A sealing gasket with long-term anti-leakage function and its preparation process

By using a combination of multi-effect modified styrene-butadiene rubber and self-healing epoxy resin in the sealing gasket, combined with the construction of acid-induced graphene oxide and functional microspheres, the problems of sealing gasket wear, cracks and aging failure are solved. It achieves efficient self-healing performance and long-lasting leakage prevention function.

CN118359889BActive Publication Date: 2024-10-25WUXI XIXI CHEM MASCH PARTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410646592.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-25
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

Existing sealing gaskets are prone to failure due to wear, cracks and aging after long-term use, resulting in a decrease in sealing performance. There is a lack of effective self-healing materials to improve long-term leakage prevention capabilities.

Method used

Using a combination of multi-effect modified styrene-butadiene rubber and self-healing epoxy resin, through acid treatment of graphene oxide, the construction of mesoporous microsphere-graphene oxide composites and functional microspheres, dynamic disulfide bonds are introduced to achieve self-repair. Repair properties and form a hybrid cross-linked structure during the vulcanization process.

Benefits of technology

It significantly improves the mechanical strength, anti-wear performance and aging resistance of the sealing gasket, provides good self-healing ability, extends the service life and reduces the probability of leakage failure, achieving long-term anti-leakage function.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118359889B_ABST
    Figure CN118359889B_ABST
Patent Text Reader

Abstract

The present invention discloses a sealing gasket with a long-term anti-leakage function and a preparation process thereof. The raw materials for preparing the sealing gasket include the following components by weight: 100 parts of multi-effect modified styrene-butadiene rubber; 13-56 parts of self-healing epoxy resin; 7.5-28 parts of nitrile rubber; 5-22 parts of white carbon black; 0.5-1.5 parts of zinc oxide; 0.4-1.2 parts of sulfur; 5.5-25 parts of additives. The sealing gasket provided by the present invention has excellent mechanical strength, wear resistance, and aging resistance, and has good self-repairing ability, can provide a long-term anti-leakage function, and has broad market application prospects; in the present invention, the multi-effect modified styrene-butadiene rubber can improve the mechanical strength and wear resistance of the system, and by introducing an ionic bond-covalent bond hybrid cross-linked network structure, it can give the sealing gasket excellent self-repairing performance and improve tensile strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sealing materials, and in particular to a sealing gasket with a long-term anti-leakage function and a preparation process thereof. Background Art

[0002] Sealing gaskets are widely used in the sealing of various equipment in modern industry. According to the material, they can be divided into metal sealing gaskets and non-metallic sealing gaskets. Metal gaskets include copper gaskets, stainless steel gaskets, iron gaskets, aluminum gaskets, etc. Non-metallic gaskets include asbestos gaskets, non-asbestos gaskets, paper gaskets, rubber gaskets, etc. Various new materials and new structures are constantly emerging, and their sealing performance is also very different. In addition, pressure fluctuations, temperature changes, loosening of bolt preload, flange tilt and misalignment, defects in sealing surfaces, and corrosion of the medium will have a great impact on the sealing effect. Therefore, how to correctly select the appropriate sealing gasket according to the actual working conditions.

[0003] Rubber gaskets have become a widely cited sealing material due to their excellent sealing performance, good wear resistance, and chemical resistance. For example, patent CN113429687B discloses a puncture-resistant rubber material and sealing gasket, and patent CN115558175A discloses a method for preparing an oil-resistant rubber gasket and a high-strength oil-resistant rubber expansion joint. During use, due to damage caused by the environment, stress, etc., the sealing gasket is inevitably prone to failure after long-term use. The main failure forms include:

[0004] 1. Wear failure

[0005] During the use of gaskets, due to the influence of friction, they will gradually wear out, which will be manifested as filamentary grinding, holes, grooves, etc. on the gasket surface. This failure form will cause the gasket performance to gradually decrease, affecting the sealing effect or even losing the sealing effect. Therefore, it is necessary to prevent wear during use, such as applying appropriate lubricants during installation and reducing friction.

[0006] 2. Crack failure

[0007] During the use of gaskets, cracks may appear due to the influence of external forces or insufficient strength. Cracks are divided into two forms: surface cracks and internal cracks. Surface cracks may cause leakage and rupture, while internal cracks may reduce the performance of the gasket and affect the sealing effect. Therefore, choosing the right material and avoiding excessive stretching can effectively prevent the occurrence of cracks.

[0008] 3. Aging failure

[0009] After long-term use, gaskets will lose their performance due to material aging, which manifests as deformation, hardening, loss of elasticity, etc. This failure form is usually related to factors such as gasket materials and use environment. For example, high temperature, ultraviolet rays and other environments will accelerate aging. Therefore, choosing the right material and avoiding excessive aging can effectively prevent aging failure.

[0010] The occurrence of failure can be reduced by improving the overall strength of the sealing material, and by introducing self-healing materials to repair crack failures, a longer-lasting sealing effect is expected to be provided.

[0011] Disulfide bonds are usually formed by coupling two thiol groups. The bond energy of disulfide bonds is weaker than that of carbon-carbon single bonds and carbon-hydrogen bonds. In many molecular structures, disulfide bonds are usually weak bonds. Introducing disulfide bonds into functional materials can make them have self-healing properties, mainly because disulfide bonds are reversible under certain conditions (Zhou Zhen, Su Xunzheng, Liu Jingcheng, et al. Research progress of intrinsic self-healing coatings prepared based on photochemical reactions [J]. Imaging Science and Photochemistry, 2020, 38(5):10.DOI:10.7517 / issn.1674-0475.200404.). The "bond" of disulfide bonds is not strong, so the connection between S atoms and S atoms is easy to break. However, the broken SS bond can reconnect with other broken SS bonds to form a new SS covalent bond "bond", so it is called a dynamic disulfide bond.

[0012] At present, the preparation of polymer materials by introducing disulfide bonds has been widely used, such as the literature: Yan Wenkang. Research on the preparation and performance of intrinsic self-healing polyurethane materials based on disulfide bonds [D]. Nanchang Hangkong University, 2021. Or patent CN104610587B a self-healing and recyclable vulcanized rubber and its preparation method and application, patent CN110862589A a styrene-butadiene rubber with self-healing function and preparation method, etc., but it usually requires heating conditions to achieve self-repair, and the repair effect is poor.

[0013] If self-healing materials can be introduced into sealing gaskets and their self-healing ability and overall performance can be further improved, it will greatly help to improve the use effect of sealing gaskets, but there is currently a lack of reliable solutions. Summary of the invention

[0014] The technical problem to be solved by the present invention is to provide a sealing gasket with a long-term anti-leakage function and a preparation process thereof in view of the deficiencies in the above-mentioned prior art.

[0015] In order to solve the above technical problems, the technical solution adopted by the present invention is: a sealing gasket with long-term anti-leakage function, characterized in that the raw materials for its preparation include the following components in parts by weight:

[0016]

[0017] Preferably, the auxiliary agent comprises, by weight: 1 to 5 parts of antioxidant, 1.5-5 parts of vulcanization accelerator, 1 to 5 parts of stearic acid, and 2 to 10 parts of paraffin.

[0018] Preferably, the multi-effect modified styrene-butadiene rubber is prepared by the following method:

[0019] S1, treating graphene oxide with acid to obtain modified graphene oxide;

[0020] S2, in situ grafting iron aluminum oxide onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite;

[0021] S3, modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres;

[0022] S4, mixing the functional microspheres, 2-acrylamide-2-methylpropane sulfonic acid and styrene-butadiene rubber to obtain the multi-effect modified styrene-butadiene rubber.

[0023] Preferably, step S2 specifically comprises:

[0024] S2-1, taking 1.75-7.0 g of modified graphene oxide and adding it to 25-100 mL of ethanol, and ultrasonically dispersing it for 15-60 min to obtain a modified graphene oxide dispersion;

[0025] S2-2, add 2-8g of hexadecyltrimethylammonium bromide to 50-200mL of ethanol, then add 2.5-10mL of hydrochloric acid with a mass concentration of 5-20%, 1-5mL of nitric acid with a mass concentration of 5-20%, 3.57-14.28g of aluminum isopropoxide, 0.315-1.26g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 35-45°C for 3-12h, and adjust the pH value to 7-8 with sodium hydroxide; let stand at room temperature for 1-4h, and then dry at 90-100°C for 6-24h, and finally calcine at 400-600°C in an air atmosphere for 1.5-6h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite.

[0026] Preferably, step S3 is specifically:

[0027] S3-1, adding 1-4 g of the mesoporous microsphere-graphene oxide composite into 100-300 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 15-60 min;

[0028] S3-2. Add 0.82-3.28 g of citric acid, 0.6-2.4 g of urea, and 0.375-1.5 g of 4-hydroxyphenylboric acid to the mixture obtained in step S3-1, and ultrasonically disperse for 30-60 min. Then transfer to a polytetrafluoroethylene-lined reactor, react at 170-190° C. for 4-12 h. After the reaction is completed, cool to room temperature, filter, wash the solid product with deionized water, and vacuum dry at 50-70° C. for 6-12 h to obtain functional microspheres.

[0029] Preferably, step S4 is specifically:

[0030] 4-16g of functional microspheres, 3.25-13.0g of 2-acrylamide-2-methylpropanesulfonic acid, 0.4-1.5g of dicumyl peroxide and 100g of styrene-butadiene rubber are added into an internal mixer and mixed at 70-80°C for 15-40min to obtain multi-effect modified styrene-butadiene rubber.

[0031] Preferably, S1, treating graphene oxide with an acid to obtain modified graphene oxide:

[0032] 5 g of graphene oxide was added to a mixed acid solution consisting of 50 mL of 60% nitric acid and 25 mL of 95% sulfuric acid, stirred and refluxed at 70° C. for 4 h, filtered, and the solid product was washed with deionized water until neutral, and vacuum dried at 90° C. for 10 h to obtain modified graphene oxide;

[0033] S2. In-situ grafting of iron and aluminum oxides onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite:

[0034] S2-1, taking 3.5 g of modified graphene oxide and adding it into 50 mL of ethanol, and ultrasonically dispersing it for 30 min to obtain a modified graphene oxide dispersion;

[0035] S2-2, add 4 g of hexadecyltrimethylammonium bromide to 100 mL of ethanol, then add 5 mL of 10% hydrochloric acid, 2 mL of 10% nitric acid, 7.14 g of aluminum isopropoxide, 0.63 g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 40° C. for 6 h; adjust the pH value to 7 with sodium hydroxide; let stand at room temperature for 2 h, then dry at 100° C. for 12 h, and finally calcine at 500° C. in an air atmosphere for 4 h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite;

[0036] S3. Modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres:

[0037] S3-1, adding 2 g of mesoporous microsphere-graphene oxide composite into 150 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 30 min;

[0038] S3-2, add 1.64g citric acid, 1.2g urea, and 0.75g 4-hydroxyphenylboric acid to the mixture obtained in step S3-1, ultrasonically disperse for 45min, then transfer to a polytetrafluoroethylene-lined reactor, react at 180°C for 6h, cool to room temperature after the reaction, filter, wash the solid product with deionized water, and vacuum dry at 60°C for 8h to obtain functional microspheres;

[0039] S4. Add 8 g of functional microspheres, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of dicumyl peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

[0040] Preferably, the self-healing epoxy resin is prepared by the following method:

[0041] Add 6-24g of bis(4-epoxypropoxy)diphenyl disulfide, 1.2-4.8g of polypropylene glycol diglycidyl ether, and 2.9-11.6g of diethylenetriamine to 12-50g of ethanol, stir and react at 65-90°C for 15-60min, place the obtained product in a vacuum oven, degas at 50-70°C for 10-40min, then keep warm at 100-130°C for 1-4h, and cool to room temperature to obtain a self-healing epoxy resin.

[0042] Preferably, the self-healing epoxy resin is prepared by the following method:

[0043] 12 g of bis(4-glycidoxy)diphenyl disulfide, 2.4 g of polypropylene glycol diglycidyl ether, and 5.8 g of diethylenetriamine were added to 25 g of ethanol, and the reaction was stirred at 80°C for 30 min. The resulting product was placed in a vacuum oven, degassed at 60°C for 20 min, then kept at 120°C for 2 h, and cooled to room temperature to obtain a self-healing epoxy resin.

[0044] The present invention also provides a process for preparing the sealing gasket with long-term anti-leakage function as described above, comprising the following steps:

[0045] Step 1, internal mixing: add multi-effect modified styrene-butadiene rubber, self-repairing epoxy resin, nitrile rubber, white carbon black, zinc oxide, antioxidant, and stearic acid into an internal mixer, mix at 70-90° C. for 3-15 minutes to obtain an internal mixing rubber compound;

[0046] Step 2, open refining: add the internal mixing rubber, sulfur, paraffin wax and vulcanization accelerator into an open refining mill, mix at 60-75°C for 5-20 minutes, discharge the material, place it in an injection molding machine for sheeting, and obtain a raw rubber gasket;

[0047] Step 3, vulcanization: vulcanize the raw rubber gasket in a vulcanizer at 155-185°C for 10-45min and a vulcanization pressure of 7-20MPa to obtain a sealing gasket.

[0048] The beneficial effects of the present invention are:

[0049] The sealing gasket provided by the present invention has excellent mechanical strength, wear resistance, aging resistance, and good self-repairing ability, can provide a long-term anti-leakage function, and has broad market application prospects;

[0050] In the present invention, the multi-effect modified styrene-butadiene rubber can improve the mechanical strength and wear resistance of the system, and by introducing an ionic bond-covalent bond hybrid cross-linked network structure, it can give the sealing gasket excellent self-repairing performance and improve the tensile strength;

[0051] In the present invention, the self-healing epoxy resin can improve the strength and chemical resistance of the system, and endow the system with good self-healing properties by introducing disulfide bonds; and the multi-effect modified styrene-butadiene rubber and the self-healing epoxy resin can produce a coordinated cooperation effect, and the self-healing performance brought by the self-healing epoxy resin to the system can be improved by means of the catalytic promotion effect of the functional microspheres in the multi-effect modified styrene-butadiene rubber on the disulfide bond exchange in the self-healing epoxy resin system; the role of the self-healing performance is: when cracks / cracks appear on the sealing gasket due to the use environment, stress, etc., the self-healing function provided by the combination of the multi-effect modified styrene-butadiene rubber and the self-healing epoxy resin can be used to repair the cracks / cracks, thereby greatly reducing the occurrence of crack failures, thereby endowing the sealing gasket with a long-term anti-leakage function; the improvement of mechanical strength, wear resistance and aging resistance can effectively reduce the probability of wear failure, aging failure, etc., thereby improving the use effect of the sealing gasket and extending its service life;

[0052] In the present invention, the addition of the self-healing epoxy resin can provide excellent self-healing performance for the sealing gasket system and further improve its wear resistance and strength. The functional microspheres of the GO-AlMnO@NB-CDs structure in the multi-effect modified styrene-butadiene rubber can also cooperate with the self-healing epoxy resin. The catalytic effect of manganese dioxide in the functional microspheres on the disulfide bond exchange reaction and the co-catalytic effect of carbon point modification can enhance the self-healing performance provided by the self-healing epoxy resin.

[0053] In the sealing gasket system of the present invention, the disulfide bonds introduced in the self-repairing epoxy resin, the ionic bonds existing in the multi-effect modified styrene-butadiene rubber system and the dynamic BO bonds can provide it with self-repairing properties, thereby giving it a long-term anti-leakage function, which can significantly improve its sealing effect and extend its service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 The XRD pattern of the multi-effect modified styrene-butadiene rubber prepared in Example 1;

[0055] Figure 2 is the infrared absorption spectrum of the functional microspheres prepared in Example 1;

[0056] Figure 3 is the test result of tensile strength in the test example;

[0057] Figure 4 This is the self-repair rate test result at 25℃ and 2h in the test case;

[0058] Figure 5 The self-repair rate test results of the test case at different treatment temperatures for 2 hours;

[0059] Figure 6 The self-repair rate test results of different treatment times at 80°C in the test example. DETAILED DESCRIPTION

[0060] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0061] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0062] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0063] The present invention provides a sealing gasket with a long-term anti-leakage function, and the raw materials for preparing the sealing gasket include the following components in parts by weight:

[0064]

[0065] The auxiliary agents include, by weight: 1 to 5 parts of antioxidant, 1.5 to 5 parts of vulcanization accelerator, 1 to 5 parts of stearic acid, and 2 to 10 parts of paraffin.

[0066] In a preferred embodiment, the multi-effect modified styrene-butadiene rubber is prepared by the following method:

[0067] S1. Treating graphene oxide with acid to obtain modified graphene oxide:

[0068] 5 g of graphene oxide is added to a mixed acid solution consisting of 25-100 mL of 60% nitric acid and 25 mL of 95% sulfuric acid, stirred and refluxed at 60-80° C. for 1-8 h, cooled to room temperature and filtered, the solid product is washed with deionized water until neutral, and vacuum dried at 80-100° C. for 6-12 h to obtain modified graphene oxide;

[0069] S2. In-situ grafting of iron and aluminum oxides onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite:

[0070] S2-1, taking 1.75-7.0 g of modified graphene oxide and adding it into 25-100 mL of ethanol, and ultrasonically dispersing it for 15-60 min to obtain a modified graphene oxide dispersion;

[0071] S2-2, add 2-8g of hexadecyltrimethylammonium bromide (CTAB) to 50-200mL of ethanol, then add 2.5-10mL of hydrochloric acid with a mass concentration of 5-20%, 1-5mL of nitric acid with a mass concentration of 5-20%, 3.57-14.28g of aluminum isopropoxide, 0.315-1.26g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 35-45°C for 3-12h, and adjust the pH value to 7-8 with sodium hydroxide; let stand at room temperature for 1-4h, and then dry at 90-100°C for 6-24h, and finally calcine at 400-600°C in an air atmosphere for 1.5-6h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite.

[0072] S3. Modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres:

[0073] S3-1, adding 1-4 g of the mesoporous microsphere-graphene oxide composite into 100-300 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 15-60 min;

[0074] S3-2, add 0.82-3.28g citric acid, 0.6-2.4g urea, and 0.375-1.5g 4-hydroxyphenylboric acid to the mixture obtained in step S3-1, ultrasonically disperse for 30-60min, then transfer to a polytetrafluoroethylene-lined reactor, react at 170-190°C for 4-12h, cool to room temperature after the reaction, filter, wash the solid product with deionized water, and vacuum dry at 50-70°C for 6-12h to obtain functional microspheres;

[0075] S4, add 4-16g of functional microspheres, 3.25-13.0g of 2-acrylamide-2-methylpropanesulfonic acid, 0.4-1.5g of dicumyl peroxide, and 100g of styrene-butadiene rubber into an internal mixer, and mix at 70-80°C for 15-40min to obtain multi-effect modified styrene-butadiene rubber.

[0076] In a preferred embodiment, the self-healing epoxy resin is prepared by the following method:

[0077] Add 6-24g of bis(4-epoxypropoxy)diphenyl disulfide, 1.2-4.8g of polypropylene glycol diglycidyl ether, and 2.9-11.6g of diethylenetriamine to 12-50g of ethanol, stir and react at 65-90°C for 15-60min, place the obtained product in a vacuum oven, degas at 50-70°C for 10-40min, then keep warm at 100-130°C for 1-4h, and cool to room temperature to obtain a self-healing epoxy resin.

[0078] The present invention also provides a preparation process of a sealing gasket with a long-term anti-leakage function, comprising the following steps:

[0079] Step 1, internal mixing: add multi-effect modified styrene-butadiene rubber, self-repairing epoxy resin, nitrile rubber, white carbon black, zinc oxide, antioxidant, and stearic acid into an internal mixer, mix at 70-90° C. for 3-15 minutes to obtain an internal mixing rubber compound;

[0080] Step 2, open refining: add the internal mixing rubber, sulfur, paraffin wax and vulcanization accelerator into an open refining mill, mix at 60-75°C for 5-20 minutes, discharge the material, place it in an injection molding machine for sheeting, and obtain a raw rubber gasket;

[0081] Step 3, vulcanization: vulcanize the raw rubber gasket in a vulcanizer at 155-185°C for 10-45min and a vulcanization pressure of 7-20MPa to obtain a sealing gasket.

[0082] In the present invention, the multi-effect modified styrene-butadiene rubber can improve the mechanical strength and wear resistance of the system, and by introducing an ionic bond-covalent bond hybrid cross-linked network structure, it can give the sealing gasket excellent self-repairing performance and improve the tensile strength;

[0083] In the present invention, the self-healing epoxy resin can improve the strength and chemical resistance of the system, and endow the system with good self-healing performance by introducing disulfide bonds; and the multi-effect modified styrene-butadiene rubber and the self-healing epoxy resin can produce a coordinated cooperation effect, and the self-healing performance brought by the self-healing epoxy resin to the system can be improved by means of the catalytic promotion effect of the functional microspheres in the multi-effect modified styrene-butadiene rubber on the disulfide bond exchange in the self-healing epoxy resin system;

[0084] The role of self-repairing performance is that when cracks / cracks appear on the sealing gasket due to the use environment, stress, etc., the self-repairing function provided by the combination of multi-effect modified styrene-butadiene rubber and self-repairing epoxy resin can be used to repair the cracks / cracks, thereby greatly reducing the occurrence of crack failures, thereby giving the sealing gasket a long-term anti-leakage function. The improvement of mechanical strength, wear resistance and aging resistance can effectively reduce the probability of wear failure, aging failure, etc., thereby improving the use effect of the sealing gasket and extending its service life.

[0085] The main mechanism of the present invention is described in detail below in conjunction with a specific preparation method to facilitate understanding of the present invention.

[0086] 1. Multi-effect modified styrene butadiene rubber:

[0087] 1. The present invention firstly performs an acid treatment on the flaky monolayer graphene oxide by mixed acid to introduce abundant oxygen-containing functional groups such as carboxyl groups on its surface;

[0088] 2. Then, manganese-doped mesoporous alumina microspheres were grafted onto the surface of the flake monolayer graphene oxide by in-situ co-precipitation to obtain a mesoporous microsphere-graphene oxide composite: GO-AlMnO. In this process, the abundant carboxyl and other oxygen-containing functional groups on the surface of the monolayer graphene oxide can adsorb a large amount of added Al 3+ and Mn 2+ , so that the metal ions are uniformly and massively connected to the surface of the monolayer graphene oxide, and CTAB is used as a template, and a sol-gel method is used to finally obtain uniformly distributed manganese dioxide-aluminum dioxide composite mesoporous microspheres, namely manganese-doped mesoporous alumina microspheres, denoted as AlMnO; the mesoporous structure can increase the surface area, which is conducive to the subsequent modification of carbon dots;

[0089] 3. Then, citric acid was used as a carbon source, urea as a nitrogen source, and 4-hydroxyphenylboric acid as a boron source, and a one-pot hydrothermal method was used to in situ modify rich nitrogen-boron co-doped carbon dots on GO-AlMnO to obtain functional microspheres GO-AlMnO@NB-CDs; the surface of the carbon dots has rich functional groups such as amino, carboxyl, and hydroxyl groups; during the preparation process, metal ions can be generated on the manganese-doped mesoporous alumina microspheres under the action of citric acid, so that citric acid, urea, and 4-hydroxyphenylboric acid can in situ form a large number of nitrogen-boron co-doped carbon dots on the manganese-doped mesoporous alumina microspheres;

[0090] 4. Finally, the functional microspheres, 2-acrylamide-2-methylpropane sulfonic acid and styrene-butadiene rubber were mixed to obtain the final multi-effect modified styrene-butadiene rubber, which was recorded as SBR-GO-AlMnO@NB-CDs. In this process, the sulfonic acid groups in 2-acrylamide-2-methylpropane sulfonic acid can form ionic bonds with the metal manganese and aluminum in the manganese-doped mesoporous alumina microspheres, and 2-acrylamide-2-methylpropane sulfonic acid is very easy to self-polymerize and grafted onto the main chain of styrene-butadiene rubber in the form of long chains and branches. The bridging effect of 2-acrylamide-2-methylpropane sulfonic acid can promote the uniform dispersion of functional microspheres in styrene-butadiene rubber. A covalent cross-linking structure can be formed in styrene-butadiene rubber, and the ionic bond cross-linking and covalent cross-linking structures are interspersed to form a hybrid cross-linking structure. When subjected to stress, the weaker ionic bonds are preferentially "sacrificed" to break and dissipate energy, and then new ionic bonds can be re-formed. The reversibility of ionic bonds gives rubber self-healing ability (Xia YZ QA facile and environmentally friendly approach to fabricate hybrid crosslinked nitrile butadiene rubber with comprehensively improved mechanical performances by incorporating sacrificial ionic bonds [J]. Polymer: The International Journal for the Science and Technology of Polymers, 2019, 161.);

[0091] The structural system of the multi-effect modified styrene-butadiene rubber synthesized and constructed by the present invention can at least bring the following effects:

[0092] 1) Manganese-doped mesoporous alumina microspheres are used as the basic carrier and provide filling. Alumina can provide the following functions: improving the hardness, strength, wear resistance and anti-aging properties of rubber; manganese dioxide has a catalytic effect on disulfide bond exchange reaction (Mei Jinfeng. Synthesis and properties of autonomous self-healing materials based on dynamic non-covalent bonds [D]. Nanjing University [2024-04-25].), thereby improving the self-healing ability of the disulfide bond-endowed system introduced in the self-healing epoxy resin;

[0093] The effects of nitrogen-boron co-doped carbon dots include: (1) first, it can introduce abundant functional groups into the functional microspheres, which is beneficial to the dispersion of the functional microspheres; (2) it has an enhancing effect on the catalytic activity of manganese dioxide, which is mainly attributed to the sp 2 and sp 3 The hybrid carbon interface structure and the huge electron acceptor / donor function promote electron transfer, which enhances the catalytic activity of manganese dioxide; (3) B doping in carbon dots enables a certain amount of dynamic BO bonds to be formed in the final system. The dynamic nature of the BO bonds makes it repairable (Li Qianqian. Conductive self-healing materials based on reversible boron-oxygen bond cross-linked terminal hydroxyl polybutadiene [D]. Hefei University of Technology [2024-04-25].), thus providing the system with a certain self-healing ability on the other hand.

[0094] The functions of graphene oxide include: improving the strength, wear resistance, oxidation resistance and weather resistance of the rubber system; however, conventional graphene oxide is easy to curl and agglomerate in the rubber system, which makes its reinforcing performance unable to be fully exerted. In the present invention, this problem can be well overcome. The main principle is: in the functional microspheres of the constructed GO-AlMnO@NB-CDs structure, the manganese-doped mesoporous alumina microspheres grafted on the surface of the modified graphene oxide pull the graphene oxide to cause it to unfold into a two-dimensional plane, thereby reducing its curling, and the carbon dots are introduced The rich functional groups can improve its dispersibility; in the process of blending with styrene-butadiene rubber, the bridging effect of 2-acrylamide-2-methylpropane sulfonic acid can promote the uniform dispersion of the functional microspheres of GO-AlMnO@NB-CDs structure in the styrene-butadiene rubber system, and maintain good stability. Through the ionic bond cross-linking and covalent cross-linking structure in the system, the modified graphene oxide is dispersed in the rubber system in the form of sheets to form a network structure, which can overcome the natural defects of graphene oxide and enhance the strengthening effect of graphene oxide on strength and wear resistance. The construction of the functional microspheres of the GO-AlMnO@NB-CDs structure can also achieve the uniform dispersion of nitrogen-boron co-doped carbon dots and manganese-doped mesoporous alumina microspheres in the rubber system. Finally, after the multi-effect modified styrene-butadiene rubber is added to the raw material system of the sealing gasket, the functional microspheres can be evenly dispersed in the entire sealing gasket system, so that the effects of each functional component in the functional microspheres can be fully exerted.

[0095] 2. Self-healing epoxy resin

[0096] In the present invention, an epoxy resin with a disulfide bond is used, diethylenetriamine is used as a curing agent, and polypropylene glycol diglycidyl ether is added to introduce a flexible segment, thereby preparing a self-healing modified epoxy resin that can achieve room temperature self-healing function through disulfide bond translocation exchange. The introduction of the flexible segment can play a reinforcing and toughening effect. In addition, the epoxy resin can improve the strength, wear resistance, chemical resistance and durability of the rubber.

[0097] The addition of self-healing epoxy resin can provide excellent self-healing properties for the sealing gasket system and further improve its wear resistance and strength. The functional microspheres of GO-AlMnO@NB-CDs structure in the multi-effect modified styrene-butadiene rubber can also cooperate with the self-healing epoxy resin. The catalytic effect of manganese dioxide in the functional microspheres on the disulfide bond exchange reaction and the co-catalytic effect of carbon dot modification can enhance the self-healing properties provided by the self-healing epoxy resin.

[0098] In the sealing gasket system of the present invention, the disulfide bonds introduced in the self-repairing epoxy resin, the ionic bonds existing in the multi-effect modified styrene-butadiene rubber system and the dynamic BO bonds can provide it with self-repairing properties, thereby giving it a long-term anti-leakage function, which can significantly improve its sealing effect and extend its service life.

[0099] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.

[0100] Sources of main reagents:

[0101] Styrene butadiene rubber, Qilu Petrochemical SBR1502, Shanghai Yiyong New Material Technology Co., Ltd.;

[0102] Graphene oxide (GO), single-layer flake graphene oxide powder, flake diameter: 1-5 μm, thickness: 0.8-1.2 nm; purchased from Nanjing Xianfeng Nanomaterials Technology Co., Ltd.

[0103] 2-Acrylamide-2-methylpropanesulfonic acid (AMPS), Shanghai Jizhi Biochemical Technology Co., Ltd.;

[0104] Bis(4-glycidoxy)diphenyl disulfide, namely 4,4'-bis(glycidoxy)diphenyl disulfide, Dalian Lianhua Chemical Co., Ltd.;

[0105] Polypropylene glycol diglycidyl ether Product No. M12292 Mw~640 Shanghai Myril Biochemical Technology Co., Ltd.;

[0106] Diethylenetriamine Nanjing Zunde Technology Co., Ltd.;

[0107] Nitrile rubber, JSRN220S, Shanghai Yiyong New Material Technology Co., Ltd.;

[0108] Antiaging agent NBC Jiangsu Runfeng Synthetic Technology Co., Ltd.;

[0109] Vulcanization accelerator TMTD, Shanghai Kaiyin Chemical Co., Ltd.;

[0110] White carbon black M-5, Jiangsu Runfeng Synthetic Technology Co., Ltd.;

[0111] Paraffin Jiangsu Runfeng Synthetic Technology Co., Ltd.;

[0112] Bisphenol A epoxy resin, brand Baling Petrochemical, E20 / CYD-011 / 601, Shanghai Yueyi Chemical Co., Ltd.;

[0113] The other raw materials not mentioned are conventional commercially available products.

[0114] Example 1

[0115] A sealing gasket with a long-term anti-leakage function, the raw materials for its preparation include the following components in parts by weight:

[0116]

[0117] The additives include, by weight: 1.5 parts of antioxidant, 1.5 parts of vulcanization accelerator, 3 parts of stearic acid and 6 parts of paraffin.

[0118] The preparation process of the sealing gasket comprises the following steps:

[0119] Step 1, internal mixing: add multi-effect modified styrene-butadiene rubber, self-repairing epoxy resin, nitrile rubber, white carbon black, zinc oxide, antioxidant and stearic acid into an internal mixer, mix at 80° C. for 7 minutes to obtain an internal mixing rubber compound;

[0120] Step 2, open refining: adding the internal mixing rubber, sulfur, paraffin wax and vulcanization accelerator into an open refining mill, mixing at 68°C for 10 minutes, discharging the material, placing it in an injection molding machine for sheeting, and obtaining a raw rubber gasket;

[0121] Step 3, vulcanization: vulcanize the raw rubber gasket in a vulcanizer at 175°C for 20 minutes and a vulcanization pressure of 15 MPa to obtain a sealing gasket.

[0122] In this embodiment, the multi-effect modified styrene-butadiene rubber is prepared by the following method:

[0123] S1. Treating graphene oxide with acid to obtain modified graphene oxide:

[0124] 5 g of monolayer flaky graphene oxide powder was added to a mixed acid solution consisting of 50 mL of 60% nitric acid and 25 mL of 95% sulfuric acid, stirred and refluxed at 70° C. for 4 h, filtered, and the solid product was washed with deionized water until neutral, and vacuum dried at 90° C. for 10 h to obtain modified graphene oxide;

[0125] S2. In-situ grafting of iron and aluminum oxides onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite:

[0126] S2-1, taking 3.5 g of modified graphene oxide and adding it into 50 mL of ethanol, and ultrasonically dispersing it for 30 min to obtain a modified graphene oxide dispersion;

[0127] S2-2, add 4 g of hexadecyltrimethylammonium bromide to 100 mL of ethanol, then add 5 mL of 10% hydrochloric acid, 2 mL of 10% nitric acid, 7.14 g of aluminum isopropoxide, 0.63 g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 40° C. for 6 h; adjust the pH value to 7 with sodium hydroxide; let stand at room temperature for 2 h, then dry at 100° C. for 12 h, and finally calcine at 500° C. in an air atmosphere for 4 h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite;

[0128] S3. Modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres:

[0129] S3-1, adding 2 g of mesoporous microsphere-graphene oxide composite into 150 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 30 min;

[0130] S3-2, add 1.64g citric acid, 1.2g urea, and 0.75g 4-hydroxyphenylboric acid to the mixture obtained in step S3-1, ultrasonically disperse for 45min, then transfer to a polytetrafluoroethylene-lined reactor, react at 180°C for 6h, cool to room temperature after the reaction, filter, wash the solid product with deionized water, and vacuum dry at 60°C for 8h to obtain functional microspheres;

[0131] S4. Add 8 g of functional microspheres, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of dicumyl peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

[0132] In this embodiment, the self-healing epoxy resin is prepared by the following method:

[0133] 12 g of bis(4-glycidoxy)diphenyl disulfide, 2.4 g of polypropylene glycol diglycidyl ether, and 5.8 g of diethylenetriamine were added to 25 g of ethanol, and the reaction was stirred at 80°C for 30 min. The resulting product was placed in a vacuum oven, degassed at 60°C for 20 min, then kept at 120°C for 2 h, and cooled to room temperature to obtain a self-healing epoxy resin.

[0134] Example 2

[0135] A sealing gasket with a long-term anti-leakage function, the raw materials for its preparation include the following components in parts by weight:

[0136] 100 parts of multi-effect modified styrene-butadiene rubber;

[0137] 25 parts of self-healing epoxy resin;

[0138]

[0139] The additives include, by weight: 1.5 parts of antioxidant, 1.5 parts of vulcanization accelerator, 3 parts of stearic acid and 6 parts of paraffin.

[0140] The preparation process of the sealing gasket comprises the following steps:

[0141] Step 1, internal mixing: add multi-effect modified styrene-butadiene rubber, self-repairing epoxy resin, nitrile rubber, white carbon black, zinc oxide, antioxidant and stearic acid into an internal mixer, mix at 80° C. for 7 minutes to obtain an internal mixing rubber compound;

[0142] Step 2, open refining: adding the internal mixing rubber, sulfur, paraffin wax and vulcanization accelerator into an open refining mill, mixing at 68°C for 10 minutes, discharging the material, placing it in an injection molding machine for sheeting, and obtaining a raw rubber gasket;

[0143] Step 3, vulcanization: vulcanize the raw rubber gasket in a vulcanizer at 175°C for 20 minutes and a vulcanization pressure of 15 MPa to obtain a sealing gasket.

[0144] In this embodiment, the multi-effect modified styrene-butadiene rubber is prepared by the following method:

[0145] S1. Treating graphene oxide with acid to obtain modified graphene oxide:

[0146] 5 g of monolayer flaky graphene oxide powder was added to a mixed acid solution consisting of 50 mL of 60% nitric acid and 25 mL of 95% sulfuric acid, stirred and refluxed at 70° C. for 4 h, filtered, and the solid product was washed with deionized water until neutral, and vacuum dried at 90° C. for 10 h to obtain modified graphene oxide;

[0147] S2. In-situ grafting of iron and aluminum oxides onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite:

[0148] S2-1, taking 3.5 g of modified graphene oxide and adding it into 50 mL of ethanol, and ultrasonically dispersing it for 30 min to obtain a modified graphene oxide dispersion;

[0149] S2-2, add 4 g of hexadecyltrimethylammonium bromide to 100 mL of ethanol, then add 5 mL of 10% hydrochloric acid, 2 mL of 10% nitric acid, 7.14 g of aluminum isopropoxide, 0.63 g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 40° C. for 6 h; adjust the pH value to 7 with sodium hydroxide; let stand at room temperature for 2 h, then dry at 100° C. for 12 h, and finally calcine at 500° C. in an air atmosphere for 4 h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite;

[0150] S3. Modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres:

[0151] S3-1, adding 2 g of mesoporous microsphere-graphene oxide composite into 150 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 30 min;

[0152] S3-2, add 1.64g citric acid, 1.2g urea, and 0.75g 4-hydroxyphenylboric acid to the mixture obtained in step 3-1, ultrasonically disperse for 45min, then transfer to a polytetrafluoroethylene-lined reactor, react at 180°C for 6h, cool to room temperature after the reaction, filter, wash the solid product with deionized water, and vacuum dry at 60°C for 8h to obtain functional microspheres;

[0153] S4. Add 8 g of functional microspheres, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of dicumyl peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

[0154] In this embodiment, the self-healing epoxy resin is prepared by the following method:

[0155] 12 g of bis(4-glycidoxy)diphenyl disulfide, 2.4 g of polypropylene glycol diglycidyl ether, and 5.8 g of diethylenetriamine were added to 25 g of ethanol, and the reaction was stirred at 80°C for 30 min. The resulting product was placed in a vacuum oven, degassed at 60°C for 20 min, then kept at 120°C for 2 h, and cooled to room temperature to obtain a self-healing epoxy resin.

[0156] Example 3

[0157] A sealing gasket with a long-term anti-leakage function, the raw materials for its preparation include the following components in parts by weight:

[0158]

[0159] The additives include, by weight: 1.5 parts of antioxidant, 1.5 parts of vulcanization accelerator, 3 parts of stearic acid and 6 parts of paraffin.

[0160] The preparation process of the sealing gasket comprises the following steps:

[0161] Step 1, internal mixing: add multi-effect modified styrene-butadiene rubber, self-repairing epoxy resin, nitrile rubber, white carbon black, zinc oxide, antioxidant and stearic acid into an internal mixer, mix at 80° C. for 7 minutes to obtain an internal mixing rubber compound;

[0162] Step 2, open refining: adding the internal mixing rubber, sulfur, paraffin wax and vulcanization accelerator into an open refining mill, mixing at 68°C for 10 minutes, discharging the material, placing it in an injection molding machine for sheeting, and obtaining a raw rubber gasket;

[0163] Step 3, vulcanization: vulcanize the raw rubber gasket in a vulcanizer at 175°C for 20 minutes and a vulcanization pressure of 15 MPa to obtain a sealing gasket.

[0164] In this embodiment, the multi-effect modified styrene-butadiene rubber is prepared by the following method:

[0165] S1. Treating graphene oxide with acid to obtain modified graphene oxide:

[0166] 5 g of monolayer flaky graphene oxide powder was added to a mixed acid solution consisting of 50 mL of 60% nitric acid and 25 mL of 95% sulfuric acid, stirred and refluxed at 70° C. for 4 h, filtered, and the solid product was washed with deionized water until neutral, and vacuum dried at 90° C. for 10 h to obtain modified graphene oxide;

[0167] S2. In-situ grafting of iron and aluminum oxides onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite:

[0168] S2-1, taking 3.8 g of modified graphene oxide and adding it into 50 mL of ethanol, and ultrasonically dispersing it for 30 min to obtain a modified graphene oxide dispersion;

[0169] S2-2, add 4 g of hexadecyltrimethylammonium bromide to 100 mL of ethanol, then add 5 mL of 10% hydrochloric acid, 2 mL of 10% nitric acid, 7.14 g of aluminum isopropoxide, 0.63 g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 40° C. for 6 h; adjust the pH value to 7 with sodium hydroxide; let stand at room temperature for 2 h, then dry at 100° C. for 12 h, and finally calcine at 500° C. in an air atmosphere for 4 h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite;

[0170] S3. Modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres:

[0171] S3-1, adding 2.5 g of mesoporous microsphere-graphene oxide composite into 150 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 30 min;

[0172] S3-2, add 1.64g citric acid, 1.2g urea, and 0.75g 4-hydroxyphenylboric acid to the mixture obtained in step 3-1, ultrasonically disperse for 45min, then transfer to a polytetrafluoroethylene-lined reactor, react at 180°C for 6h, cool to room temperature after the reaction, filter, wash the solid product with deionized water, and vacuum dry at 60°C for 8h to obtain functional microspheres;

[0173] S4. Add 7.5 g of functional microspheres, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of diisopropylbenzene peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

[0174] In this embodiment, the self-healing epoxy resin is prepared by the following method:

[0175] 12 g of bis(4-glycidoxy)diphenyl disulfide, 2 g of polypropylene glycol diglycidyl ether, and 5.5 g of diethylenetriamine were added to 25 g of ethanol, and the reaction was stirred at 80°C for 30 min. The resulting product was placed in a vacuum oven, degassed at 60°C for 20 min, then kept at 120°C for 2 h, and cooled to room temperature to obtain a self-healing epoxy resin.

[0176] Comparative Example 1

[0177] This example is basically the same as Example 1, except that styrene-butadiene rubber is used instead of the multi-effect modified styrene-butadiene rubber in Example 1.

[0178] Comparative Example 2

[0179] This example is basically the same as Example 1, with the only difference being that bisphenol A epoxy resin is used instead of the self-healing epoxy resin in Example 1.

[0180] Comparative Example 3

[0181] This example is basically the same as Example 1, except that the multi-effect modified styrene-butadiene rubber in this example is prepared by the following method:

[0182] S1. Preparation of mesoporous microspheres:

[0183] 4 g of hexadecyltrimethylammonium bromide was added to 100 mL of ethanol, and then 5 mL of 10% hydrochloric acid, 2 mL of 10% nitric acid, 7.14 g of aluminum isopropoxide, and 0.63 g of manganese dichloride were added, and the mixture was stirred at 40°C for 6 h in a sealed state; the pH value was adjusted to 7 with sodium hydroxide; the mixture was allowed to stand at room temperature for 2 h, and then dried at 100°C for 12 h, and finally calcined at 500°C in an air atmosphere for 4 h, cooled to room temperature, and ground to obtain mesoporous microspheres;

[0184] S2. Modify the mesoporous microspheres with boron-nitrogen-doped carbon dots to obtain functional microspheres:

[0185] S2-1, add 2 g of mesoporous microspheres into 150 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically disperse for 30 min;

[0186] S2-2, add 1.64 g of citric acid, 1.2 g of urea, and 0.75 g of 4-hydroxyphenylboric acid to the mixture obtained in step S2-1, ultrasonically disperse for 45 min, then transfer to a polytetrafluoroethylene-lined reactor, react at 180° C. for 6 h, cool to room temperature after the reaction, filter, wash the solid product with deionized water, and vacuum dry at 60° C. for 8 h to obtain functional microspheres;

[0187] S3. Add 8 g of functional microspheres, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of dicumyl peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

[0188] Comparative Example 4

[0189] This example is basically the same as Example 1, except that the multi-effect modified styrene-butadiene rubber in this example is prepared by the following method:

[0190] S1, treating graphene oxide with acid to obtain modified graphene oxide; the same as in Example 1;

[0191] S2, in situ grafting iron aluminum oxide onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite; the same as Example 1;

[0192] S3. Add 8 g of mesoporous microsphere-graphene oxide composite, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of diisopropylbenzene peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

[0193] Comparative Example 5

[0194] This example is basically the same as Example 1, except that the multi-effect modified styrene-butadiene rubber in this example is prepared by the following method:

[0195] S1, treating graphene oxide with acid to obtain modified graphene oxide; the same as Example 1;

[0196] S2. Add 2 g of modified graphene oxide, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of diisopropylbenzene peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

[0197] Comparative Example 6

[0198] This example is basically the same as Example 1, except that the multi-effect modified styrene butadiene rubber in this example is prepared by the following method: 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of diisopropylbenzene peroxide, and 100 g of styrene butadiene rubber are added to an internal mixer and mixed at 75° C. for 25 min to obtain a multi-effect modified styrene butadiene rubber.

[0199] Performance Characterization

[0200] 1. Taking Example 1 as an example, the multi-effect modified styrene-butadiene rubber prepared therein was subjected to XRD detection and compared with the XRD pattern of AMPS. The detection results are as follows: Figure 1 As shown, it can be seen from the XRD spectrum that the characteristic peaks of AMPS in the spectrum of the multi-effect modified styrene butadiene rubber have basically disappeared, indicating that AMPS has been basically completely reacted. Wherein, AlMnO represents manganese-doped mesoporous alumina microspheres, and its preparation method is basically the same as step S2 of Example 1, except that modified graphene oxide is not added; the spectrum of AlMnO is used as a reference.

[0201] 2. The infrared absorption spectrum of the functional microspheres prepared in Example 1 was obtained by referring to Figure 2 The characterization results show that the functional microspheres have abundant functional groups, such as -CH 3 、-CH 2 -, -NH, COC, -OH, -C=O, BC, etc. These functional groups mainly come from carbon dots modified on mesoporous microspheres and modified graphene oxide (-NH and BC mainly come from carbon dots).

[0202] Performance Testing

[0203] Preparation of test materials:

[0204] According to the formulas of the embodiment and the comparative example, the raw materials for preparing the sealing gasket were prepared into test materials for subsequent testing. The preparation method was similar to that of the sealing gasket, as follows:

[0205] Step 1, internal mixing: add multi-effect modified styrene-butadiene rubber, self-repairing epoxy resin, nitrile rubber, white carbon black, zinc oxide, antioxidant and stearic acid into an internal mixer, mix at 80° C. for 7 minutes to obtain an internal mixing rubber compound;

[0206] Step 2, open refining: adding the internal mixing rubber, sulfur and paraffin into an open refining mill, mixing at 68°C for 10 minutes, discharging and forming to obtain a raw rubber material;

[0207] Step 3: Vulcanization: vulcanize the raw rubber material in a vulcanizer at 175°C for 20 minutes and a vulcanization pressure of 15 MPa to obtain a test material.

[0208] 3. Tensile strength test

[0209] Referring to the standard "GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", the test materials corresponding to the embodiments and comparative examples were first made into dumbbell-shaped specimens, and then the tensile strength was measured using a tensile testing machine.

[0210] The test results are shown in Table 1 and Figure 3 As shown:

[0211] Table 1

[0212]

[0213] From the test results in Table 1, it can be seen that the test materials of Examples 1-3 have higher tensile strengths. Comparative Example 1 lacks the reinforcing and modifying functions of functional microspheres and 2-acrylamide-2-methylpropanesulfonic acid, and the tensile strength decreases significantly; Comparative Example 6 lacks the reinforcing and modifying functions of functional microspheres, and the tensile strength also decreases significantly. Comparison of the results of Comparative Example 3 with those of Example 1 shows that the introduction of modified graphene oxide in the system can improve the tensile strength; in Comparative Example 5, the tensile strength decreases due to the inability to overcome the defects of graphene oxide such as easy agglomeration.

[0214] 4. Self-healing performance test

[0215] According to the standard "GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", the test materials corresponding to the embodiments and comparative examples were prepared into test strips, and then completely cut in the middle, and then completely aligned, and self-repaired under corresponding conditions. Each group was tested 6 times, and the average value of the self-repair rate was calculated. The calculation formula of the self-repair rate η is:

[0216] σ 0 represents the original tensile strength (MPa), σ h It indicates the tensile strength after repair (MPa).

[0217] 4-1. Test the self-repair rate at 25℃ and 2h treatment

[0218] The test results are shown in Table 2 and Figure 4 As shown:

[0219] Table 2

[0220]

[0221]

[0222] It can be seen from the test results that the test material of Example 1 has a higher room temperature self-healing ability. In Example 1, the dynamic BO bond and the catalytic effect of manganese dioxide on the disulfide exchange reaction are lacking, so the self-healing performance is reduced; in Example 2, no epoxy resin with disulfide bonds is added, and the self-healing performance decreases the most. It still retains some self-healing ability due to the presence of dynamic BO bonds in the multi-effect modified styrene-butadiene rubber; the self-healing performance of Example 4 decreases, indicating that the nitrogen-boron co-doped carbon dots in the functional microsphere system have an enhancing effect on the catalytic effect of manganese dioxide in the disulfide exchange reaction; the self-healing performance of Example 5 decreases, which is attributed to the lack of ionic bonds introduced by manganese-doped mesoporous alumina microspheres and BO bonds introduced by nitrogen-boron co-doped carbon dots; the self-healing performance of Example 5 decreases, which is attributed to the lack of auxiliary enhancement of the functional microspheres on the self-healing performance.

[0223] 4-2. Test the self-repair rate of 2h treatment at different treatment temperatures

[0224] The test results are shown in Table 3 and Figure 5 As shown:

[0225] Table 3

[0226]

[0227] It can be seen from the test results that as the temperature increases, the self-repair rate shows a trend of gradually increasing, indicating that the sealing gasket material of the present invention has good self-repair ability at room temperature and can exert better self-repair effect in a high temperature environment of 60-120°C.

[0228] 4-3. Self-repair rate at different treatment times at 80°C

[0229] The test results are shown in Table 4 and Figure 6 As shown:

[0230] Table 4

[0231]

[0232]

[0233] From the test results, it can be seen that as the repair time increases, the self-repair rate tends to gradually increase.

[0234] 5. Compression and resilience test: The sealing gaskets prepared in the examples and comparative examples were tested in accordance with GB / T20671 "Non-metallic gasket material classification system and test methods Gasket material compression rate and resilience rate test methods". The test results are shown in Table 5 below.

[0235] Table 5

[0236]

[0237] 6. Sealing test: The sealing gaskets prepared in the embodiments and comparative examples were tested in accordance with GB / T20671 “Classification system and test methods for non-metallic gasket materials - Sealing test methods for gasket materials”; the test results are shown in Table 6 below.

[0238] Table 6

[0239]

[0240] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A sealing gasket with long-term anti-leakage function, It is characterized in that The raw materials for its preparation include the following components by weight: 100 parts of multi-effect modified styrene-butadiene rubber; 13-56 parts of self-healing epoxy resin; 7.5-28 parts of nitrile rubber; 5-22 parts of white carbon black; Zinc oxide 0.5-1.5 parts; Sulfur 0.4-1.2 parts; 5.5-25 parts of additives; The multi-effect modified styrene-butadiene rubber is prepared by the following method: S1, treating graphene oxide with acid to obtain modified graphene oxide; S2, in situ grafting manganese aluminum oxide onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite; S3, modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres; S4, mixing the functional microspheres, 2-acrylamide-2-methylpropane sulfonic acid and styrene-butadiene rubber to obtain the multi-effect modified styrene-butadiene rubber; The self-healing epoxy resin is prepared by the following method: Add 6-24g of bis(4-glycidoxy)diphenyl disulfide, 1.2-4.8g of polypropylene glycol diglycidyl ether, and 2.9-11.6g of diethylenetriamine to 12-50g of ethanol, stir and react at 65-90°C for 15-60min, place the obtained product in a vacuum oven, degas at 50-70°C for 10-40min, then keep warm at 100-130°C for 1-4h, and cool to room temperature to obtain a self-healing epoxy resin.

2. The sealing gasket with long-term anti-leakage function according to claim 1, It is characterized in that The auxiliary agent comprises, by weight: 1 to 5 parts of antioxidant, 1.5 to 5 parts of vulcanization accelerator, 1 to 5 parts of stearic acid, and 2 to 10 parts of paraffin.

3. The sealing gasket with long-term anti-leakage function according to claim 1, It is characterized in that Step S2 is specifically as follows: S2-1, taking 1.75-7.0 g of modified graphene oxide and adding it into 25-100 mL of ethanol, and ultrasonically dispersing it for 15-60 min to obtain a modified graphene oxide dispersion; S2-2, add 2-8g of hexadecyltrimethylammonium bromide to 50-200mL of ethanol, then add 2.5-10mL of hydrochloric acid with a mass concentration of 5-20%, 1-5mL of nitric acid with a mass concentration of 5-20%, 3.57-14.28g of aluminum isopropoxide, 0.315-1.26g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 35-45°C for 3-12h, and adjust the pH value to 7-8 with sodium hydroxide; let stand at room temperature for 1-4h, and then dry at 90-100°C for 6-24h, and finally calcine at 400-600°C in an air atmosphere for 1.5-6h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite.

4. The sealing gasket with long-term anti-leakage function according to claim 1, It is characterized in that Step S3 is specifically as follows: S3-1, adding 1-4 g of the mesoporous microsphere-graphene oxide composite into 100-300 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 15-60 min; S3-2. Add 0.82-3.28 g of citric acid, 0.6-2.4 g of urea, and 0.375-1.5 g of 4-hydroxyphenylboric acid to the mixture obtained in step S3-1, and ultrasonically disperse for 30-60 min. Then transfer to a polytetrafluoroethylene-lined reactor, react at 170-190° C. for 4-12 h. After the reaction is completed, cool to room temperature, filter, wash the solid product with deionized water, and vacuum dry at 50-70° C. for 6-12 h to obtain functional microspheres.

5. The sealing gasket with long-term anti-leakage function according to claim 1, It is characterized in that Step S4 is specifically as follows: 4-16g of functional microspheres, 3.25-13.0g of 2-acrylamide-2-methylpropanesulfonic acid, 0.4-1.5g of dicumyl peroxide and 100g of styrene-butadiene rubber are added into an internal mixer and mixed at 70-80°C for 15-40min to obtain multi-effect modified styrene-butadiene rubber.

6. The sealing gasket with long-term anti-leakage function according to claim 1, It is characterized in that The multi-effect modified styrene-butadiene rubber is prepared by the following method: S1. Treating graphene oxide with acid to obtain modified graphene oxide: 5 g of graphene oxide was added to a mixed acid solution consisting of 50 mL of 60% nitric acid and 25 mL of 95% sulfuric acid, stirred and refluxed at 70° C. for 4 h, filtered, and the solid product was washed with deionized water until neutral, and vacuum dried at 90° C. for 10 h to obtain modified graphene oxide; S2. In-situ grafting of manganese aluminum oxide onto the modified graphene oxide to obtain a mesoporous microsphere-graphene oxide composite: S2-1, taking 3.5 g of modified graphene oxide and adding it into 50 mL of ethanol, and ultrasonically dispersing it for 30 min to obtain a modified graphene oxide dispersion; S2-2, add 4 g of hexadecyltrimethylammonium bromide to 100 mL of ethanol, then add 5 mL of 10% hydrochloric acid, 2 mL of 10% nitric acid, 7.14 g of aluminum isopropoxide, 0.63 g of manganese dichloride, and the modified graphene oxide dispersion obtained in step S2-1, and stir in a sealed state at 40° C. for 6 h; adjust the pH value to 7 with sodium hydroxide; let stand at room temperature for 2 h, then dry at 100° C. for 12 h, and finally calcine at 500° C. in an air atmosphere for 4 h, cool to room temperature, and grind to obtain a mesoporous microsphere-graphene oxide composite; S3. Modifying the mesoporous microsphere-graphene oxide composite with boron-nitrogen doped carbon dots to obtain functional microspheres: S3-1, adding 2 g of mesoporous microsphere-graphene oxide composite into 150 mL of a mixed solution consisting of deionized water and ethanol in a volume ratio of 1:1, and ultrasonically dispersing for 30 min; S3-2, add 1.64g citric acid, 1.2g urea, and 0.75g 4-hydroxyphenylboric acid to the mixture obtained in step S3-1, ultrasonically disperse for 45min, then transfer to a polytetrafluoroethylene-lined reactor, react at 180°C for 6h, cool to room temperature after the reaction, filter, wash the solid product with deionized water, and vacuum dry at 60°C for 8h to obtain functional microspheres; S4. Add 8 g of functional microspheres, 6.5 g of 2-acrylamide-2-methylpropane sulfonic acid, 1 g of dicumyl peroxide, and 100 g of styrene-butadiene rubber into an internal mixer, and mix at 75° C. for 25 min to obtain a multi-effect modified styrene-butadiene rubber.

7. The sealing gasket with long-term anti-leakage function according to claim 1, It is characterized in that The self-healing epoxy resin is prepared by the following method: 12 g of bis(4-glycidoxy)diphenyl disulfide, 2.4 g of polypropylene glycol diglycidyl ether, and 5.8 g of diethylenetriamine were added to 25 g of ethanol, and the mixture was stirred and reacted at 80°C for 30 min. The obtained product was placed in a vacuum oven, degassed at 60°C for 20 min, then kept at 120°C for 2 h, and cooled to room temperature to obtain a self-healing epoxy resin.

8. A process for preparing a sealing gasket with a long-term anti-leakage function as claimed in any one of claims 2 to 7, It is characterized in that The following steps are involved: Step 1, internal mixing: add multi-effect modified styrene-butadiene rubber, self-repairing epoxy resin, nitrile rubber, white carbon black, zinc oxide, antioxidant, and stearic acid into an internal mixer, mix at 70-90° C. for 3-15 minutes to obtain an internal mixing rubber compound; Step 2, open refining: add the internal mixing rubber, sulfur, paraffin wax and vulcanization accelerator into an open refining mill, mix at 60-75°C for 5-20 minutes, discharge the material, place it in an injection molding machine for sheeting, and obtain a raw rubber gasket; Step 3, vulcanization: vulcanize the raw rubber gasket in a vulcanizer at 155-185°C for 10-45min and a vulcanization pressure of 7-20MPa to obtain a sealing gasket.