TPU film with moisture permeability and its processing technology
By using modified sepiolite fiber to cross-link with lignin in the TPU film to form an organic network structure, combined with the inorganic skeleton, the problem of insufficient moisture permeability and tensile strength of the TPU film is solved, and higher moisture permeability and tensile strength are achieved. mechanical properties, expanding the scope of applications.
Patent Information
- Application Number
- CN202410595892.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-14
AI Technical Summary
Existing TPU films have deficiencies in moisture permeability and poor mechanical properties such as tensile strength, which limits their application scope.
Modified sepiolite fiber is used, and lignin is loaded on its surface and cross-linked with thermoplastic polyurethane elastomer, toughening agent, etc. to form an organic network structure, combined with the inorganic skeleton structure, to improve the moisture permeability and tensile strength of the TPU film.
It significantly improves the moisture permeability and tensile strength of the TPU film, expands its application range, and enhances the toughness and hygroscopicity of the film through the uniform dispersion and cross-linked structure of modified sepiolite fibers.
Smart Images

Figure BDA0004838935960000101
Abstract
Description
Technical Field
[0001] The present application relates to the field of TPU films, and more specifically, to a moisture-permeable TPU film and a processing technology thereof. Background Art
[0002] Thermoplastic polyurethane elastomer TPU is a type of polymer made from oligomer polyols, polyisocyanates and chain extenders as the main raw materials. It has excellent comprehensive properties such as high strength, high toughness, wear resistance, oil resistance, and good processing performance. TPU film is a film made from TPU masterbatch through calendering, casting, film blowing or coating. It has the characteristics of high elongation, high strength, high wear resistance and low temperature resistance. It has unique applications in medical, electronic, chemical, construction, national defense and textile.
[0003] TPU film has high waterproof performance, but usually has poor permeability to small molecules such as oxygen and water vapor. In related technologies, the moisture permeability of TPU film is often improved by increasing the hydrophilicity of TPU polymer materials and preparing non-porous hydrophilic films. Non-porous hydrophilic films can prevent large molecular water droplets from passing through due to their non-porous structure. At the same time, due to the presence of more hydrophilic groups in the polymer chain segments, they can interact with water molecules through hydrogen bonds and other intermolecular forces, adsorb water molecules on the high humidity side, and then transfer them to the low humidity side for desorption, thereby achieving a moisture permeable effect.
[0004] However, the mechanical properties of common hydrophilic TPU films, such as tensile strength, are poor and their application range is limited, so there is room for improvement. Summary of the invention
[0005] In order to improve the tensile properties of a moisture permeable TPU film, the present application provides a TPU film having both excellent moisture permeability and tensile properties and a processing technology thereof.
[0006] In the first aspect, the present application provides a TPU film with moisture permeability, which adopts the following technical solution:
[0007] A TPU film with moisture permeability, comprising the following components in parts by weight:
[0008] 100 parts of thermoplastic polyurethane elastomer,
[0009] Modified sepiolite fiber 10-20 parts,
[0010] 4-10 parts of toughening agent,
[0011] 1-4 parts of antioxidants,
[0012] 8-12 parts of anti-adhesive;
[0013] The modified sepiolite fiber is lignin-modified sepiolite fiber.
[0014] By adopting the above technical solution, the modified sepiolite fiber has abundant water channels and pore structures, and has abundant hydrophilic groups on the surface, which can improve the moisture permeability of the TPU film. After the TPU film adsorbs water molecules on the high humidity side with the help of the hydrophilic groups, the water molecules can be transferred from the water channel structure of the modified sepiolite fiber to the low humidity side, thereby promoting the improvement of the moisture permeability effect and efficiency of the TPU film.
[0015] The modified sepiolite fiber has good wear resistance, corrosion resistance, elasticity, etc. The modified sepiolite fiber can form a network-like inorganic skeleton structure when dispersed in the TPU system, promote the improvement of the mechanical properties of the TPU film, and enhance the tensile strength of the TPU film; the lignin loaded on the surface of the modified sepiolite fiber can cross-link with thermoplastic polyurethane elastomers, toughening agents, etc. to form an organic network structure, improve the uniformity of the dispersion of the modified sepiolite fiber in the TPU system, and connect the organic system with the inorganic sepiolite fiber skeleton system, further promote the improvement of the tensile strength of the TPU film, and at the same time, can make the sepiolite stably dispersed in the TPU system, further improve the hygroscopicity, which is beneficial to enhance the use effect of the TPU film and expand the application range.
[0016] Preferably, the preparation method of the modified sepiolite fiber comprises:
[0017] Add lignin and high molecular surfactant into the solvent, mix well, and perform ultrasonic treatment at 30-50° C. for 5-20 minutes to obtain a modified solution;
[0018] The sepiolite fiber is immersed in the modification solution, mixed evenly, the pH value is adjusted to 4.5-6, ultrasonic treatment is performed at 60-90° C. for 60-120 minutes, suction filtration is performed, and drying is performed to obtain lignin-modified sepiolite fiber.
[0019] Preferably, in the modified solution, the mass fraction of lignin is 5-15%, the mass fraction of the high molecular surfactant is 10-25%; and the mass of the sepiolite fiber is 15-30% of the modified solution.
[0020] By adopting the above technical scheme, the lignin molecule has a phenylpropane network skeleton structure, and the molecular side chain contains rich active hydrophilic groups. The lignin molecule interacts with the polymer surfactant, and the hydrophobic segment of the polymer surfactant wraps the phenylpropane skeleton of the lignin molecule. The hydrophilic end and the active group of the lignin molecule form hydrogen bonds and other interaction forces to form a lignin coating; the lignin coating then interacts with the sepiolite fiber, and the hydroxyl groups of the polymer surfactant and the active groups of lignin react with the active silicon hydroxyl groups on the surface of the sepiolite fiber and are grafted onto the sepiolite fiber to obtain lignin-modified sepiolite fiber; the hydrophobic skeleton of lignin is wrapped by a more flexible polymer surfactant chain segment, which is beneficial to the improvement of tensile properties. The rich active groups of lignin can improve the water absorption of the sepiolite fiber, and can interact with organic molecules such as TPU and toughening agent in the TPU film to form a cross-linked structure, thereby improving the compatibility of the sepiolite fiber with the organic system, promoting the uniform dispersion of the sepiolite fiber, and being beneficial to improving the moisture permeability and tensile strength of the TPU film.
[0021] Preferably, the polymer surfactant is a carboxymethyl chitosan derivative, and the preparation method comprises:
[0022] Dissolve carboxymethyl chitosan in water, adjust the pH value to 10-11, add dodecyl glycidyl ether, mix well, react at 60-80°C for 6-8h, adjust the pH value to 4-5, precipitate with acetone, wash the product, filter, and vacuum dry to obtain a carboxymethyl chitosan derivative.
[0023] Preferably, the usage ratio of the carboxymethyl chitosan to dodecyl glycidyl ether is 1:(0.8-1.2) g / mL.
[0024] By adopting the above technical scheme, the hydrophilicity of carboxymethyl chitosan is good, carboxymethyl chitosan undergoes a condensation reaction with dodecyl glycidyl ether, and a hydrophobic side chain is introduced into the generated carboxymethyl chitosan derivative. The hydrophobic segment of the carboxymethyl chitosan derivative wraps the phenylpropane skeleton of lignin, and the hydrophilic end has a high reaction activity with the active silanol group on the surface of the sepiolite fiber, which is beneficial to improving the loading efficiency and effect of lignin on the surface of the sepiolite fiber.
[0025] Preferably, the lignin is hydroxymethylated lignin.
[0026] Preferably, the preparation method of the hydroxymethylated lignin comprises:
[0027] The alkali lignin is dissolved in a sodium hydroxide solution, dispersed evenly, the pH value is adjusted to 10.5-12, formaldehyde solution is added thereto, mixed evenly, reacted at 75-90°C for 90-150 minutes, the pH value of the reaction solution is adjusted to 3-4, kept warm at 55-65°C for 60 minutes, filtered, washed with water until neutral, and vacuum dried to obtain hydroxymethylated lignin.
[0028] Preferably, the mass concentration of the formaldehyde solution is 37%; the mass ratio of the alkali lignin to the formaldehyde solution is 1:(0.25-0.75).
[0029] By adopting the above technical scheme, the alkali lignin molecular chain contains multiple groups such as oxygen, phenolic hydroxyl, aldehyde and carboxyl groups, but the hydroxyl content is limited. By reacting alkali lignin with formaldehyde to increase the hydroxyl content on the lignin molecular chain, it is beneficial to improve the reactivity and hydrophilicity of the lignin molecules.
[0030] Preferably, the sepiolite fiber needs to be activated before the modification operation, and the activation treatment step includes: calcining the sepiolite fiber at 200-300°C for 10-20 minutes, placing the calcined sepiolite fiber in a sodium hydroxide solution, ultrasonically treating it for 20-40 minutes, filtering, washing, and drying to obtain activated sepiolite fiber.
[0031] By adopting the above technical scheme, high-temperature activation can remove zeolite water in the sepiolite fiber, increase the pore size of the sepiolite fiber, and increase the strength and number of surface activation centers; then treated with sodium hydroxide solution to reduce soluble impurities in the sepiolite fiber, and form a large number of hydroxyl groups on the surface of the sepiolite fiber, thereby improving the reaction activity of the sepiolite fiber.
[0032] Preferably, the toughening agent is hydroxyethyl acrylate.
[0033] By adopting the above technical solution, hydroxyethyl acrylate can form hydrogen bonds with TPU and lignin molecules loaded on modified sepiolite fibers, participate in the hydrogen bond cross-linking network, increase short flexible chains, and improve the toughness and tensile strength of the TPU film.
[0034] Preferably, the antioxidant comprises a hindered phenol antioxidant and a phosphite antioxidant in a mass ratio of 1:(1-3).
[0035] By adopting the above technical solution, the oxygen aging rate of the TPU film is slowed down.
[0036] In a second aspect, the present application provides a processing technology for a moisture-permeable TPU film, which adopts the following technical solution:
[0037] A processing technology for a moisture-permeable TPU film comprises the following steps:
[0038] Thermoplastic polyurethane elastomer, modified sepiolite fiber, toughening agent, antioxidant and anti-adhesive agent are mixed according to a proportion to form a mixture;
[0039] The mixed material is extruded, cooled, and pelletized to obtain premixed particles;
[0040] The premixed particles are formed by extrusion casting to obtain a TPU film with moisture permeability.
[0041] Preferably, the screw speed of the tape-casting step of the premixed particles is 100-300 r / min, the extrusion temperature is 80-200° C., the die temperature is 100-200° C., and the roller speed is 300-500 m / min.
[0042] By adopting the above technical solution, a TPU film with good moisture permeability, better toughness and tensile strength can be produced, which helps to expand the application scope of the TPU film and enhance the use effect.
[0043] In summary, this application has the following beneficial effects:
[0044] 1. In the present application, the modified sepiolite fiber is dispersed in the TPU system to form a network-like inorganic skeleton structure, which promotes the improvement of the mechanical properties of the TPU film and enhances the tensile strength of the TPU film; the lignin loaded on the surface of the modified sepiolite fiber can cross-link with the thermoplastic polyurethane elastomer, toughening agent, etc. to form an organic network structure, improve the uniformity of the dispersion of the modified sepiolite fiber in the TPU system, and connect the organic system with the inorganic sepiolite fiber skeleton system, further promote the improvement of the tensile strength of the TPU film, which is conducive to enhancing the use effect of the TPU film and expanding the scope of application;
[0045] 2. In this application, hydroxymethylated lignin is preferably used to increase the hydroxyl content on the lignin molecular chain, which is beneficial to improving the reactivity and hydrophilicity of the lignin molecules, promoting the improvement of the water absorption of the TPU film, further improving the moisture permeability of the TPU film, and promoting the hydrogen bond crosslinking between the hydroxymethylated lignin and the TPU and toughening agent small molecules, thereby improving the toughness of the TPU film.
[0046] 3. In the present application, it is preferred to activate the sepiolite fiber before the modification operation, which expands the pores of the water channels and holes of the sepiolite fiber and improves the surface activity of the sepiolite fiber, which helps to promote the loading of lignin by the sepiolite fiber and further improve the moisture permeability and tensile strength of the TPU film. DETAILED DESCRIPTION
[0047] To further help understand the technical solution of the present invention, the technical solution of the present invention is described in more detail below by providing several specific implementation examples. All of these described embodiments are only partial embodiments of the present invention, not all;
[0048] The following specific embodiments may be combined with each other, and the same or similar concepts or processes may not be repeated in some embodiments; and the reaction devices, monomer compounds, organic solvents, etc. involved in the following embodiments are all commercially available.
[0049] The following specific embodiments may be combined with each other, and the same or similar concepts or processes therein may not be described in detail in some embodiments.
[0050] The following examples are further explanations of the present invention, but the present invention is not limited thereto. Unless otherwise specified in the examples, the percentages are all by mass.
[0051] Preparation Example
[0052] Preparation Example 1
[0053] This preparation example provides a modified sepiolite fiber, and the preparation method is as follows:
[0054] 1.2 kg of wheat straw alkali lignin and 1.8 kg of high molecular surfactant were added into 7 kg of water, stirred and mixed evenly, and ultrasonically treated at 45°C for 20 min to obtain a modified solution;
[0055] 2 kg of sepiolite fiber was immersed in the above modified solution, stirred and dispersed evenly, 0.1 mol / L hydrochloric acid solution was added dropwise to adjust the pH value to 5, ultrasonically treated at 65° C. for 2 h, filtered, and vacuum dried at 70° C. to obtain lignin modified sepiolite fiber.
[0056] In this preparation example, the polymer surfactant is glycerol polyoxyethylene ether G-18, model number is Kepler kpl-30432.
[0057] Preparation Example 2
[0058] The difference between this preparation example and the preparation example is that the preparation method of the modified sepiolite fiber is as follows:
[0059] 0.5 kg of wheat straw alkali lignin and 1 kg of glycerol polyoxyethylene ether were added into 8.5 kg of water, stirred and mixed evenly, and ultrasonically treated at 45°C for 20 min to obtain a modified solution;
[0060] 1.5 kg of sepiolite fiber was immersed in the above modification solution, stirred and dispersed evenly, the pH value was adjusted to 5, ultrasonic treatment was performed at 65° C. for 2 h, suction filtered, and vacuum dried at 70° C. to obtain lignin modified sepiolite fiber.
[0061] Preparation Example 3
[0062] The difference between this preparation example and the preparation example is that the preparation method of the modified sepiolite fiber is as follows:
[0063] 1.5 kg of wheat straw alkali lignin and 2.5 kg of glycerol polyoxyethylene ether were added into 8.5 kg of water, stirred and mixed evenly, and ultrasonically treated at 45°C for 20 min to obtain a modified solution;
[0064] 3 kg of sepiolite fiber was immersed in the above modified solution, stirred and dispersed evenly, the pH value was adjusted to 5, ultrasonic treatment was performed at 65° C. for 2 h, suction filtered, and vacuum dried at 70° C. to obtain lignin modified sepiolite fiber.
[0065] Preparation Example 4
[0066] The only difference between this preparation example and preparation example 1 is that the polymer surfactant is a carboxymethyl chitosan derivative. The preparation method of the carboxymethyl chitosan derivative is as follows:
[0067] 2 kg of carboxymethyl chitosan was dissolved in 7 L of water, 0.2 mol / L of sodium hydroxide solution was added dropwise to adjust the pH value to 10.5, 2 L of dodecyl glycidyl ether was added thereto, the mixture was stirred and mixed, and the mixture was reacted at 75 ° C for 6 h, 10% acetic acid solution was added dropwise to adjust the pH value to 4.5, 5 L of acetone was added and allowed to stand for 12 h, and the reactant was completely precipitated, filtered, washed three times with acetone, filtered, and vacuum dried at 50 ° C to obtain a carboxymethyl chitosan derivative.
[0068] The preparation method of modified sepiolite fiber is as follows:
[0069] 1.2 kg of wheat straw alkali lignin and 1.8 kg of carboxymethyl chitosan derivative were added into 7 kg of water, stirred and mixed evenly, and ultrasonically treated at 45°C for 20 min to obtain a modified solution;
[0070] 2 kg of sepiolite fiber was immersed in the above modified solution, stirred and dispersed evenly, 0.1 mol / L hydrochloric acid solution was added dropwise to adjust the pH value to 5, ultrasonically treated at 65° C. for 2 h, filtered, and vacuum dried at 70° C. to obtain lignin modified sepiolite fiber.
[0071] Preparation Example 5
[0072] The only difference between this preparation example and preparation example 4 is that the lignin is hydroxymethylated lignin, and the preparation method is as follows:
[0073] 2 kg of wheat straw alkali lignin was dissolved in 8 L of 0.2 mol / L sodium hydroxide solution and dispersed evenly. The pH value was adjusted to 11 with 20 wt % sodium hydroxide solution. 1 kg of 37 % formaldehyde solution was added thereto. The mixture was mixed and reacted at 80° C. for 120 min. The pH value of the reaction solution was adjusted to 3.5 with 10 wt % hydrochloric acid solution. The mixture was kept warm at 60° C. for 60 min. The mixture was hot filtered, washed with water until neutral, and vacuum dried at 45° C. to obtain hydroxymethylated lignin.
[0074] The preparation method of modified sepiolite fiber is as follows:
[0075] 1.2 kg of hydroxymethylated lignin and 1.8 kg of carboxymethyl chitosan derivative were added into 7 kg of water, stirred and mixed evenly, and ultrasonically treated at 45°C for 20 min to obtain a modified solution;
[0076] 2 kg of sepiolite fiber was immersed in the above modified solution, stirred and dispersed evenly, 0.1 mol / L hydrochloric acid solution was added dropwise to adjust the pH value to 5, ultrasonically treated at 65° C. for 2 h, filtered, and vacuum dried at 70° C. to obtain lignin modified sepiolite fiber.
[0077] Preparation Example 6
[0078] The only difference between this preparation example and preparation example 5 is that the preparation method of hydroxymethylated lignin is as follows:
[0079] 2 kg of wheat straw alkali lignin was dissolved in 8 L of 0.2 mol / L sodium hydroxide solution and dispersed evenly. The pH value was adjusted to 11 with 20 wt% sodium hydroxide solution. 0.5 kg of 37% formaldehyde solution was added thereto. The mixture was mixed and reacted at 80° C. for 120 min. The pH value of the reaction solution was adjusted to 3.5 with 10 wt% hydrochloric acid solution. The mixture was kept warm at 60° C. for 60 min. The mixture was hot filtered, washed with water until neutral, and vacuum dried at 45° C. to obtain hydroxymethylated lignin.
[0080] Preparation Example 7
[0081] The only difference between this preparation example and preparation example 5 is that the preparation method of hydroxymethylated lignin is as follows:
[0082] 2 kg of wheat straw alkali lignin was dissolved in 8 L of 0.2 mol / L sodium hydroxide solution and dispersed evenly. The pH value was adjusted to 11 with 20 wt % sodium hydroxide solution. 1.5 kg of 37 % formaldehyde solution was added thereto. The mixture was mixed and reacted at 80° C. for 120 min. The pH value of the reaction solution was adjusted to 3.5 with 10 wt % hydrochloric acid solution. The mixture was kept warm at 60° C. for 60 min. The mixture was hot filtered, washed with water until neutral, and vacuum dried at 45° C. to obtain hydroxymethylated lignin.
[0083] Preparation Example 8
[0084] The only difference between this preparation example and preparation example 5 is that the sepiolite fiber is activated before the modification operation. The activation operation is as follows:
[0085] 2.5 kg of sepiolite fiber was calcined at 260° C. for 15 min, and then the calcined sepiolite fiber was placed in 5 L of 0.2 mol / L sodium hydroxide solution, ultrasonically treated for 30 min, filtered, washed with water until neutral, and vacuum dried at 60° C. to obtain activated sepiolite fiber.
[0086] The preparation method of modified sepiolite fiber is as follows:
[0087] 1.2 kg of hydroxymethylated lignin and 1.8 kg of carboxymethyl chitosan derivative were added into 7 kg of water, stirred and mixed evenly, and ultrasonically treated at 45°C for 20 min to obtain a modified solution;
[0088] 2 kg of activated sepiolite fiber was immersed in the above-mentioned modified solution, stirred and dispersed evenly, 0.1 mol / L hydrochloric acid solution was added dropwise to adjust the pH value to 5, ultrasonically treated at 65° C. for 2 h, filtered, and vacuum dried at 70° C. to obtain lignin-modified sepiolite fiber.
[0089] Example
[0090] Example 1
[0091] This embodiment discloses a TPU film with moisture permeability, including the following components by weight: 10 kg of thermoplastic polyurethane elastomer, 1.5 kg of modified sepiolite fiber, 0.6 kg of toughening agent, 0.25 kg of antioxidant, and 1 kg of anti-sticking agent.
[0092] In this embodiment, the thermoplastic polyurethane elastomer includes 2.5 kg of Huafeng HF-90MVT-7 and 7.5 kg of Reid 7263; the modified sepiolite fiber is prepared by the method in Preparation Example 1; the toughening agent is hydroxyethyl acrylate; the antioxidant is obtained by mixing antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2; and the anti-sticking agent is purchased from Junyue New Materials Technology Co., Ltd.
[0093] The processing technology of TPU film with moisture permeability is as follows:
[0094] The thermoplastic polyurethane elastomer, modified sepiolite fiber, toughening agent, antioxidant and anti-sticking agent of the above mass are put into a mixer, and stirred and mixed at 85° C. to form a mixture;
[0095] The mixed material is put into a twin-screw extruder for extrusion, and pelletized after cooling to obtain premixed pellets;
[0096] The premixed particles were put into a casting machine for extrusion casting, wherein the screw speed was 100 r / min, the extrusion temperature was 200° C., the die temperature was 100° C., and the roller speed was 300 m / min to obtain a TPU film with moisture permeability.
[0097] Example 2
[0098] The only difference between this embodiment and embodiment 1 is that the moisture-permeable TPU film includes the following components in weight: 10 kg of thermoplastic polyurethane elastomer, 1 kg of modified sepiolite fiber, 0.4 kg of toughening agent, 0.4 kg of antioxidant, and 1.2 kg of anti-sticking agent.
[0099] Example 3
[0100] The only difference between this embodiment and embodiment 1 is that the moisture-permeable TPU film includes the following components by mass: 10 kg of thermoplastic polyurethane elastomer, 2 kg of modified sepiolite fiber, 1 kg of toughening agent, 0.1 kg of antioxidant, and 0.8 kg of anti-sticking agent.
[0101] Example 4
[0102] The only difference between this embodiment and embodiment 1 is that the modified sepiolite fiber is prepared by the method of preparation example 2.
[0103] Example 5
[0104] The only difference between this embodiment and embodiment 1 is that the modified sepiolite fiber is prepared by the method of preparation example 3.
[0105] Example 6
[0106] The only difference between this embodiment and embodiment 1 is that the modified sepiolite fiber is prepared by the method of preparation example 4.
[0107] Example 7
[0108] The only difference between this embodiment and embodiment 1 is that the modified sepiolite fiber is prepared by the method of preparation example 5.
[0109] Example 8
[0110] The only difference between this embodiment and embodiment 1 is that the modified sepiolite fiber is prepared by the method of preparation example 6.
[0111] Example 9
[0112] The only difference between this embodiment and embodiment 1 is that the modified sepiolite fiber is prepared by the method of embodiment 7.
[0113] Example 10
[0114] The only difference between this embodiment and embodiment 1 is that the modified sepiolite fiber is prepared by the method of embodiment 8.
[0115] Comparative Example
[0116] Comparative Example 1
[0117] The only difference between this comparative example and Example 1 is that the TPU film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 0.6 kg of toughening agent, 0.25 kg of antioxidant, and 1 kg of anti-sticking agent.
[0118] The processing technology of TPU film is as follows:
[0119] Put the thermoplastic polyurethane elastomer, toughening agent, antioxidant and anti-sticking agent of the above mass into a mixer, stir and mix at 85°C to form a mixture;
[0120] The mixed material is put into a twin-screw extruder for extrusion, and pelletized after cooling to obtain premixed pellets;
[0121] The premixed particles are put into a casting machine for extrusion casting to obtain a TPU film with moisture permeability.
[0122] Comparative Example 2
[0123] The only difference between this comparative example and Example 1 is that the TPU film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 1.5 kg of sepiolite fiber, 0.6 kg of toughening agent, 0.25 kg of antioxidant, and 1 kg of anti-sticking agent.
[0124] The processing technology of TPU film is as follows:
[0125] The thermoplastic polyurethane elastomer, sepiolite fiber, toughening agent, antioxidant and anti-sticking agent of the above mass are put into a mixer, and stirred and mixed at 85° C. to form a mixture;
[0126] The mixed material is put into a twin-screw extruder for extrusion, and pelletized after cooling to obtain premixed pellets;
[0127] The premixed particles are put into a casting machine for extrusion casting to obtain a TPU film with moisture permeability.
[0128] Comparative Example 3
[0129] The only difference between this comparative example and Example 1 is that the TPU film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 1.5 kg of lignin, 0.6 kg of toughening agent, 0.25 kg of antioxidant, and 1 kg of anti-sticking agent.
[0130] The processing technology of TPU film is as follows:
[0131] The thermoplastic polyurethane elastomer, lignin, toughening agent, antioxidant and anti-sticking agent of the above mass are put into a mixer, and stirred and mixed at 85° C. to form a mixture;
[0132] The mixed material is put into a twin-screw extruder for extrusion, and pelletized after cooling to obtain premixed pellets;
[0133] The premixed particles are put into a casting machine for extrusion casting to obtain a TPU film with moisture permeability.
[0134] Comparative Example 4
[0135] The only difference between this comparative example and Example 1 is that the TPU film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 1 kg of sepiolite fiber, 0.5 kg of lignin, 0.6 kg of toughening agent, 0.25 kg of antioxidant, and 1 kg of anti-sticking agent.
[0136] The processing technology of TPU film is as follows:
[0137] The thermoplastic polyurethane elastomer, sepiolite fiber, lignin, toughening agent, antioxidant and anti-sticking agent of the above mass are put into a mixer, and stirred and mixed at 85° C. to form a mixture;
[0138] The mixed material is put into a twin-screw extruder for extrusion, and pelletized after cooling to obtain premixed pellets;
[0139] The premixed particles are put into a casting machine for extrusion casting to obtain a TPU film with moisture permeability.
[0140] Performance testing
[0141] The TPU films prepared in each embodiment and each comparative example were cut into test samples of the same size and subjected to the following tests: Test 1: Moisture permeability test: Referring to the international standard ASTM-E96BW water vapor inverted cup method, a fabric moisture permeability meter was used to test the MVTR (moisture vapor transmission rate) of the TPU film samples in each embodiment and each comparative example;
[0142] Test 2: Tensile strength test: The transverse tensile strength and elongation at break of the TPU film samples of each embodiment and each comparative example were tested with reference to the international standard ASTM-D882-18. The sample film thickness was 0.016 mm, the sample width was 25 mm, the chuck distance was 50 mm, and the test speed was 500 mm / min.
[0143] The test results are summarized in Table 1.
[0144] Table 1
[0145]
[0146]
[0147] Combining Examples 1-5 and Table 1, it can be seen that the MVTR value of the TPU film prepared according to the formula and method disclosed in this application is greater than 6800 g / (m 2 × 24h), the elongation at break is greater than 500%, and the tensile strength is high, indicating that the moisture-permeable TPU film of the present application has better moisture-permeability, good toughness, and excellent tensile properties, which helps to expand the application scenarios of the TPU film.
[0148] It can be seen from Example 1 and Comparative Examples 1-4 and Table 1 that adding lignin-modified sepiolite fibers to the TPU film system can promote the improvement of the moisture permeability and tensile strength of the TPU film; lignin is grafted to the sepiolite fibers through a polymer surfactant, thereby improving the compatibility of the sepiolite fibers with the TPU system, promoting the uniform dispersion of the sepiolite fibers, and connecting the organic cross-linked network system with the inorganic fiber network structure, thereby promoting the improvement of the toughness and tensile strength of the TPU film; and lignin enriches the hydrophilic groups in the TPU film system, thereby enhancing the hydrophilicity of the TPU film, and the TPU film can adsorb water molecules on the high humidity side, and quickly transfer them to the low humidity side for desorption through the water channel structure of the sepiolite fibers, thereby promoting the improvement of the moisture permeability of the TPU film.
[0149] It can be seen from Example 1 and Example 6 and Table 1 that the use of hydroxymethyl chitosan derivatives as polymer surfactants helps to further improve the moisture permeability and toughness of the TPU film. This may be because the hydroxymethyl chitosan derivatives have strong hydrophilicity and reaction activity, which is beneficial to promoting the loading of lignin by sepiolite fiber.
[0150] It can be seen from Example 1, Examples 7-9 and Table 1 that the selection of hydroxymethylated lignin can further enrich the hydrophilic groups of the TPU film, promote the improvement of the hydrophilicity of the TPU film, and thus help to further improve the moisture permeability of the TPU film, and can promote the hydrogen bond crosslinking between the hydroxymethylated lignin and the TPU and toughening agent small molecules, thereby improving the toughness of the TPU film.
[0151] It can be seen from Example 1, Example 10 and Table 1 that activation treatment of sepiolite fiber is beneficial to promoting the improvement of moisture permeability and tensile strength of TPU film. This may be because the activation treatment expands the pores of water channels and holes of sepiolite fiber and improves the surface activity of sepiolite fiber, which helps to promote the loading of sepiolite fiber on lignin.
[0152] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A TPU film with moisture permeability, characterized in that: The composition comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer, Modified sepiolite fiber 10-20 parts, 4-10 parts of toughening agent, 1-4 parts of antioxidants, 8-12 parts of anti-adhesive; The modified sepiolite fiber is lignin-modified sepiolite fiber; The preparation method of the modified sepiolite fiber comprises: Add lignin and high molecular surfactant into the solvent, mix well, and perform ultrasonic treatment at 30-50° C. for 5-20 minutes to obtain a modified solution; The sepiolite fiber is immersed in the modified solution, mixed evenly, the pH value is adjusted to 4.5-6, ultrasonically treated at 60-90° C. for 60-120 min, filtered, and dried to obtain lignin-modified sepiolite fiber; In the modified solution, the mass fraction of lignin is 5-15%, the mass fraction of the high molecular surfactant is 10-25%; the mass of the sepiolite fiber is 15-30% of the modified solution; The toughening agent is hydroxyethyl acrylate.
2. The moisture-permeable TPU film according to claim 1, characterized in that: The polymer surfactant is a carboxymethyl chitosan derivative, and the preparation method of the carboxymethyl chitosan derivative comprises: Dissolve carboxymethyl chitosan in water, adjust the pH value to 10-11, add dodecyl glycidyl ether, mix well, react at 60-80°C for 6-8h, adjust the pH value to 4-5, precipitate with acetone, wash the product, filter, and vacuum dry to obtain a carboxymethyl chitosan derivative.
3. The moisture-permeable TPU film according to claim 1, characterized in that: The lignin is hydroxymethylated lignin.
4. The moisture-permeable TPU film according to claim 1, characterized in that: The sepiolite fiber needs to be activated before the modification operation, and the activation treatment step includes: The sepiolite fiber is calcined at 200-300° C. for 10-20 minutes, and then the calcined sepiolite fiber is placed in a sodium hydroxide solution, ultrasonically treated for 20-40 minutes, filtered, washed, and dried to obtain activated sepiolite fiber.
5. The moisture-permeable TPU film according to claim 1, characterized in that: The antioxidant comprises a hindered phenol antioxidant and a phosphite antioxidant in a mass ratio of 1:(1-3).
6. A process for processing a moisture-permeable TPU film according to any one of claims 1 to 5, characterized in that: The following steps are involved: Thermoplastic polyurethane elastomer, modified sepiolite fiber, toughening agent, antioxidant and anti-adhesive agent are mixed according to a proportion to form a mixture; Extruding, cooling and pelletizing the mixed material to obtain premixed particles; The premixed particles are formed by extrusion casting to obtain a TPU film with moisture permeability.
7. The process for processing a moisture-permeable TPU film according to claim 6, characterized in that: The screw speed of the tape-casting step of the premixed particles is 100-300 r / min, the extrusion temperature is 80-200° C., the die temperature is 100-200° C., and the roller speed is 300-500 m / min.
Citation Information
Patent Citations
Sepiolite / polyurethane nanocomposite material and preparation method thereof
CN102796238A
Preparation method of breathable and moisture-absorbent PU leather
CN107794777A