Preparation method and application of asphalt anti-ultraviolet additive

By reacting rosin acid or monounsaturated fatty acid with maleic anhydride and other compounds in a high UV radiation environment to form a stable chelate, an asphalt anti-UV additive with wide adaptability and simple process can be prepared to solve the current problem. There are technical problems with the narrow application range and complex process of asphalt anti-UV agents, which significantly extends the service life of asphalt pavement.

CN118344255BActive Publication Date: 2024-10-11JIANGSU ZENGGUANG COMPOSITE MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410442735.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-10-11
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

Existing asphalt anti-UV agents have problems such as high technical requirements, complex processes and narrow application range, making it difficult to effectively extend the service life of asphalt pavements in high UV radiation environments.

Method used

It uses rosin acid or monounsaturated fatty acid to react with maleic anhydride, catalyst, polyol, europium trioxide and other compounds at specific temperatures and conditions to form a stable chelate, and prepare a widely adaptable and simple process. Asphalt anti-UV additives.

Benefits of technology

This asphalt anti-UV additive significantly improves the anti-UV performance of asphalt, extends the service life of asphalt pavement, and is suitable for various types of asphalt substrates, including base asphalt, SBS modified asphalt, etc., significantly improving the anti-aging of asphalt ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004789711030000081
    Figure BDA0004789711030000081
  • Figure BDA0004789711030000091
    Figure BDA0004789711030000091
Patent Text Reader

Abstract

This application relates to the field of asphalt UV-resistant preparation technology, and in particular to a method for preparing an asphalt UV-resistant additive and its application, comprising the following preparation steps: S1, adding compound 1, a catalyst, and maleic anhydride to a reactor, heating to 150-170℃, and stirring for 4.5-5.5 h to obtain modified compound 1; S2, adding modified compound 1, a catalyst, and a polyol to the reactor, heating to 175-185℃, and stirring for 3.5-4.5 h to obtain an asphalt UV-resistant intermediate; S3, mixing europium trioxide and an acidic solvent until europium trioxide is completely dissolved, then adding the asphalt UV-resistant intermediate, heating to 105-115℃, and stirring for 0.75-1.2 h to obtain the asphalt UV-resistant additive; wherein compound 1 is rosin acid or a monounsaturated fatty acid, and the asphalt UV-resistant additive prepared by the above method has good UV resistance, the process is simple and the application range is wide, and it can be used for various types of asphalt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of asphalt anti-ultraviolet preparation, and in particular to a preparation method and application of an asphalt anti-ultraviolet additive. Background Art

[0002] Asphalt road is a road paved with composite materials composed of asphalt, fillers and compounding agents. It has high strength and can withstand the weight and pressure of vehicles and pedestrians. It is one of the main projects of roadbed construction in my country. Although asphalt can increase the strength and load-bearing capacity of roads, asphalt will age after a long time, seriously shortening the service life of asphalt roads. The main causes of asphalt aging are heat aging, pressure aging and ultraviolet aging. Especially in Xinjiang and Tibet in my country, where the altitude is high, the sunshine time is long, the ultraviolet radiation intensity is high, and strong ultraviolet rays can easily accelerate the aging of asphalt pavement. After aging, asphalt pavement will crack, deform and deteriorate in sliding properties, which seriously affects road safety.

[0003] In order to extend the service life of asphalt roads, CN110872442A discloses an anti-ultraviolet asphalt aging agent, modified asphalt and its preparation method. An asphalt anti-ultraviolet agent is prepared by using nano titanium dioxide, dopamine hydrochloride and hindered amine light stabilizer. The anti-ultraviolet agent needs to react with a specific modified asphalt to achieve a certain anti-ultraviolet effect. The scope of use is limited and it is not suitable for mass production of asphalt with anti-ultraviolet ability.

[0004] CN113105669A discloses a road asphalt anti-aging agent and a method of using the same. The asphalt anti-aging agent is prepared by compounding a nickel-containing compound, an antioxidant, and a hindered amine light stabilizer, and the anti-aging agent has limited improvement on the anti-ultraviolet aging performance of asphalt.

[0005] CN114437558 B discloses an anti-ultraviolet aging and weathering asphalt and its preparation method. A component: modified epoxy resin, B component: modified matrix asphalt and curing agent are used. The preparation method AB components are too complicated and the cost is high, which is difficult to be industrialized.

[0006] CN101434472A discloses a method for improving the anti-ultraviolet aging performance of modified asphalt. The method includes adding CeO2 nanomaterials and ultraviolet absorber UV-531 with the function of absorbing ultraviolet rays to the asphalt. The ultraviolet absorber used in the method is easy to volatilize at high temperatures, and the CeO2 nanomaterial is easy to produce a segregation effect in the asphalt, affecting its anti-ultraviolet performance.

[0007] It can be seen that the current asphalt anti-ultraviolet agent has the following problems: high technical requirements, complex process, need to be used together with specific modified asphalt to exert anti-ultraviolet performance, and narrow application range. Improvements are needed. Summary of the invention

[0008] In order to solve the current problems of high technical requirements, complex processes and narrow application range of asphalt anti-UV, the present application provides an asphalt anti-UV additive with good anti-UV effect, long duration, simple technical process, easy quantification production and wide range of use.

[0009] A method for preparing an asphalt anti-ultraviolet additive comprises the following preparation steps:

[0010] S1, adding compound 1, a catalyst and maleic anhydride into a reactor, raising the temperature to 150-170° C., stirring and reacting for 4.5-5.5 hours, to obtain a modified compound 1;

[0011] S2, adding the modified compound 1, the catalyst and the polyol into the reactor, raising the temperature to 175-185° C., stirring and reacting for 3.5-4.5 hours, to obtain an asphalt anti-ultraviolet intermediate;

[0012] S3, stirring and mixing europium trioxide and an acidic solvent until europium trioxide is completely dissolved, then adding the asphalt anti-ultraviolet intermediate, heating to 105-115° C., stirring and reacting for 0.75-1.2 hours, and obtaining an asphalt anti-ultraviolet additive;

[0013] The compound 1 is rosin acid or monounsaturated fatty acid.

[0014] By adopting the above technical scheme, the asphalt anti-UV additive is prepared, which has good anti-UV effect, simple process and wide range of use. It can be used for base asphalt, SBS modified asphalt, SBR modified asphalt, PE modified asphalt, polyurethane modified asphalt, rubber powder asphalt, high-viscosity and high-elastic asphalt, construction asphalt and hydraulic asphalt, etc.

[0015] In the present application, in step S1, compound 1 reacts with maleic anhydride so that the cyclic structure of maleic anhydride is connected to compound 1. In step S2, polyol reacts with modified compound 1 so that the ether bond is opened to form a cyan anti-ultraviolet intermediate. In step S3, europium trioxide is dissolved in an acidic solvent to form trivalent europium ions. The trivalent europium ions react with the asphalt anti-ultraviolet intermediate so that the trivalent europium ions and the asphalt anti-ultraviolet intermediate form a complex. The trivalent europium ions have good anti-ultraviolet effects, and the structure of the formed complex is stable, and can maintain good anti-ultraviolet effects for a long time. After the trivalent europium ions form a chelate with the asphalt anti-ultraviolet intermediate, the structure is stable and not easy to lose, and can play a good anti-ultraviolet effect for a long time.

[0016] Preferably, the structural formula of the monounsaturated fatty acid is CH3(CH2)n 1 C=C(CH2)n 2 COOH, n1 is 2-12, n2 is 2-9.

[0017] By adopting the above technical solution, the reaction efficiency of monounsaturated fatty acid and maleic anhydride is improved, and the generation of by-products is reduced.

[0018] Preferably, the molar ratio of the compound 1 to the maleic anhydride is 1:(1-1.2).

[0019] By adopting the above technical solution, the molar ratio of compound 1 and maleic anhydride is optimized, so that compound 1 and maleic anhydride can react fully, the reaction efficiency is improved, and then the production efficiency is improved.

[0020] Preferably, the molar ratio of the europium trioxide to the asphalt anti-ultraviolet intermediate is 1:(2-10).

[0021] By adopting the above technical scheme, the molar ratio of europium trioxide to the asphalt anti-UV intermediate is optimized, so that the trivalent europium ions can fully react with the asphalt anti-UV intermediate to form a structurally stable chelate, which is beneficial to improving the anti-UV effect of the asphalt anti-UV additive and extending the anti-UV time.

[0022] Preferably, the catalyst in step S1 is one of iodine, concentrated sulfuric acid or concentrated phosphoric acid.

[0023] By adopting the above technical solution, compound 1 and maleic anhydride can be fully reacted, the reaction efficiency is improved, and then the production efficiency is improved.

[0024] Preferably, the catalyst in step S2 is concentrated sulfuric acid or concentrated phosphoric acid.

[0025] By adopting the above technical solution, the modified compound 1 and the polyol can fully react, the generation of impurities can be reduced, and the production efficiency can be improved.

[0026] Preferably, the mass fraction of concentrated sulfuric acid is 80-98%, and the mass fraction of concentrated phosphoric acid is 85-95%.

[0027] Preferably, the polyol includes any one of ethylene glycol, glycerol, 1,2-propylene glycol and 1,4-butanediol.

[0028] By adopting the above technical scheme, it is beneficial to form a structurally stable asphalt anti-UV intermediate, which can react quickly and fully with trivalent europium ions to form a structurally stable chelate, which is beneficial to increasing the service life and anti-UV effect of the asphalt anti-UV additive.

[0029] Preferably, in step S1, the molar ratio of the catalyst to the compound 1 is 1:(89-185), and in step S2, the molar ratio of the catalyst to the polyol is 1:(106-157).

[0030] By adopting the above technical solution, the reaction efficiency of step S1 and step S2 is improved and the reaction time is shortened.

[0031] In the second aspect, the present application provides an application of an anti-ultraviolet additive for asphalt, using the following technical solution:

[0032] An application of an asphalt anti-ultraviolet additive, wherein the asphalt anti-ultraviolet additive is mixed with at least one of base asphalt, SBS modified asphalt, SBR modified asphalt, PE modified asphalt, polyurethane modified asphalt, rubber powder asphalt, high-viscosity and high-elastic asphalt, construction asphalt and hydraulic asphalt in any proportion.

[0033] By adopting the above technical solution, the application scope of asphalt anti-UV additives can be further expanded, the adaptability of asphalt anti-UV additives can be improved, and the service life of asphalt can be extended.

[0034] In summary, this application has the following beneficial effects:

[0035] 1. The present application adopts rosin acid or monounsaturated fatty acid, maleic anhydride, catalyst, polyol, europium trioxide and acidic solvent to prepare asphalt anti-ultraviolet additive, which has good ultraviolet radiation effect and can greatly improve the service life of asphalt pavement in areas with strong ultraviolet radiation such as plateaus.

[0036] 2. The asphalt anti-ultraviolet additive in this application has a wide range of adaptability and can enhance the anti-ultraviolet aging ability of various asphalts including: base asphalt, SBS modified asphalt, SBR modified asphalt, high viscosity modified asphalt, etc.

[0037] 3. The production process is simple and convenient, and the method of use is simple. The asphalt anti-ultraviolet additive in this application is dispersed with the corresponding asphalt at a high speed to enhance the asphalt's anti-ultraviolet aging ability. DETAILED DESCRIPTION

[0038] Example

[0039] Example 1

[0040] An asphalt anti-ultraviolet additive is prepared by the following method:

[0041] S1. Add 140 g (0.4629 mol) of rosin acid, 0.3 g (iodine, 0.0024 mol) of catalyst and 50 g (0.5099 mol) of maleic anhydride into the reactor, heat to 150°C, stir and react for 4.5 hours to obtain modified rosin acid; (the molar ratio of rosin acid to maleic anhydride is 1:1.1, and the molar ratio of iodine to rosin acid is 1:193)

[0042] S2. Add 90g (0.2362mol) of modified rosin acid, 1g of catalyst (85% concentrated sulfuric acid, 0.0082mol) and 80g of polyol (propylene glycol, 0.8687mol) into the reactor, heat to 175°C, stir and react for 3.5h to obtain an asphalt anti-ultraviolet intermediate; (the molar ratio of modified rosin acid to propylene glycol is 1:3.7, and the molar ratio of concentrated sulfuric acid to propylene glycol is 1:106)

[0043] S3. Mix 35g (0.1550mol) of europium trioxide and 20g of concentrated hydrochloric acid until the europium trioxide is completely dissolved, then add 147g (0.3419mol) of asphalt anti-ultraviolet intermediate, heat to 105°C, stir and react for 0.75h to obtain asphalt anti-ultraviolet additive. (The molar ratio of europium trioxide to asphalt anti-ultraviolet intermediate is 1:2.2)

[0044] Example 2

[0045] An asphalt anti-ultraviolet additive is prepared by the following method:

[0046] S1. Add 140 g (0.4629 mol) of rosin acid, 0.26 g (80% concentrated sulfuric acid, 0.0021 mol) of catalyst and maleic anhydride (0.5555 mol) into the reactor, heat to 170°C, stir and react for 5.5 h to obtain modified rosin acid; (the molar ratio of rosin acid to maleic anhydride is 1:1.2, and the molar ratio of concentrated sulfuric acid (0.0021 mol) to rosin acid is 1:220)

[0047] S2. Add 90g (0.2362mol) of modified rosin acid, 2.1g (80% concentrated sulfuric acid, 0.017mol) of catalyst and 91g (propylene glycol, 0.9920mol) of polyol to the reactor, heat to 185°C, stir and react for 4.5h to obtain an asphalt anti-ultraviolet intermediate; (the molar ratio of modified rosin acid to propylene glycol is 1:4.2, and the molar ratio of concentrated sulfuric acid to propylene glycol is 1:157)

[0048] S3, stir and mix 7.7g (0.0342mol) of europium trioxide and 4g of concentrated hydrochloric acid until the europium trioxide is completely dissolved, then add 147g (0.3419mol) of asphalt anti-ultraviolet intermediate, heat to 115°C, stir and react for 1.2h to obtain asphalt anti-ultraviolet additive. (The molar ratio of europium trioxide to asphalt anti-ultraviolet intermediate is 1:10).

[0049] Example 3

[0050] An anti-ultraviolet additive for asphalt. The difference between this embodiment and embodiment 1 is that the polyol is 66g of 2-propylene glycol, and the remaining amounts, types and experimental parameters of the experimental raw materials are consistent with those of embodiment 1.

[0051] Example 4

[0052] An anti-ultraviolet additive for asphalt. The difference between this embodiment and embodiment 1 is that the polyol is 54g of ethylene glycol, and the remaining amounts, types and experimental parameters of the experimental raw materials are consistent with those of embodiment 1.

[0053] Example 5

[0054] An asphalt anti-ultraviolet additive is prepared by the following method:

[0055] S1. Add 130.7 g of monounsaturated fatty acid, 0.3 g of catalyst (0.0024 mol of iodine) and 50 g of maleic anhydride into the reactor, heat to 150°C, stir and react for 4.5 hours to obtain modified monounsaturated fatty acid; (the molar ratio of monounsaturated fatty acid to maleic anhydride is 1:1.1, and the molar ratio of iodine to monounsaturated fatty acid is 1:193)

[0056] S2. Add 88.8 g (0.2362 mol) of modified monounsaturated fatty acid (376), 1 g of catalyst (85% concentrated sulfuric acid, 0.0082 mol) and 80 g of polyol (propylene glycol, 0.8687 mol) into the reactor, heat to 175°C, stir and react for 3.5 hours to obtain an asphalt anti-ultraviolet intermediate; (the molar ratio of monounsaturated fatty acid to propylene glycol is 1:3.7, and the molar ratio of concentrated sulfuric acid to propylene glycol is 1:106)

[0057] S3, stir and mix 35g (0.1550mol) of europium trioxide and 20g of concentrated hydrochloric acid until the europium trioxide is completely dissolved, then add 151.8g (0.3419mol) 444 of asphalt anti-ultraviolet intermediate, heat to 105°C, stir and react for 0.75h, and obtain asphalt anti-ultraviolet additive. (The molar ratio of europium trioxide to asphalt anti-ultraviolet intermediate is 1:2.2).

[0058] Monounsaturated fatty acid CH3(CH2) 6 C=C(CH2) 6 COOH.

[0059] Example 6

[0060] An asphalt anti-ultraviolet additive is prepared by the following method:

[0061] S1. Add 130.7 g (0.4629 mol) of monounsaturated fatty acid, 0.26 g (mass fraction 80% concentrated sulfuric acid, 0.0021 mol) of catalyst and maleic anhydride (0.5555 mol) into the reactor, heat to 170°C, stir and react for 5.5 hours to obtain modified monounsaturated fatty acid; (the molar ratio of monounsaturated fatty acid to maleic anhydride is 1:1.2, and the molar ratio of iodine to monounsaturated fatty acid is 1:220)

[0062] S2, add 88.8 (0.2362 mol) of modified monounsaturated fatty acid, 2.1 g of catalyst (80% concentrated sulfuric acid, 0.017 mol) and 91 g of polyol (propylene glycol, 0.9920 mol) into the reactor, heat to 185°C, stir and react for 4.5 hours to obtain asphalt anti-ultraviolet intermediate; (the molar ratio of monounsaturated fatty acid to propylene glycol is 1:4.2, and the molar ratio of concentrated sulfuric acid to propylene glycol is 1:157)

[0063] S3, stir and mix 7.7g (0.0342mol) of europium trioxide and 4g of concentrated salt until the europium trioxide is completely dissolved, then add 151.8g (0.3419mol) of asphalt anti-ultraviolet intermediate, heat to 115°C, stir and react for 1.2h to obtain asphalt anti-ultraviolet additive. (The molar ratio of europium trioxide to asphalt anti-ultraviolet intermediate is 1:2.2)

[0064] Example 7

[0065] An asphalt anti-ultraviolet additive is prepared by the following method:

[0066] S1. Add 124.7 g (0.4629 mol) of monounsaturated fatty acid, 0.26 g (mass fraction 80% concentrated sulfuric acid, 0.0021 mol) of catalyst and maleic anhydride (0.5555 mol) into the reactor, heat to 170°C, stir and react for 5.5 hours to obtain modified monounsaturated fatty acid; (the molar ratio of monounsaturated fatty acid to maleic anhydride is 1:1.2, and the molar ratio of iodine to monounsaturated fatty acid is 1:220)

[0067] S2, add 85.7 (0.2362 mol) of modified monounsaturated fatty acid, 2.1 g of catalyst (80% concentrated sulfuric acid, 0.017 mol) and 91 g of polyol (propylene glycol, 0.9920 mol) into the reactor, heat to 185°C, stir and react for 4.5 hours to obtain asphalt anti-ultraviolet intermediate; (the molar ratio of monounsaturated fatty acid to propylene glycol is 1:4.2, and the molar ratio of concentrated sulfuric acid to propylene glycol is 1:157)

[0068] S3, stir and mix 7.7g (0.0342mol) of europium trioxide and 4g of concentrated salt until the europium trioxide is completely dissolved, then add 147.6g (0.3419mol) of asphalt anti-ultraviolet intermediate, heat to 115°C, stir and react for 1.2h to obtain asphalt anti-ultraviolet additive. (The molar ratio of europium trioxide to asphalt anti-ultraviolet intermediate is 1:2.2)

[0069] Monounsaturated fatty acid CH3(CH2) 5 C=C(CH2) 6 COOH.

[0070] Comparative Example

[0071] Comparative Example 1

[0072] An anti-ultraviolet additive for asphalt. The difference between this comparative example and Example 1 is that isopimaric acid is used instead of rosin acid, and the remaining experimental raw material amounts, types and experimental parameters are consistent with those in Example 1.

[0073] Comparative Example 2

[0074] An anti-ultraviolet additive for asphalt. The difference between this comparative example and Example 5 is that cis-9,12-octadecadienoic acid is used instead of monounsaturated fatty acid, and the remaining experimental raw material amounts, types and experimental parameters are consistent with Example 5.

[0075] Comparative Example 3

[0076] An anti-ultraviolet additive for asphalt. The difference between this comparative example and Example 1 is that cerium dioxide is used instead of europium trioxide, and the remaining experimental raw material amounts, types and experimental parameters are consistent with those in Example 1.

[0077] Comparative Example 4

[0078] An anti-ultraviolet additive for asphalt. The difference between this comparative example and Example 1 is that nicotinic anhydride is used instead of maleic anhydride, and the remaining experimental raw material amounts, types and experimental parameters are consistent with those in Example 1.

[0079] Comparative Example 5

[0080] An anti-ultraviolet additive for asphalt. The difference between this comparative example and Example 1 is that ethanol is used instead of polyol, and the remaining experimental raw material amounts, types and experimental parameters are consistent with those in Example 1.

[0081] Application Examples

[0082] Application Example 1

[0083] A UV-resistant asphalt is prepared by the following method:

[0084] Add 10 g of the asphalt anti-ultraviolet additive in Example 1 into 990 g of No. 70 base asphalt and disperse evenly to obtain anti-ultraviolet asphalt.

[0085] The difference between Application Example 2-11 and Application Example 1 is that the asphalt anti-ultraviolet additive in the anti-ultraviolet asphalt comes from different embodiments and comparative example 1, as shown in Table 1:

[0086] Table 1 Sources of asphalt anti-ultraviolet additives

[0087] Application Examples Source of asphalt anti-ultraviolet additives Application Example 1 Example 1 Application Example 2 Example 2 Application Example 3 Example 3 Application Example 4 Example 4 Application Example 5 Example 5 Application Example 6 Example 6 Application Example 7 Example 7 Application Example 8 Comparative Example 1 Application Example 9 Comparative Example 2 Application Example 10 Comparative Example 3 Application Example 11 Comparative Example 4 Application Example 12 Comparative Example 5

[0088] Application Example 13

[0089] A UV-resistant asphalt is prepared by the following method:

[0090] Add 10 g of the asphalt anti-ultraviolet additive in Example 1 into 990 g of SBS modified asphalt and disperse evenly to obtain anti-ultraviolet asphalt.

[0091] Application Example 14

[0092] A UV-resistant asphalt is prepared by the following method:

[0093] 10 g of the asphalt anti-ultraviolet additive in Example 1 was added to 990 g of SBR modified asphalt and dispersed evenly to obtain anti-ultraviolet asphalt.

[0094] Application Example 15

[0095] A UV-resistant asphalt is prepared by the following method:

[0096] Add 10 g of the asphalt anti-ultraviolet additive in Example 1 to 990 g of PE modified asphalt and disperse evenly to obtain anti-ultraviolet asphalt.

[0097] Application Example 16

[0098] A UV-resistant asphalt is prepared by the following method:

[0099] Add 10 g of the asphalt anti-ultraviolet additive in Example 1 to 990 g of rubber powder asphalt and disperse evenly to obtain anti-ultraviolet asphalt.

[0100] Application Example 17

[0101] A UV-resistant asphalt is prepared by the following method:

[0102] Add 10 g of the asphalt anti-ultraviolet additive in Example 1 to 990 g of polyurethane modified asphalt and disperse evenly to obtain anti-ultraviolet asphalt.

[0103] Application Example 18

[0104] A UV-resistant asphalt is prepared by the following method:

[0105] Add 10 g of the asphalt anti-ultraviolet additive in Example 1 to 990 g of high-viscosity and high-elastic asphalt, and disperse evenly to obtain anti-ultraviolet asphalt.

[0106] Performance testing

[0107] The anti-UV asphalt prepared in accordance with Example 1-18 was tested for its aging resistance.

[0108] Detection method / test method

[0109] UV aging performance test: carried out in a UV oven, the UV intensity is 1500umW / cm, the test temperature is 60°C, and the time is 168h. Among them, the application of comparative example 1 only has No. 70 base asphalt, the application of comparative example 2 only has SBS modified asphalt, the application of comparative example 3 only has SBR modified asphalt, the application of comparative example 4 only has PE modified asphalt, the application of comparative example 5 only has rubber powder asphalt, the application of comparative example 6 only has polyurethane modified asphalt, and the application of comparative example 7 only has high-viscosity and high-elastic asphalt.

[0110] The modified asphalt was tested for penetration ratio, 5°C elongation and softening point difference according to the relevant provisions of "Test Specifications for Asphalt and Asphalt Mixtures for Highway Engineering" (JTJE20-2011). The test data are shown in Table 2:

[0111] Table 2 Experimental data of application examples 1-17 and comparative examples 1-7

[0112]

[0113]

[0114] It can be seen from Application Examples 1-17 and Application Comparative Examples 1-7 in combination with Table 2 that the asphalt anti-UV additive prepared by the present application is used in asphalt, which can effectively improve the anti-UV performance of asphalt, delay asphalt aging, and increase the service life of asphalt roads.

[0115] By comparing Application Example 1 with Application Comparative Example 7, the experimental data of the penetration ratio and 5°C elongation in Application Example 1 are significantly smaller than those in Application Example 1; the softening point difference value of Application Comparative Example 7 is greater than that in Application Example 1. After adding the asphalt anti-ultraviolet additive prepared in this application, the anti-aging performance of asphalt is greatly improved.

[0116] By comparing Application Example 1 with Application Examples 8 and 10-12, the experimental data of needle penetration ratio and 5°C elongation in Application Examples 8 and 10-12 are significantly smaller than those in Application Example 1; the softening point difference value of Application Examples 8 and 10-12 is greater than that of Application Example 1;

[0117] Comparing Application Example 5 with Application Example 9, the experimental data of needle penetration ratio and 5℃ elongation in Application Example 9 are significantly smaller than those in Application Example 5; the softening point difference value of Application Example 9 is greater than that of Application Example 5.

[0118] Description: This application prepares an asphalt anti-ultraviolet additive by using rosin acid or monounsaturated fatty acid, maleic anhydride, a catalyst, a polyol, europium trioxide and an acidic solvent, which can greatly improve the anti-ultraviolet performance of the asphalt anti-ultraviolet additive.

[0119] Compared with Application Example 1 and Application Example 7, Application Example 13 and Application Example 2, Application Example 14 and Application Example 3, Application Example 15 and Application Example 4, Application Example 16 and Application Example 5, Application Example 17 and Application Example 6, and Application Example 17 and Application Example 7, the experimental data of needle penetration ratio and 5°C elongation of Application Example 1 and Application Examples 13-18 are significantly improved, and the softening degree difference data changes little, indicating that the asphalt anti-UV additive in this application can adapt to a variety of asphalts and effectively improve the anti-UV performance of asphalt.

[0120] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing an asphalt anti-ultraviolet additive, characterized in that: The method comprises the following preparation steps: S1, adding compound 1, a catalyst and maleic anhydride into a reactor, raising the temperature to 150-170° C., stirring and reacting for 4.5-5.5 hours, to obtain a modified compound 1; S2, adding the modified compound 1, the catalyst and the polyol into the reactor, raising the temperature to 175-185° C., stirring and reacting for 3.5-4.5 hours, to obtain an asphalt anti-ultraviolet intermediate; S3, stirring and mixing europium trioxide and an acidic solvent until europium trioxide is completely dissolved, then adding the asphalt anti-ultraviolet intermediate, heating to 105-115° C., stirring and reacting for 0.75-1.2 hours, and obtaining an asphalt anti-ultraviolet additive; The compound 1 is rosin acid or monounsaturated fatty acid; The structural formula of the monounsaturated fatty acid is CH3(CH2)6C=C(CH2)6COOH or CH3(CH2)5C=C(CH2)6COOH; The catalyst in step S1 is iodine or concentrated sulfuric acid; The catalyst in step S2 is concentrated sulfuric acid; The polyol includes any one of ethylene glycol, glycerol or 1,2-propylene glycol.

2. The method for preparing an asphalt anti-ultraviolet additive according to claim 1, characterized in that: The molar ratio of the compound 1 to the maleic anhydride is 1:(1-1.2).

3. The method for preparing an asphalt anti-ultraviolet additive according to claim 1, characterized in that: The molar ratio of the modified compound 1 to the polyol is 1:(3.7-4.2).

4. The method for preparing an asphalt anti-ultraviolet additive according to any one of claims 1 or 2, characterized in that: The molar ratio of the europium trioxide to the asphalt anti-ultraviolet intermediate is 1:(2.2-10).

5. The method for preparing an asphalt anti-ultraviolet additive according to claim 1, characterized in that: In step S1, the molar ratio of the catalyst to the compound 1 is 1:(89-185), and in step S2, the molar ratio of the catalyst to the polyol is 1:(106-157).

6. An application of an anti-ultraviolet additive for asphalt, characterized in that: The asphalt anti-UV additive is mixed with at least one of base asphalt, SBS modified asphalt, SBR modified asphalt, PE modified asphalt, polyurethane modified asphalt, rubber powder asphalt, high viscosity and high elastic asphalt, construction asphalt and hydraulic asphalt in any proportion, and the asphalt anti-UV additive is obtained by the preparation method of an asphalt anti-UV additive described in any one of claims 1 to 5.