A UHPC based on microfibrillated cellulose and its preparation method and application

By adding microfibrillated cellulose to ultra-high performance concrete to increase the dissociation energy and matrix strength of hydration products, combined with the bridging effect of steel fibers, the problem of improving the penetration resistance of ultra-high performance concrete has been solved, and significant improvements have been achieved. The mechanical properties and high-speed impact resistance have been improved, expanding its application scope.

CN118359404BActive Publication Date: 2024-10-25SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410376428.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-25
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

After increasing the compressive strength of existing ultra-high performance concrete, the penetration resistance cannot be further improved, and the matrix is ​​relatively weak, and there is a lack of effective technical means to improve its penetration resistance.

Method used

By adding microfibrillated cellulose to ultra-high performance concrete, the dissociation energy of hydration products is increased, thereby improving the matrix strength. Through the synergistic bridging effect of microcellulose and steel fibers, the occurrence and expansion of cracks are inhibited, and the resistance to high-speed impact is improved. performance.

Benefits of technology

It significantly improves the compressive strength, peak strain and first crack load of ultra-high performance concrete, reduces the penetration depth and pit diameter, and has excellent high-speed impact and explosion resistance, expanding its application scope in protection projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118359404B_ABST
    Figure CN118359404B_ABST
Patent Text Reader

Abstract

The present invention discloses a UHPC based on microfibrillated cellulose and a preparation method and application, belonging to the technical field of new building materials. UHPC is prepared from raw materials including the following components by mass: 1377-1577 parts of cement, 35-43 parts of steel fiber, 120-180 parts of silica fume, 0.6-1.0 parts of microfibrillated cellulose, 410-510 parts of water and 3.8-4.8 parts of polycarboxylic acid high-performance water reducer. The present invention replaces the van der Waals bond with weaker dissociation energy originally present in hydrated calcium silicate (C-S-H) with a hydrogen bond with higher dissociation energy, so that the matrix of ultra-high performance concrete needs to consume more energy when it is damaged and the dissociation of hydration products occurs, thereby improving the strength of the matrix of ultra-high performance concrete, and then improving the mechanical properties and anti-penetration ability of ultra-high performance concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new building materials, and in particular relates to a UHPC based on microfibrillated cellulose and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Ultra-High Performance Concrete (UHPC) is a new type of cement-based composite material with ultra-high strength, high toughness and high durability. Correspondingly, its anti-penetration performance is significantly improved compared to ordinary concrete. However, when the compressive strength of ultra-high performance concrete continues to increase after reaching a certain threshold, the anti-penetration performance does not further improve, that is, there is a platform effect in the improvement of anti-penetration performance. This platform effect is usually attributed to: on the one hand, coarse aggregates that are conducive to improving anti-penetration performance are eliminated during the preparation of ultra-high performance concrete; on the other hand, the matrix of ultra-high performance concrete is relatively weak.

[0004] At present, there are Chinese patents such as CN 117510158 A (Ultra-high performance concrete and its preparation method and application) that provide a technical solution for adding aggregates to ultra-high performance concrete. However, there is still a lack of effective technical means in the technical direction of how to improve the matrix performance of ultra-high performance concrete to improve its anti-penetration ability. Summary of the invention

[0005] In order to address the deficiencies of the prior art, the purpose of the present invention is to provide a UHPC based on microfibrillated cellulose and a preparation method and application thereof, by adding microfibrillated cellulose to increase the dissociation energy of the hydration product, thereby further improving the anti-penetration ability from the perspective of improving the matrix strength.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] In a first aspect, the present invention provides a UHPC based on microfibrillated cellulose, which is prepared from raw materials comprising the following components in parts by weight:

[0008] 1377-1577 parts of cement, 35-43 parts of steel fiber, 120-180 parts of silica fume, 0.6-1.0 parts of microfibrillated cellulose, 410-510 parts of water and 3.8-4.8 parts of polycarboxylic acid high-performance water reducing agent.

[0009] In a second aspect, the present invention provides a method for preparing the above-mentioned UHPC based on microfibrillated cellulose, comprising the following steps:

[0010] S1, mixing and dispersing the microfibrillated cellulose with a portion of water, and homogenizing the mixture to obtain a microfibrillated cellulose solution;

[0011] S2, mixing cement and silica fume until uniform, to obtain a first mixture;

[0012] S3, adding the microfibrillated cellulose solution and the polycarboxylate high-performance water-reducing agent prepared in S1 to the first mixture, stirring evenly, adding the remaining water, stirring until uniform, to obtain a second mixture;

[0013] S4. Sieve steel fibers into the second mixture, stir until uniform, and then pour and cure.

[0014] In a third aspect, the present invention provides an application of the above-mentioned UHPC based on microfibrillated cellulose in protective engineering and structural engineering.

[0015] The beneficial effects of the present invention are:

[0016] 1. Each anhydroglucose unit in the microfibrillated cellulose used in the present invention contains three hydroxyl groups, which will form hydrogen bonds when the hydroxyl groups combine with the hydration products in the concrete matrix, especially calcium silicate hydrate (CSH). The hydrogen bonds with higher dissociation energy replace the van der Waals bonds with lower dissociation energy in the calcium silicate hydrate (CSH), so that the matrix of the ultra-high performance concrete consumes more energy when the hydration products dissociate when the ultra-high performance concrete is damaged, thereby improving the strength of the ultra-high performance concrete matrix, and further improving the mechanical properties and anti-penetration ability of the ultra-high performance concrete.

[0017] 2. The present invention uses microfibrillated cellulose with a longer aspect ratio than ordinary cellulose to produce a bridging effect to inhibit the generation and expansion of cracks under the high-speed impact penetration of the projectile. At the same time, because microfibrillated cellulose and steel fiber are two fibers with different scales and strengths, their synergistic bridging effect changes the failure mode of ultra-high performance concrete under high-speed impact: from a crushing failure mode to a failure mode with good integrity, reducing the splashing of matrix fragments.

[0018] 3. Since microfibrillated cellulose has good hydrophilicity and hygroscopicity, during the preparation process, when it adheres to cement particles, it can break the outer shell formed by hydrated cement and further promote the hydration inside the cement particles. The degree of cement hydration can be increased from 56% to 61%. As a new type of internal curing agent, microfibrillated cellulose can also significantly and effectively reduce the autogenous shrinkage of concrete through a dual mechanism: the first mechanism is the internal curing effect, which leads to an increase in the early characteristic volume expansion, thereby significantly reducing the subsequent autogenous shrinkage. The second mechanism is related to the nano-enhancement effect that causes matrix bridging, thereby improving volume stability. These two mechanisms further reduce the internal stress of high-performance concrete blocks during service and improve their mechanical properties.

[0019] 4. By testing the mix ratio of the present invention, the compressive strength and peak strain of the ultra-high performance concrete with added microfibrillated cellulose were increased by 10.7% and 32% respectively, and the initial crack load was increased by 49% but the peak load did not change compared with the control group without microfibrillated cellulose. The penetration depth of the microfibrillated cellulose modified ultra-high performance concrete provided by the present invention under the action of a projectile of ~600m / s is 63.4mm and the pit diameter is 82.6mm. Compared with the control group without microfibrillated cellulose, the penetration depth is reduced by 20.3%. The excellent high-speed impact explosion resistance performance has greatly increased the application scope of ultra-high performance concrete in protective engineering. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0021] Figure 1 is a stress-strain curve diagram of an embodiment of a specific embodiment of the present invention;

[0022] Figure 2 is a force-displacement curve diagram of an embodiment of the present invention under a four-point bending test;

[0023] Figure 3 is a comparison curve of the hydration degree of the embodiment and the comparative example in the specific implementation mode of the present invention;

[0024] Figure 4 is a comparison curve of the degree of autogenous shrinkage deformation of the embodiment and the comparative example in the specific implementation mode of the present invention;

[0025] Figure 5 It is a comparison diagram of the pit diameters of the embodiment and the comparative example in the specific implementation manner of the present invention, wherein (a) is the pit diameter diagram of embodiment 1, and (b) is the pit diameter diagram of comparative example 1. DETAILED DESCRIPTION

[0026] A typical embodiment of the present invention provides a UHPC based on microfibrillated cellulose, which is prepared from raw materials including the following components in parts by weight:

[0027] 1377-1577 parts of cement, 35-43 parts of steel fiber, 120-180 parts of silica fume, 0.6-1.0 parts of microfibrillated cellulose, 410-510 parts of water and 3.8-4.8 parts of polycarboxylic acid high-performance water reducing agent.

[0028] Optionally, the cement is ordinary Portland cement of grade 52.5 or grade 52.5R, which has good compatibility with the polycarboxylic acid-based high-efficiency water reducing agent.

[0029] Optionally, the steel fiber is a copper-plated straight steel fiber with an average length of 13 mm and an average diameter of 0.16 mm, a tensile strength greater than 2500 MPa, an elastic modulus of 200 GPa, and a density of 7800 kg / m 3 .

[0030] Optionally, the silica fume has an amorphous silicon dioxide content greater than 95 wt % and a specific surface area greater than 21.0 m 2 / g, with a specific density greater than 2.2, which is an ultra-fine dry powder that has not been fully encrypted.

[0031] Optionally, microfibrillated cellulose (MFC), also known as micronized cellulose, refers to cellulose with a fiber structure of 2-10 nm thick and tens of microns in length;

[0032] Technical documents such as "Zhao Huafeng. Research on the properties of microfibrillated cellulose / polylactic acid packaging film [D]. Tianjin University of Science and Technology" and "Jiang Yan. Research on the influence of lignin on the preparation process and properties of microfibrillated fibers [D]. Guangxi University, 2019" disclose the chemical structure of microfibrillated cellulose;

[0033] The characteristics of its chemical structure are:

[0034]

[0035] Each anhydroglucose unit in microfibrillated cellulose contains multiple hydroxyl groups (3 in the above chemical structure), which can combine with calcium silicate hydrate (CSH) in the concrete matrix to form stronger hydrogen bonds to replace the weaker van der Waals bonds, thereby improving the strength of the ultra-high performance concrete matrix.

[0036] Optionally, the high-efficiency water reducer is a polycarboxylic acid water reducer, and the selected polycarboxylic acid water reducer has a solid content greater than 35% and a density of 1100 kg / m 3 .

[0037] Another typical embodiment of the present invention provides a method for preparing the above-mentioned UHPC based on microfibrillated cellulose, comprising the following steps:

[0038] S1, mixing and dispersing the microfibrillated cellulose with a portion of water, and homogenizing the mixture to obtain a microfibrillated cellulose solution;

[0039] S2, mixing cement and silica fume until uniform, to obtain a first mixture;

[0040] S3, adding the microfibrillated cellulose solution prepared in S1 to the first mixture, stirring evenly, adding a polycarboxylic acid high-performance water reducer, stirring evenly, adding the remaining water, stirring until uniform, to obtain a second mixture;

[0041] S4. Sieve steel fibers into the second mixture, stir until uniform, and then pour and cure.

[0042] Optionally, in S1, the microfibrillated cellulose is mixed with water accounting for 70% of the total water volume and then immersed for 24 hours to form a suspension, and the subsequent homogenization process includes: magnetic stirring for 10 minutes, and then ultrasonic dispersion for 30 minutes to form a stable microfibrillated cellulose solution, which is placed in a set temperature and humidity environment for standby use;

[0043] Optionally, the homogenization treatment of the microfibrillated cellulose solution may also be carried out by only performing magnetic stirring, and the stirring time is greater than 10 minutes.

[0044] Optionally, place in an environment with a temperature of 20±2°C and a relative humidity of >95%RH for standby use.

[0045] Optionally, in S2, cement and silica fume are mixed and stirred at a low speed for 20-40 minutes until they are uniform.

[0046] Optionally, in S3, after adding the microfibrillated cellulose solution and the water reducing agent, stir at a low speed for 2-3 minutes until uniform; after adding the water reducing agent, stir at a low speed for 3-5 minutes until uniform; after adding the remaining water, stir at a low speed for 3 to 5 minutes until uniform.

[0047] Optionally, in S4, after the fresh concrete has good fluidity, a square-hole sieve is used to drop the steel fiber sieve into the second mixture to prevent the steel fiber from agglomerating, and the mixture is stirred at a medium speed for 3 to 5 minutes until it is uniform;

[0048] Specifically, after the cementitious material can be well mixed and no obvious unhydrated material emerges on the surface of the fresh concrete, the steel fiber is sieved in.

[0049] Optionally, in S4, after high-speed stirring for 1 to 2 minutes, the mixture is cast into a mold and cured under standard curing conditions to a specified age;

[0050] Specifically, under the conditions of a temperature of 20±2°C and a relative humidity>95%RH, curing is performed to a specified age.

[0051] Optionally, the casting can be vibrated slightly for 1 to 2 minutes to help expel air bubbles and improve its density;

[0052] After pouring, cover with plastic film to prevent surface moisture loss and demould after 24 hours.

[0053] Another typical embodiment of the present invention provides the application of the above-mentioned anti-penetration UHPC based on microfibrillated cellulose modification and / or the above-mentioned preparation method, including: application in protective engineering and structural engineering;

[0054] Specifically, it includes: application in underground fortifications, nuclear waste storage facilities, missile protection positions, large-span bridge beam and slab structures, and rail transit bridge surfaces;

[0055] Also includes: Application in bridge reinforcement.

[0056] Example 1

[0057] A UHPC based on microfibrillated cellulose, comprising the following components in parts by weight:

[0058] 1477 parts of 52.5 or 52.5R grade ordinary Portland cement, 39 parts of copper-coated straight steel fiber, 148 parts of silica fume, 0.8 parts of microfibrillated cellulose, 455 parts of water and 4.3 parts of polycarboxylic acid high-performance water reducer,

[0059] Among them, microfibrillated cellulose is a commercially available product.

[0060] The preparation method is:

[0061] 0.8 parts of microfibrillated cellulose were soaked in 318.5 parts of water (70% of the amount in 455 parts of water) for 24 hours to form a suspension; the suspension was magnetically stirred for 10 minutes, and then ultrasonically dispersed for 30 minutes to promote the uniform dispersion of the microfibrillated cellulose before it was formally added into the concrete, and then the prepared microfibrillated cellulose solution was placed in an environment with ambient temperature (20±2°C) and relative humidity (>95%RH) for use.

[0062] Add 1477 parts of cement and 148 parts of silica fume into the mixer at one time, and stir at low speed for 2-3 minutes until mixed evenly.

[0063] Add the prepared microfibrillated cellulose solution to the mixer, stir evenly, then add 4.3 parts of polycarboxylic acid high-performance water reducer, continue stirring until evenly mixed, then add 136.5 parts of water (30% of the amount in 455 parts of water), and continue stirring at a low speed until evenly mixed.

[0064] Place 39 parts of copper-plated straight steel fibers in a square hole sieve, add them evenly into the mixer by sieving to prevent agglomeration, and stir at medium speed until uniform while sieving.

[0065] The slurry after medium-speed stirring is stirred at high speed and then poured into a mold, and cured under standard curing conditions (temperature: 20±2°C, and relative humidity: >95%RH) to a specified age.

[0066] Example 2

[0067] A UHPC based on microfibrillated cellulose, comprising the following components in parts by weight:

[0068] 1377 parts of 52.5 or 52.5R grade ordinary Portland cement, 35 parts of copper-coated straight steel fiber, 120 parts of silica fume, 0.6 parts of microfibrillated cellulose, 410 parts of water and 3.8 parts of polycarboxylic acid high-performance water reducer;

[0069] Among them, microfibrillated cellulose is a commercially available product.

[0070] The preparation method is the same as that in Example 1.

[0071] Example 3

[0072] A UHPC based on microfibrillated cellulose, comprising the following components in parts by weight:

[0073] 1577 parts of 52.5 or 52.5R grade ordinary Portland cement, 43 parts of copper-coated straight steel fiber, 180 parts of silica fume, 1.0 parts of microfibrillated cellulose, 510 parts of water and 4.8 parts of polycarboxylic acid high-performance water-reducing agent;

[0074] Among them, microfibrillated cellulose is a commercially available product.

[0075] The preparation method is the same as that in Example 1.

[0076] Comparative Example 1

[0077] Compared with Example 1, the difference in the formula components is that the ultra-high performance concrete without microfibrillated cellulose includes the following components in parts by weight: 1479 parts of 52.5 grade or 52.5R grade ordinary Portland cement, 148 parts of silica fume, 39 parts of copper-plated straight steel fibers, 452 parts of water and 4 parts of polycarboxylic acid-based high-efficiency water reducer.

[0078] The difference in the preparation method is that no microfibrillated cellulose solution is used, but water is directly used.

[0079] Conventional mechanical tests and high-speed projectile penetration resistance tests were performed on the ultra-high performance concrete of the above-mentioned embodiments and comparative examples. The results are shown in Table 1. The stress-strain specimen size and stress-strain curve are shown in Table 1. Figure 1 The specimen dimensions and force-displacement curve of the four-point bending test are shown in Figure 2 The test process of the high-speed projectile penetration resistance performance is the same as that of the Chinese patent application with application number 2023117815297 (a kind of penetration-resistant ultra-high performance concrete and its preparation method and application), but the target speed is increased from 400m / s to 600m / s.

[0080] Table 1

[0081]

[0082] In Table 1, penetration depth refers to the distance from the impact surface of the target to the deepest point of the crater;

[0083] The crater diameter is the diameter of an equivalent circle with the same area as the target crater;

[0084] The crater volume refers to the volume of the target crater.

[0085] It can be seen that: in terms of mechanical properties, as shown in Table 1 and Figure 1 As shown in Table 1, the compressive strength of Example 1 is increased by 10.7% and the peak strain is increased by 32% compared with that of Comparative Example 1. Figure 2 As shown, the initial crack load increased by 49%, but the peak load did not change, indicating that the present invention has made a breakthrough in the technical direction of improving the matrix strength of ultra-high performance concrete and fully exerted the mechanical potential of ultra-high performance concrete;

[0086] In terms of the performance against high-speed projectile penetration, under the action of a projectile at ~600m / s, as shown in Table 1 and Figure 5 As shown, Figure 5 The penetration depth of the microfibrillated cellulose modified ultra-high performance concrete of Comparative Example 1 represented by (a) is 63.4 mm and the pit diameter is 82.6 mm. Figure 5 Compared with Comparative Example 1 (penetration depth of 79.5 mm, opening diameter of 89.3 mm) which does not contain microfibrillated cellulose as shown in (b), the penetration depth is reduced by 20.3%.

[0087] Compared with comparative example 1, the mechanical properties of Example 1 are greatly improved, which is mainly attributed to the strong covalent bonds formed between the hydration products in the ultra-high performance concrete due to the addition of microfibrillated cellulose;

[0088] At the molecular level, the main substance that provides cohesion and mechanical properties in cement-based composites is the hydration product of ordinary Portland cement, mainly calcium silicate hydrate (CSH), most of which are connected by weak van der Waals forces. Molecules connected by van der Waals forces can dissociate when subjected to an energy of 0.4 to 4.0 kJ / mol. Each anhydroglucose unit in microfibrillated cellulose contains three hydroxyl groups. When the hydroxyl groups combine with CSH, stronger hydrogen bonds are formed to replace van der Waals forces for connection. The dissociation energy of hydrogen bonds is 42 kJ / mol, which is significantly higher than that of van der Waals bonds. As a result, the mechanical properties of ultra-high performance concrete have also been significantly improved.

[0089] During the hydration process, the hydrated cement will form a harder shell outside the unhydrated cement particles, preventing the interior of the cement particles from further hydrating, causing local fluctuations in the degree of hydration inside and outside the particles, that is, uneven hydration on the scale of cement particles. Since microfibrillated cellulose has good hydrophilicity and hygroscopicity, it will adhere to the cement particles after being added to the ultra-high performance concrete matrix, and a harder shell will be formed on the outside of the cement particles, and the microfibrillated cellulose will be trapped in the shell. The microfibrillated cellulose inside and outside the shell provides a channel for water to be transported to the interior of the unhydrated cement, thereby further improving the hydration degree of the cement. At the same time, microfibrillated cellulose will generate a lot of heat during hydration, which is also conducive to the further hydration of cement. The compressive strength, flexural strength, toughness and anti-penetration performance of ultra-high performance concrete are greatly improved.

[0090] Hydration test results Figure 3 As shown, the hydration degree was determined by hydrothermal method; the autogenous shrinkage deformation test results are shown in Figure 4 As shown, the autogenous shrinkage deformation is measured by a non-contact bellows shrinkage and expansion measuring instrument, which reflects the effective improvement of the technical solution of the present invention on the autogenous shrinkage deformation;

[0091] It can be seen from Table 1 that compared with the target of Comparative Example 1, the target of Example 1 has excellent mechanical properties and anti-penetration performance, especially the pit diameter. The penetration depth of the ultra-high performance concrete in Example 1 under the action of an 8mm diameter projectile and a target impact speed of ~600m / s is 63.4mm, which is 20% lower than that of the ultra-high performance concrete (79.5mm) without microfibrillated cellulose in Comparative Example 1; the pit diameter is 82.6, which is 7.5% lower than that of the ultra-high performance concrete (89.3mm) without microfibrillated cellulose in Comparative Example 1; the mass loss rate of the projectile in Example 1 is higher than that in Comparative Example 1, indicating that the warhead of the projectile in Example 1 is more seriously worn. It can be seen that after the hydration reaction between microfibrillated cellulose and CSH, the compressive strength of the concrete is significantly improved, and more energy is required to destroy the covalent bond, so the pit diameter is also significantly reduced.

[0092] The present invention provides an ultra-high performance concrete based on microfibrillated cellulose with high anti-penetration performance and excellent mechanical properties, and its anti-penetration performance is significantly higher than that of Comparative Example 1 which does not contain microfibrillated cellulose. It can be seen that the "organic-inorganic CSH hybrid" formed by the addition of microfibrillated cellulose has greatly improved the mechanical properties and anti-penetration performance of ultra-high performance concrete. On the one hand, microfibrillated cellulose can provide stronger covalent bonds for ultra-high performance concrete, thereby improving its mechanical properties; on the other hand, microfibrillated cellulose adsorbed on cement particles can promote further hydration of cement by utilizing its strong hydrophilicity and hygroscopicity. The matrix performance of ultra-high performance concrete is improved from multiple aspects, which makes up for the relatively weak shortcomings of the matrix performance in ultra-high performance concrete and gives full play to the overall mechanical potential of ultra-high performance concrete.

[0093] Microfibrillated cellulose further optimizes the mechanical properties and anti-penetration performance of ultra-high performance concrete, making it more widely used in the field of modern new protective materials. It can be used in underground fortifications, nuclear waste storage devices, missile protection positions, large-span bridge beam and slab structures, rail transit bridge surface layers; it can also be used in bridge reinforcement.

[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A UHPC based on microfibrillated cellulose, characterized in that: It is prepared from raw materials comprising the following components in parts by weight: 1377-1577 parts of cement, 35-43 parts of steel fiber, 120-180 parts of silica fume, 0.6-1.0 parts of microfibrillated cellulose, 410-510 parts of water and 3.8-4.8 parts of polycarboxylic acid high-performance water reducer; The microfibrillated cellulose refers to cellulose with a fiber structure of 2 to 10 nm thick and a length of tens of microns; The method for preparing UHPC based on microfibrillated cellulose comprises the following steps: S1, mixing and dispersing microfibrillated cellulose with a portion of water, and homogenizing to obtain a microfibrillated cellulose solution; specifically, mixing the microfibrillated cellulose with water and then soaking to form a suspension, then magnetically stirring, and then ultrasonically dispersing to form a stable microfibrillated cellulose solution, and placing it in a set temperature and humidity environment for standby; S2, mixing cement and silica fume until uniform, to obtain a first mixture; S3, adding the microfibrillated cellulose solution prepared in S1 to the first mixture, stirring evenly, adding a polycarboxylic acid high-performance water reducer, stirring evenly, adding the remaining water, stirring until uniform, to obtain a second mixture; S4. Sieve steel fibers into the second mixture, stir until uniform, and then pour and cure.

2. The UHPC based on microfibrillated cellulose according to claim 1, characterized in that The cement is ordinary Portland cement of grade 52.5 or grade 52.5R.

3. The UHPC based on microfibrillated cellulose according to claim 1, characterized in that The steel fiber is a copper-plated straight steel fiber with an average length of 13 mm and an average diameter of 0.16 mm, a tensile strength of more than 2500 MPa, and an elastic modulus of 200 GPa.

4. The UHPC based on microfibrillated cellulose according to claim 1, characterized in that The silica ash has an amorphous silicon dioxide content greater than 95wt%, a specific surface area greater than 21.0 m2 / g, and a specific density greater than 2.

2.

5. The UHPC based on microfibrillated cellulose according to claim 1, characterized in that The polycarboxylic acid high-performance water reducer is a polycarboxylic acid-based water reducer with a solid content greater than 35% and a density of 1100 kg / m3.

6. The UHPC based on microfibrillated cellulose according to any one of claims 1 to 5, characterized in that: It is prepared from raw materials comprising the following components in parts by weight: 1477 parts of 52.5 or 52.5R grade ordinary Portland cement, 39 parts of copper-coated straight steel fibers, 148 parts of incompletely densified silica fume, 0.8 parts of microfibrillated cellulose, 455 parts of water and 4.3 parts of polycarboxylic acid high-performance water-reducing agent.

7. A method for preparing UHPC based on microfibrillated cellulose according to any one of claims 1 to 6, characterized in that: The steps include: S1, mixing and dispersing the microfibrillated cellulose with a portion of water, and homogenizing the mixture to obtain a microfibrillated cellulose solution; S2, mixing cement and silica fume until uniform, to obtain a first mixture; S3, adding the microfibrillated cellulose solution prepared in S1 to the first mixture, stirring evenly, adding a polycarboxylic acid high-performance water reducer, stirring evenly, adding the remaining water, stirring until uniform, to obtain a second mixture; S4. Sieve steel fibers into the second mixture, stir until uniform, and then pour and cure.

8. The preparation method according to claim 7, characterized in that: In S1, the microfibrillated cellulose is mixed with water and then soaked to form a suspension, followed by magnetic stirring and ultrasonic dispersion to form a stable microfibrillated cellulose solution, which is placed in a set temperature and humidity environment for use.

9. The preparation method according to claim 7, characterized in that: In S2, cement and silica fume are mixed and stirred at a low speed for 20-40 minutes until they are uniform.

10. The preparation method according to claim 7, characterized in that: In S3, after adding the microfibrillated cellulose solution and the water reducing agent, stir at a low speed for 2-3 minutes until uniform; after adding the water reducing agent, stir at a low speed for 3-5 minutes until uniform; after adding the remaining water, stir at a low speed for 3-5 minutes until uniform.

11. The preparation method according to claim 7, characterized in that: In S4, a square hole sieve is used to drop the steel fiber sieve into the second mixture, and the mixture is stirred at a medium speed for 3 to 5 minutes until it is uniform. After stirring at a high speed for 1 to 2 minutes, the mixture is cast into shape and cured under standard curing conditions to a specified age.

12. An application of the UHPC based on microfibrillated cellulose as claimed in any one of claims 1 to 6 or the preparation method as claimed in any one of claims 7 to 11 in protective engineering and structural engineering, characterized in that: include: It is used in underground fortifications, nuclear waste storage facilities, missile protection positions, large-span bridge beam and slab structures, and rail transit bridge surfaces.

13. A use according to claim 12, characterized in that: include: Application in bridge reinforcement.