperature of 700℃, the sintering time was 4h, and the heating and cooling rates of the calcination process were both set to 5℃ / min. After the program was completed and cooled, it was sieved (mesh size 300 mesh) to obtain LMFP positive electrode material.
[0133] Example 2
[0134] (1) Manganese nitrate, ferrous sulfate and the first chelating agent (citric acid) are dissolved in deionized water to prepare a first mixed solution, wherein the total concentration of iron and manganese metal ions in the first mixed solution is 60 g / L, the molar ratio of manganese to iron is 7:3, and the concentration of citric acid is 3 g / L; the precipitant (ammonium dihydrogen phosphate) and the second chelating agent (ammonia water) are dissolved in deionized water to prepare a second mixed solution, wherein the concentration of ammonium dihydrogen phosphate in the second mixed solution is 4 g / L and the concentration of ammonia water is 8 g / L; the precipitant (ammonium hydrogen phosphate) is dissolved in water to prepare a precipitant aqueous solution with a concentration of 60 g / L; the third chelating agent (ammonia water) and the precipitant (the mass ratio of phosphoric acid to ammonium dihydrogen phosphate is 1:3) are dissolved in water to prepare a buffer base solution with a pH of 4.5, wherein the molar ratio of ammonia water to ammonium dihydrogen phosphate is 1:1, and the concentration of ammonium dihydrogen phosphate is 8 g / L.
[0135] (2) In order to ensure uniform stirring at the initial stage of the reaction, 500 mL of buffer base liquid is added to the double-layer glass reactor, and a water bath is used to control the temperature during the reaction to be constant at 50°C; a peristaltic pump is used to slowly pump the first mixed solution, the second mixed solution and the precipitant aqueous solution into the reactor at the same time. The volumes of the first mixed solution, the second mixed solution and the precipitant aqueous solution are 1 L, 3 L and 3 L, respectively. The pH value during the reaction is maintained at 4.5 by adjusting the feeding rate of the second mixed solution; the stirring speed during the dropwise addition of the three solutions is 900 rpm, and nitrogen is continuously introduced for protection. The reaction is carried out for 4 hours. After the reaction is completed, the precursor slurry is aged at 50°C for 1 hour to obtain a precursor slurry; the precursor slurry is washed with deionized water to remove impurities until the conductivity of the washed deionized water is 128 μS / cm. The washed precursor is placed in a 110°C forced air oven and dried for 8 hours to remove moisture to obtain an olivine-type lithium manganese iron phosphate positive electrode material precursor.
[0136] (3) The above-mentioned olivine-type lithium manganese iron phosphate positive electrode material precursor (measured Mn:Fe=68:32) was ground with lithium carbonate and glucose in a mortar according to a molar ratio of 1:1.02:0.1, mixed evenly and loaded into a crucible; the crucible was sent into a tubular furnace for sintering, and high-purity nitrogen gas was required to be introduced into the furnace in advance. When the oxygen content in the furnace was 8ppm, the calcination program was started, and the first calcination temperature was set to 400℃, the sintering time was 4h, the temperature was increased to the second calcination temperature of 770℃, the sintering time was 4h, and then the temperature was reduced to the third calcination temperature of 700℃, the sintering time was 5h, and the heating and cooling rates of the calcination process were both set to 4℃ / min. After the program was completed and cooled, it was sieved (mesh size 300 mesh) to obtain LMFP positive electrode material.
[0137] Example 3
[0138] (1) Manganese nitrate, ferrous nitrate and a first complexing agent (lactic acid to sodium citrate in a mass ratio of 1:1) were dissolved in deionized water to prepare a first mixed solution, wherein the total concentration of iron and manganese metal ions in the first mixed solution was 100 g / L, the molar ratio of manganese to iron was 7:3, and the total concentration of lactic acid and sodium citrate was 4.5 g / L; a precipitant (diammonium hydrogen phosphate) and a second complexing agent (ethylenediaminetetraacetic acid) were dissolved in deionized water to prepare a second mixed solution, wherein the molar ratio of diammonium hydrogen phosphate in the second mixed solution was 100 g / L. The concentration is 9g / L, and the concentration of EDTA is 15g / L; the precipitant (the molar ratio of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate is 1:1:1:1) is dissolved in water to prepare a precipitant aqueous solution with a concentration of 90g / L; the third complexing agent (citric acid) and the precipitant (ammonium dihydrogen phosphate) are dissolved in water to prepare a buffer base solution with a pH of 4.3, wherein the molar ratio of citric acid to ammonium dihydrogen phosphate is 1:5, and the concentration of ammonium dihydrogen phosphate is 12g / L.
[0139] (2) In order to ensure uniform stirring at the initial stage of the reaction, 1L of buffer base liquid is added to the double-layer glass reactor, and a water bath is used to control the temperature during the reaction to be constant at 55°C; a peristaltic pump is used to slowly pump the first mixed solution, the second mixed solution and the precipitant aqueous solution into the reactor at the same time. The volumes of the first mixed solution, the second mixed solution and the precipitant aqueous solution are 1L, 2L and 2L respectively. The pH value during the reaction is maintained at 4.3 by adjusting the feeding rate of the second mixed solution; the stirring speed during the dropwise addition of the three solutions is 600rpm, and nitrogen is continuously introduced for protection. The reaction is carried out for 4 hours. After the reaction is completed, the precursor slurry is aged at 55°C for 2 hours to obtain a precursor slurry; the precursor slurry is washed with deionized water to remove impurities until the conductivity of the washed deionized water is 136μS / cm. The washed precursor is placed in a 120°C forced air oven and dried for 6 hours to remove moisture to obtain an olivine-type lithium manganese iron phosphate positive electrode material precursor.
[0140] (3) The above-mentioned olivine-type lithium manganese iron phosphate positive electrode material precursor (measured Mn:Fe=71:29) was ground with lithium carbonate and glucose in a mortar according to a molar ratio of 1:1.02:0.12, mixed evenly and loaded into a crucible; the crucible was sent into a tubular furnace for sintering, and high-purity nitrogen gas was required to be introduced into the furnace in advance. When the oxygen content in the furnace was 6ppm, the calcination program was started, and the first calcination temperature was set to 350℃, the sintering time was 4h, the temperature was increased to the second calcination temperature of 790℃, the sintering time was 3h, and then the temperature was reduced to the third calcination temperature of 650℃, and the sintering time was 6h. The heating and cooling rates of the calcination process were both set to 5℃ / min. After the program was completed and cooled, it was sieved (mesh size 300 mesh) to obtain LMFP positive electrode material.
[0141] Example 4
[0142] Compared with Example 1, the only difference is that the pH of the reaction system is 4.5.
[0143] Example 5
[0144] Compared with Example 2, the only difference is that the buffer base solution of the reaction system is prepared by dissolving a third complexing agent (ascorbic acid) and a precipitant (phosphoric acid to ammonium phosphate in a mass ratio of 1:4) in water, wherein the concentration of ascorbic acid is 2 g / L and the concentration of ammonium phosphate is 8 g / L.
[0145] Example 6
[0146] Compared with Example 3, the only difference is that the second mixed solution is prepared by dissolving a precipitant (diammonium hydrogen phosphate) and a second complexing agent (ammonia water and tris(2-aminoethyl)triacetic acid in a mass ratio of 1:1) into deionized water, and in the second mixed solution, the concentration of diammonium hydrogen phosphate is 4.8 g / L, and the concentration of tris(2-aminoethyl)triacetic acid is 8 g / L.
[0147] Comparative Example 1
[0148] This comparative example provides a method for preparing a positive electrode material precursor, which is the same as Example 1 except that the first mixed solution does not contain the first complexing agent.
[0149] Comparative Example 2
[0150] Compared with Example 1, the only difference is that the pH of the reaction system is 3.5.
[0151] Comparative Example 3
[0152] Compared with Example 1, the only difference is that the pH of the reaction system is 5.
[0153] Comparative Example 4
[0154] Compared with Example 1, the only difference is that the pH of the reaction system is 5.5.
[0155] 2. Test Method
[0156] 1. SEM test
[0157] The precursors prepared in Example 1, Example 4 and Comparative Examples 1 to 4 were subjected to SEM testing using a MERLIN Compact field emission scanning electron microscope (model: Quanta200FEG) produced by Zeiss. The test results are shown in Figures 2 to 7 .
[0158] 2. Performance test of secondary batteries
[0159] The LMFP positive electrode material prepared in Example 1, Example 4 and Comparative Example 1 was mixed with conductive carbon black and PVDF binder in a mass ratio of 90:5:5, and coated on a 12 μm thick aluminum foil. The electrode piece was then placed in an oven at 110° C. and dried for 10 h. The dried electrode piece was punched into a positive electrode disc with a diameter of 15 mm and pressed to a compact density of 1.8 g / cm 3 Roll pressing was used, with a lithium sheet of 16 mm in diameter as the counter electrode, and the electrolyte was 1 M LiPF6 dissolved in EC:EMC:DEC with a volume ratio of 1:1:1. The battery was assembled in an LG2400 / 1000TS glove box produced by Weige Gas Purification Technology (Suzhou) Co., Ltd. to obtain a button-type half-cell, which was then subjected to rate performance testing.
[0160] The battery performance test system (model: CT3002A) of Wuhan Blue Electric Electronic Technology Co., Ltd. was used for testing. The test temperature was 25°C, the voltage range was 2~4.35V, and the rate range was 0.1C~3C. The test results are as follows: Figures 8-10 shown.
[0161] III. Analysis of test results of various embodiments and comparative examples
[0162] Please refer to Figures 2~4 ,pass Figures 2~4 It can be seen that adding the first chelating agent to the first mixed solution can effectively pre-complex the ferrous ions in the solution, thereby achieving the co-precipitation of manganese and iron elements to form an olivine-like precursor. If there is no first chelating agent in the first mixed solution, the ferrous ions therein are easily oxidized into trivalent iron ions, which are difficult to co-precipitate with manganese ions during the co-precipitation reaction, thereby failing to form a precursor with regular and uniform morphology.
[0163] Please refer to Figures 2 to 7 ,pass Figures 2 to 7 It can be seen that when the pH is 4-4.5, olivine LMFP precursors with regular morphology and uniform size can be obtained; but when the pH is higher than 5, the material nucleation rate is too fast and the precursor cannot grow in an orderly and uniform manner, indicating that in this case the precursor synthesis becomes more difficult to control; when the pH is lower than 3.5, the precursor nucleation rate is too slow, the thickness of the growth layer is thin, and the crystal growth rate is slow, resulting in the precursor being fragmented.
[0164] Please refer to Figures 8-10 ,pass Figures 8-10 It can be seen that when the pH of the coprecipitation reaction is 4, the LMFP cathode material prepared from the prepared precursor has a discharge capacity of 145 mAh / g at 0.1C and a discharge capacity of 126 mAh / g at 2C; when the pH of the coprecipitation reaction is 4.5, the LMFP cathode material prepared from the prepared precursor has a discharge capacity of 158 mAh / g at 0.1C and a discharge capacity of 142 mAh / g at 2C. It can be seen that at a suitable pH (e.g., 4.5), the LMFP cathode material prepared from the prepared precursor has a high capacity and good rate performance. When the first complexing agent is not added to the first mixed solution, the LMFP cathode material prepared from the prepared precursor has a poor rate performance, and the discharge capacity at 2C is only 96 mAh / g.
[0165] In summary, the present application prepares the precursor by the co-precipitation method, so that the precursor has a regular and uniform morphology, and the LMFP positive electrode material prepared from the precursor has good electrochemical properties.
[0166] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a lithium manganese iron phosphate positive electrode material precursor, characterized in that: The following steps are involved: Prepare a first mixed solution containing ferrous salt, manganese salt and a first complexing agent, a second mixed solution containing a second complexing agent and a first precipitant, a precipitant aqueous solution containing the second precipitant, and a buffer base solution containing a third precipitant and a third complexing agent; The first mixed solution, the second mixed solution and the precipitant aqueous solution are added to the buffer base solution at the same time to perform a co-precipitation reaction, and a lithium manganese iron phosphate positive electrode material precursor is obtained after aging, washing and drying; wherein, The first complexing agent includes one or more of citric acid, sodium citrate, ascorbic acid, lactic acid and malic acid; The second complexing agent includes one or more of ammonia, ethylenediaminetetraacetic acid, diisopropylaminotetraacetic acid and tris(2-aminoethyl)triacetic acid; The third complexing agent includes one or more of citric acid, sodium citrate, ammonia water, ascorbic acid, lactic acid and malic acid; The first precipitant includes one or more of phosphoric acid, diammonium hydrogen phosphate, diammonium phosphate and ammonium phosphate; The second precipitant comprises one or more of phosphoric acid, diammonium hydrogen phosphate, diammonium phosphate and ammonium phosphate; The third precipitant includes one or more of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate and ammonium phosphate; The pH value is maintained at 4-4.5 during the coprecipitation reaction.
2. The method for preparing the lithium manganese iron phosphate positive electrode material precursor according to claim 1, characterized in that: The ferrous salt includes one or more of ferrous sulfate, ferrous nitrate, ferrous oxalate and ferrous chloride; and / or The manganese salt includes one or more of manganese sulfate, manganese nitrate, manganese acetate, manganese oxalate and manganese chloride.
3. The method for preparing the lithium manganese iron phosphate positive electrode material precursor according to claim 1, characterized in that: In the first mixed solution, the total concentration of manganese ions and ferrous ions is 10-120 g / L, and the concentration of the first complexing agent is 2-10 g / L; and / or In the second mixed solution, the mass ratio of the second complexing agent to the first precipitating agent is 1:(0.2-0.6).
4. The method for preparing the lithium manganese iron phosphate positive electrode material precursor according to claim 1, characterized in that: In the precipitant aqueous solution, the concentration of the second precipitant is 10-120 g / L; and / or In the buffer base solution, the concentration of the third complexing agent is 2-10 g / L, the concentration of the third precipitating agent is 6-80 g / L, and the pH of the buffer base solution is 2-6.
5. The method for preparing the lithium manganese iron phosphate positive electrode material precursor according to claim 1, characterized in that: The volume ratio of the first mixed solution, the second mixed solution, the precipitant aqueous solution and the buffer base solution is (1-3): (2-9): (2-9):
1.
6. The method for preparing the lithium manganese iron phosphate positive electrode material precursor according to claim 1, characterized in that: During the coprecipitation reaction, the temperature of the coprecipitation reaction is 50-60° C.; and / or During the aging process, the aging temperature is 50-60° C., the aging time is 1-6 hours, and the pH of the reaction system is 4-4.
5.
7. A lithium manganese iron phosphate positive electrode material precursor, characterized in that: The lithium iron manganese phosphate positive electrode material precursor is obtained by the preparation method of the lithium iron manganese phosphate positive electrode material precursor according to any one of claims 1 to 6.
8. A lithium iron manganese phosphate positive electrode material, characterized in that: The lithium iron manganese phosphate positive electrode material is prepared by uniformly mixing the lithium iron manganese phosphate positive electrode material precursor described in claim 7 with a lithium source and then using a high-temperature solid phase method.
9. A positive electrode sheet, characterized in that: Including the lithium iron manganese phosphate positive electrode material as described in claim 8.
10. A secondary battery, characterized in that: The secondary battery comprises the positive electrode sheet according to claim 9.
Citation Information
Cited By
Manganese iron phosphate precursor, preparation method therefor, positive electrode material, electrode sheet and battery
EP4691995A1