Array nanospray needle manufacturing method based on press molding and array nanospray needle
The array micron spray needle convex mold is prepared by photolithography and wet etching, and the oxygen plasma-assisted pressing method is used to form nano-channels, which solves the problems of shrinking the inner diameter of the spray needle and high manufacturing cost in the existing technology, and achieves a simple, low-cost Low-cost array nano-jet needle manufacturing improves printing resolution.
Patent Information
- Application Number
- CN202410816626.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-24
AI Technical Summary
The existing technology has problems of high manufacturing cost and complex process steps in reducing the inner diameter of the spray needle to improve printing resolution, especially in nanostructure manufacturing.
An array nano-nozzle manufacturing method based on press molding is used to prepare an array micron nozzle convex mold through photolithography and wet etching. Combined with the soft elastic material characteristics of PDMS and the oxygen plasma-assisted pressing method, the array nozzle cover plate and The bonding of micron spray needles forms nanochannels.
The manufacturing of array nano-jet needles with simple process, low cost and short manufacturing cycle is realized, which improves the printing resolution and reduces the manufacturing cost.
Smart Images

Figure CN118372492B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of micro-electromechanical technology, and in particular to a method for manufacturing an array nano-spray needle based on press molding and an array nano-spray needle. Background Art
[0002] Electrohydraulic jet printing is an additive manufacturing method that does not require a photolithography mask and can deposit various functional materials directly on the required functional area. It can be used in the thin film transistor (TFT) manufacturing of large-format flexible liquid crystal displays, organic light-emitting diode (OLED) manufacturing, organic solar cell manufacturing, biochemical printing, 3D printing and printed electronics. Among them, electrohydraulic jet printing has a scale effect, and the size of the inner diameter of the needle is the main factor affecting the printing resolution. Therefore, how to further reduce the inner diameter of the needle and improve the printing resolution is a key issue that needs to be solved urgently.
[0003] At present, nanostructure manufacturing mostly adopts ion beam direct writing, electron beam exposure, laser direct writing and other methods, which can directly obtain nanoscale spray needles, but the above methods rely on expensive process equipment and have high manufacturing costs. By manufacturing silicon nano molds over a large area and replicating the nano mold patterns to manufacture nano spray needles, this method greatly reduces the manufacturing cost, but the process steps are complicated and the manufacturing cycle is long. Summary of the invention
[0004] The present invention overcomes the shortcomings of the prior art and provides a method for manufacturing an array nanospray needle based on press molding and an array nanospray needle with simple process, low cost and short manufacturing cycle.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for manufacturing an array nanospray needle based on pressing molding, comprising the following steps:
[0006] Step 1. Treat the array micro-needle and the array needle cover with oxygen plasma, and then proceed to step 2;
[0007] The method for preparing the array micro-spray needle comprises the following steps:
[0008] Step a.1. Obtaining an array micro-needle convex mold, wherein the array micro-needle convex mold is prepared by photolithography and wet etching;
[0009] Step a.2. Using the array micro-needle convex mold prepared in step a.1, prepare an unbonded array micro-needle by a casting method;
[0010] The preparation method of the array needle cover plate comprises:
[0011] Step b.1. Obtaining an array needle cover plate mold;
[0012] The preparation method of the array spray needle cover plate mold comprises:
[0013] The glass substrate is treated with oxygen plasma, a photoresist is spin-coated on the glass substrate, and a pre-baking is performed, and then a cover plate mask is used for ultraviolet exposure, and then a post-baking and development is performed to obtain an array needle cover plate mold;
[0014] Step b.2. Casting the PDMS mixed solution into the array needle cover plate mold obtained in step b.1 to make an array needle cover plate blank; demolding and shaping the array needle cover plate blank to obtain an array needle cover plate;
[0015] Step 2. Align the array micro-needle processed in step 1 with the array needle cover plate, and proceed to step 3;
[0016] Step 3. Press the array needle cover plate at the microchannel of the array micro needle to collapse the array needle cover plate and contact and bond with the bottom of the microchannel of the array micro needle, so that the array needle cover plate leaves nanochannels in the microchannel of the array micro needle, and obtain an array nano needle.
[0017] In a preferred embodiment of the present invention, in step a.1, the method of photolithography and wet etching of the array micro-needle convex mold comprises the following steps:
[0018] A silicon wafer with a silicon dioxide layer with a thickness of 100 nm was selected as the silicon wafer substrate.
[0019] Place the silicon wafer substrate in a drying tower with HMDS atmosphere and let it stand for 10 to 20 minutes.
[0020] Spin coat a layer of photoresist on the dried silicon wafer substrate, with a low speed of 500-800 rpm and a spin coating time of 6-10 s, and a high speed of 5000-7000 rpm and a spin coating time of 30-40 s;
[0021] Place the silicon wafer substrate with photoresist on a horizontal hot plate and bake for 20-30 minutes; then take it out and cool it to room temperature, then expose it to ultraviolet light through a needle mask, and the exposure time is 45-90 seconds;
[0022] After developing the exposed photoresist for 45-60 seconds, an array micron needle structure is obtained on the photoresist on the silicon wafer substrate, and the residual developer is removed in deionized water; finally, the film is placed on a hot plate at 60-90°C for 30-45 minutes to harden the film;
[0023] The silicon wafer substrate with the array micro-needle structure is placed in a hydrofluoric acid solution at a water bath temperature of 45-60° C. to etch the silicon dioxide layer on the silicon wafer substrate for 9-12 seconds, and the array micro-needle structure is transferred to the silicon dioxide layer of the silicon wafer substrate;
[0024] Then, the silicon wafer is placed in an acetone solution and soaked for 30 to 60 minutes to remove the photoresist and obtain an array micro-needle convex mold.
[0025] In a preferred embodiment of the present invention, in step a.2, the casting method of the unbonded array micro-needle comprises the following steps:
[0026] Step a.2.1. Place the array micro-spray needle convex mold in a drying tower in a trimethylsiloxane atmosphere for 10 to 20 minutes, then pour the PDMS mixed solution on the array micro-spray needle convex mold, and place it in a vacuum environment of 10Pa for 1 to 2 hours to remove bubbles in the PDMS mixed solution while ensuring that the PDMS mixed solution fills the array micro-spray needle convex mold;
[0027] Step a.2.2. Place the array micro-needle convex mold filled in step a.2.1 in a vacuum oven at 60~85℃ for curing for 2~4h; separate the cured needle profile blank from the array micro-needle convex mold, and remove excess waste on the needle profile blank to obtain an unbonded array micro-needle.
[0028] In a preferred embodiment of the present invention, the PDMS mixed solution is a mixed solution of PDMS and a curing agent in a volume ratio of 4:1 to 10:1.
[0029] In a preferred embodiment of the present invention, in step b.1, the glass substrate is subjected to oxygen plasma treatment at a treatment power of 45 to 80 W and a treatment time of 15 to 20 s;
[0030] The photoresist is spin-coated on the glass substrate at a low speed of 500-800 rpm and a spin-coating time of 6-10 s, and a high speed of 3000-5000 rpm and a spin-coating time of 30-40 s;
[0031] The pre-bake is to place the glass substrate coated with photoresist on a horizontal hot plate for step baking;
[0032] During the UV exposure process through the cover mask, the photoresist is first cooled to room temperature and then UV-exposed through the cover mask for 4 to 7 minutes;
[0033] In the post-baking development, the UV-exposed photoresist is placed on a hot plate and post-baked for 2 to 5 minutes, and developed for 60 to 90 seconds to obtain an array needle cover plate mold.
[0034] In a preferred embodiment of the present invention, in step b.2, the method for casting the array needle cover blank comprises:
[0035] The array needle cover plate mold is placed in a drying tower in a trimethylsiloxane atmosphere for 10 to 20 minutes, and then the PDMS mixed solution is poured on the array needle cover plate mold; and it is placed in a vacuum environment of 10Pa for 1 to 2 hours to remove excess bubbles in the PDMS mixed solution while ensuring that the PDMS mixed solution completely fills the array needle cover plate mold; and then it is placed in a vacuum oven at 60 to 85°C for 2 to 4 hours to obtain a cured array needle cover plate blank.
[0036] In a preferred embodiment of the present invention, the PDMS mixed solution is a mixed solution of PDMS and a curing agent in a volume ratio of 4:1 to 10:1.
[0037] In a preferred embodiment of the present invention, in step b.2, the demoulding and shaping method of the array needle cover plate blank comprises:
[0038] The solidified array needle cover plate blank is separated from the array needle cover plate mold and taken out; then the outer surface of the array needle cover plate blank is shaped to obtain the array needle cover plate contour; then, according to the required array needle cover plate shape, grooves are cut on the array needle cover plate contour to manufacture the needle liquid storage tank, and the array needle cover plate is obtained.
[0039] In a preferred embodiment of the present invention, the photoresist is AZ703, AZ5214E, AZ701, BP212, BN308, or SU-8 photoresist; and / or the silicon dioxide layer is replaced by an Al, Cr, Au, Ag, or Ni metal film layer.
[0040] In a preferred embodiment of the present invention, an array of nanospray needles is prepared by the above-mentioned manufacturing method of array of nanospray needles based on press molding.
[0041] The present invention solves the defects existing in the technical background, and the beneficial technical effects of the present invention are:
[0042] The invention discloses a method for manufacturing an array nano-spray needle based on press molding and an array nano-spray needle. The invention adopts photolithography and wet etching methods to prepare an array micro-spray needle convex mold, and replicates the graphic structure on the array micro-spray needle convex mold by casting to obtain an unbonded array micro-spray needle; and adopts photolithography and casting methods to manufacture a polymer array spray needle cover plate.
[0043] Taking advantage of the soft elastic material characteristics of PDMS, the oxygen plasma-assisted pressing method is used to cleverly collapse the PDMS array needle cover at the micron channel of the array micron needle and contact with the bottom of the micron channel of the PDMS array micron needle to form irreversible bonding, thereby leaving a nanochannel in each micron channel, thus obtaining a polymer array nanoneedle. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0045] Figure 1 It is a flow chart of preparing the array micro-spray needle convex mold in the preferred embodiment of the present invention;
[0046] Figure 2 is a manufacturing flow chart of an unbonded array micro-spray needle in a preferred embodiment of the present invention;
[0047] Figure 3 It is a manufacturing flow chart of the array spray needle cover plate mold in the preferred embodiment of the present invention;
[0048] Figure 4 is a manufacturing flow chart of an array needle cover plate in a preferred embodiment of the present invention;
[0049] Figure 5 2 is a schematic diagram of the structure of the micro-spray needle array and the spray needle array cover plate being pressed and bonded in a preferred embodiment of the present invention;
[0050] Figure 6 Schematic diagram of the structure of the array nanospray needle in the preferred embodiment of the present invention;
[0051] Figure 7 is a scanning electron microscope image of an array micro-spray needle structure in a preferred embodiment of the present invention;
[0052] Figure 8 is a scanning electron microscope cross-sectional view of the array nanospray needle nanochannel in a preferred embodiment of the present invention;
[0053] Fig. 9 is a scanning electron microscope image of a liquid reservoir and a micron channel in an unbonded array nanospray needle in a preferred embodiment of the present invention;
[0054] In the figure: 1. Silicon wafer; 2. Silicon dioxide layer; 3. AZ703 photoresist; 4. Spray needle mask; 5. Ultraviolet light; 6. PDMS; 7. Glass substrate; 8. SU-8 photoresist; 9. Cover mask. DETAILED DESCRIPTION
[0055] The present invention will now be further described in detail with reference to the accompanying drawings and embodiments. These drawings are simplified schematic diagrams that only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.
[0056] It should be noted that if there are directional indications (such as up, down, bottom, top, etc.) involved in the embodiments of the present invention, the directional indication is only used to explain the relative position relationship, movement, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly. The terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Unless otherwise clearly specified and defined, the terms "set", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. Embodiment 1
[0057] like Figure 1 As shown, a method for manufacturing an array nanospray needle based on press molding comprises the following steps:
[0058] Step 1. Treat the array micro-needle and the array needle cover with oxygen plasma, and then proceed to step 2;
[0059] Step 2. Align the array micro-needle processed in step 1 with the array needle cover plate, and proceed to step 3;
[0060] Step 3. Press the array needle cover plate at the microchannel of the array needle to collapse the array needle cover plate and contact and bond with the bottom of the microchannel of the array micro needle, so that the array needle cover plate leaves nanochannels in the microchannel of the array micro needle, and obtains an array nano needle (such as Figure 5 In a preferred embodiment, the array needle cover plate leaves nanochannels on both sides of the microchannels of the array micro needles.
[0061] Specifically, the method for preparing the array micro-spray needle includes the following steps:
[0062] Step a.1. Obtain an array micro-needle convex mold, wherein the array micro-needle convex mold is prepared by photolithography and wet etching. The preparation process of the array micro-needle convex mold is as follows: Figure 1 shown.
[0063] More specifically, in step a.1, the method of photolithography and wet etching of the array micro-needle convex mold includes the following steps:
[0064] a.1.1. Select a silicon wafer 1 with a silicon dioxide layer 2 with a thickness of 100nm as the silicon wafer substrate. First, place the silicon wafer substrate at a temperature of 100~150℃ and bake for 30min to remove moisture from the surface of the silicon wafer. Then place it in a drying tower with an HMDS (hexamethyldisilazane) atmosphere and let it stand for 10~20min, and then place it on a hot plate at 100~150℃ and bake for 5~10min. Spin coat a layer of photoresist on the dried silicon wafer substrate, with a low speed of 500~800rpm, a spin coating time of 6~10s, and a high speed of 5000~7000rpm, and a spin coating time of 30~40s. Furthermore, the photoresist uses AZ703, AZ5214E, AZ701, BP212, BN308, or SU-8 photoresist. In this embodiment, the photoresist used in this step is AZ703 photoresist 3. As Figure 1 As shown in 1a.
[0065] a.1.2. Place the silicon wafer substrate coated with photoresist on a horizontal hot plate and bake for 20-30 minutes; then take it out and cool it to room temperature, then expose it to ultraviolet light through a needle mask 4, and the exposure time is 45-90 seconds (such as Figure 1 1b in FIG). Furthermore, the exposure time should be controlled within 45 to 90 seconds. If the exposure time is too short and the exposure dose is insufficient, the photoresist in the exposed area cannot be completely dissolved in the developer during the development process, and an ideal pattern cannot be generated. If the exposure time is too long, the exposure size will be increased due to light diffraction, and the obtained photoresist pattern will be narrower than the mask pattern.
[0066] a.1.3. Developing to obtain array micro-needle structure (such as Figure 1 1c in FIG). The exposed photoresist is developed for 45 to 60 seconds to obtain an array micro-needle structure, and the residual developer is removed in deionized water; finally, the film is placed on a hot plate at 60 to 90° C. for 30 to 45 minutes.
[0067] a.1.4. Place the silicon wafer substrate with the array micro-spray needle structure in a hydrofluoric acid solution at a water bath temperature of 45-60°C to etch the silicon dioxide layer 2 on the silicon wafer substrate for 9-12 seconds, and transfer the array micro-spray needle structure to the silicon dioxide layer 2 of the silicon wafer substrate to obtain the array micro-spray needle structure (such as Figure 1 1d in Figure 1).
[0068] a.1.5. Soak the silicon wafer substrate in acetone solution for 30-60 minutes to remove the photoresist and obtain an array micro-needle convex mold (such as Figure 11e in FIG. 1). If the etching time of the silicon wafer in the acetone solution is too short, under-etching will occur, and the array micro-needle structure cannot be completely transferred to the silicon dioxide layer 2 substrate; if the etching time is too long, lateral etching will occur, resulting in a reduction in the width of the array micro-needle structure. However, it is not limited to this. In other embodiments, the silicon dioxide layer 2 can be replaced by an Al, Cr, Au, Ag, or Ni metal film layer.
[0069] Step a.2. Use the array micro-needle convex mold prepared in step a.1 to prepare an unbonded array micro-needle by casting. Figure 2 shown.
[0070] More specifically, in step a.2, the casting method of the unbonded array micro-needle includes the following steps:
[0071] Step a.2.1. Place the array micro-needle convex mold in a drying tower with trimethylsiloxane atmosphere for 10-20 min, and then pour the PDMS mixed solution on the array micro-needle convex mold (such as Figure 2 2a in FIG). The PDMS mixture is placed in a vacuum environment of 10 Pa for 1 to 2 hours to remove excess bubbles in the PDMS mixture and ensure that the PDMS mixture completely fills the array micro-needle convex mold. Furthermore, the PDMS mixture is a mixture of PDMS (polydimethylsiloxane) and a curing agent in a volume ratio of 4:1 to 10:1.
[0072] Step a.2.2. Place the array micro-needle convex mold filled in step b1 in a vacuum oven at 60-85°C for 2-4 hours; separate the solidified needle profile blank from the array micro-needle convex mold, and remove the excess waste on the needle profile blank to obtain an unbonded array micro-needle (such as Figure 2 2b in Figure 1).
[0073] Specifically, the method for preparing the array needle cover plate includes:
[0074] Step b.1. Obtain an array needle cover plate mold.
[0075] More specifically, Figure 3 As shown, the preparation method of the array spray needle cover plate mold includes:
[0076] The glass substrate is treated with oxygen plasma, the photoresist is spin-coated on the glass substrate 7, and pre-baked, and then ultraviolet exposure is performed through the cover mask 9, and then post-baked and developed (such as Figure 3 3c in the figure); obtaining an array needle cover plate mold (as shown in Figure 33d in FIG). Pre-baking is only used to remove most of the solvent in the photoresist, not curing, and UV exposure can cure the photoresist. Further, the photoresist uses AZ703, AZ5214E, AZ701, BP212, BN308, or SU-8 photoresist. In this embodiment, the photoresist used in this step is SU-8 photoresist 8. Among them, the processing power of the glass substrate for oxygen plasma treatment is 45~80W, and the processing time is 15~20s; the low speed rotation speed of the photoresist spin-coated on the glass substrate 7 is 500~800rpm, and the spin-coating time is 6~10s; the high speed rotation speed is 3000~5000rpm, and the spin-coating time is 30~40s; the pre-baking is to place the glass substrate 7 coated with photoresist on a horizontal hot plate for step baking; in the process of ultraviolet exposure through the cover mask 9, the photoresist is first cooled to room temperature and then ultraviolet exposure is performed through the cover mask, and the exposure time is 4~7min; in the post-baking and developing process, the photoresist after ultraviolet exposure is placed on a hot plate and post-baked for 2~5min, and developed for 60~90s to obtain an array nozzle cover mold.
[0077] Step b.2. Figure 4 As shown, the PDMS mixed solution is poured into the array needle cover plate mold obtained in step b.1 to cast the array needle cover plate blank; the array needle cover plate blank is demoulded and shaped to obtain the array needle cover plate.
[0078] More specifically, in step b.2, the array needle cover plate blank casting method includes: placing the array needle cover plate mold in a drying tower in a trimethylsiloxane atmosphere for 10 to 20 minutes, then pouring the PDMS mixed solution on the array needle cover plate mold; and placing it in a vacuum environment of 10Pa for 1 to 2 hours to remove excess bubbles in the PDMS mixed solution while ensuring that the PDMS mixed solution completely fills the array needle cover plate mold (such as Figure 4 4e in FIG); and then placed in a vacuum oven at 60-85°C for curing for 2-4 hours to obtain a cured array needle cover plate blank. Further, the PDMS mixed solution uses a PDMS and curing agent mixed solution with a volume ratio of 4:1-10:1.
[0079] In step b.2, the demoulding and shaping method of the array needle cover plate blank includes: separating and removing the solidified array needle cover plate blank from the array needle cover plate mold to achieve demoulding (such as Figure 4 4f in the figure); then, the outer surface of the array needle cover plate blank is modified to obtain the array needle cover plate profile; and then, according to the required array needle cover plate shape, a groove is cut on the array needle cover plate profile to manufacture a needle reservoir to obtain the array needle cover plate (as shown in FIG. Figure 4 4j in the figure). The needle reservoir is formed by punching holes and grooves on the outline of the array needle cover plate by a punching machine. Embodiment 2
[0080] An array nanospray needle is prepared by the array nanospray needle manufacturing method based on pressing molding described in Example 1. Utilizing the soft elastic material characteristics of PDMS, an oxygen plasma-assisted pressing method is used to cleverly cause the PDMS array spray needle cover plate at the micro-channel of the array micro-spray needle to collapse and contact with the bottom of the micro-channel of the PDMS array micro-spray needle to form an irreversible bond, thereby leaving a nano-channel in each micro-channel, and obtaining a polymer array nanospray needle. Furthermore, in a preferred embodiment, due to the pressing method, the PDMS array spray needle cover plate at the micro-channel of the array micro-spray needle is partially collapsed and embedded in the micro-channel of the PDMS array micro-spray needle, and contacts with the bottom of the micro-channel of the array micro-spray needle to form an irreversible bond (such as Figure 6 As shown, the array needle cover plate is bonded to the array micro needle, the collapsed portion of the array needle cover plate is embedded in the micro channel of the array micro needle, and the array needle cover plate is located above the array micro needle); and two nano channels are left on both sides of each micro channel, that is, a polymer array nano needle is obtained. In a preferred embodiment, the collapsed portion of the array needle cover plate is embedded in the micro channel of the array micro needle, and contacts with the bottom of the micro channel of the array micro needle to form an irreversible bond, leaving two 100 nm nano channels on both sides of each micro channel.
[0081] Working principle:
[0082] The present invention firstly manufactures the needle micro-channel by photolithography technology, then ingeniously adopts the pressing method with the assistance of oxygen plasma treatment to obtain the needle array nano-channel, and finally obtains the polymer array nano-needle. The present invention first manufactures the needle micro-channel, then uses the oxygen plasma assisted pressing method to obtain the needle nano-channel, and obtains the array nano-needle in two steps, with simple process steps, high efficiency and low cost.
[0083] The invention adopts photolithography and wet etching method to prepare array micron spray needle convex mold, replicates the graphic structure on the array micron spray needle convex mold by casting method to obtain unbonded array micron spray needle; adopts photolithography and casting method to manufacture polymer array spray needle cover plate.
[0084] The above specific implementation methods are specific support for the scheme ideas proposed in the present invention, and cannot be used to limit the protection scope of the present invention. Any equivalent changes or equivalent modifications made on the basis of this technical scheme in accordance with the technical ideas proposed in the present invention still fall within the scope of protection of the technical scheme of the present invention.
Claims
1. A method for manufacturing an array nanospray needle based on pressing molding, characterized in that: The following steps are involved: Step 1. Treat the array micro-needle and the array needle cover with oxygen plasma, and then proceed to step 2; The method for preparing the array micro-spray needle comprises the following steps: Step a.
1. Obtaining an array micro-needle convex mold, wherein the array micro-needle convex mold is prepared by photolithography and wet etching; In step a.1, the method of photolithography and wet etching of the array micro-needle convex mold comprises the following steps: A silicon wafer with a silicon dioxide layer with a thickness of 100 nm was selected as the silicon wafer substrate. Place the silicon wafer substrate in a drying tower with HMDS atmosphere and let it stand for 10 to 20 minutes. Spin coat a layer of photoresist on the dried silicon wafer substrate, with a low speed of 500-800 rpm and a spin coating time of 6-10 s, and a high speed of 5000-7000 rpm and a spin coating time of 30-40 s; Place the silicon wafer substrate with photoresist on a horizontal hot plate and bake for 20-30 minutes; then take it out and cool it to room temperature, then expose it to ultraviolet light through a needle mask, and the exposure time is 45-90 seconds; After developing the exposed photoresist for 45-60 seconds, an array micron needle structure is obtained on the photoresist on the silicon wafer substrate, and the residual developer is removed in deionized water; finally, the film is placed on a hot plate at 60-90°C for 30-45 minutes to harden the film; The silicon wafer substrate with the array micro-needle structure is placed in a hydrofluoric acid solution at a water bath temperature of 45-60° C. to etch the silicon dioxide layer on the silicon wafer substrate for 9-12 seconds, and the array micro-needle structure is transferred to the silicon dioxide layer of the silicon wafer substrate; Then, the silicon wafer is placed in an acetone solution and soaked for 30 to 60 minutes to remove the photoresist and obtain an array micro-spray needle convex mold; Step a.
2. Using the array micro-needle convex mold prepared in step a.1, prepare an unbonded array micro-needle by a casting method; In step a.2, the casting method of the unbonded array micro-needle comprises the following steps: Step a.2.
1. Place the array micro-spray needle convex mold in a drying tower in a trimethylsiloxane atmosphere for 10 to 20 minutes, then pour the PDMS mixed solution on the array micro-spray needle convex mold, and place it in a vacuum environment of 10Pa for 1 to 2 hours to remove bubbles in the PDMS mixed solution while ensuring that the PDMS mixed solution fills the array micro-spray needle convex mold; Step a.2.
2. Place the array micro-needle convex mold filled in step a.2.1 in a vacuum oven at 60-85°C for curing for 2-4 hours; separate the cured needle profile blank from the array micro-needle convex mold, and remove excess waste on the needle profile blank to obtain an unbonded array micro-needle; The preparation method of the array needle cover plate comprises: Step b.
1. Obtaining an array needle cover plate mold; The preparation method of the array spray needle cover plate mold comprises: The glass substrate is treated with oxygen plasma, a photoresist is spin-coated on the glass substrate, and a pre-baking is performed, and then a cover plate mask is used for ultraviolet exposure, and then a post-baking and development is performed to obtain an array needle cover plate mold; Step b.
2. Casting the PDMS mixed solution into the array needle cover plate mold obtained in step b.1 to make an array needle cover plate blank; demolding and shaping the array needle cover plate blank to obtain an array needle cover plate; In step b.2, the demoulding and shaping method of the array needle cover plate blank includes: The solidified array needle cover plate blank is separated from the array needle cover plate mold and taken out; then the outer surface of the array needle cover plate blank is shaped to obtain the array needle cover plate profile; then, according to the required array needle cover plate shape, a nozzle liquid reservoir is manufactured on the array needle cover plate profile to obtain the array needle cover plate; Step 2. Align the array micro-needle processed in step 1 with the array needle cover plate, and proceed to step 3; Step 3. Press the array needle cover plate at the microchannel of the array micro needle to collapse the array needle cover plate and contact the bottom of the microchannel of the array micro needle to form an irreversible bond, so that the array needle cover plate leaves nanochannels in the microchannel of the array micro needle to obtain an array nano needle.
2. The method for manufacturing an array nanospray needle based on pressing molding according to claim 1, characterized in that: In step a.2.1, the PDMS mixed solution is a mixed solution of PDMS and a curing agent in a volume ratio of 4:1 to 10:
1.
3. The method for manufacturing an array nanospray needle based on pressing molding according to claim 2, characterized in that: In step b.1, the glass substrate is subjected to oxygen plasma treatment with a treatment power of 45 to 80 W and a treatment time of 15 to 20 s; The photoresist is spin-coated on the glass substrate at a low speed of 500-800 rpm and a spin-coating time of 6-10 s, and a high speed of 3000-5000 rpm and a spin-coating time of 30-40 s; The pre-bake is to place the glass substrate coated with photoresist on a horizontal hot plate for step baking; During the UV exposure process through the cover mask, the photoresist is first cooled to room temperature and then UV-exposed through the cover mask for 4 to 7 minutes; In the post-baking development, the UV-exposed photoresist is placed on a hot plate and post-baked for 2 to 5 minutes, and developed for 60 to 90 seconds to obtain an array needle cover plate mold.
4. The method for manufacturing an array nanospray needle based on pressing molding according to claim 3, characterized in that: In step b.2, the array needle cover plate blank casting method includes: The array needle cover plate mold is placed in a drying tower in a trimethylsiloxane atmosphere for 10 to 20 minutes, and then the PDMS mixed solution is poured on the array needle cover plate mold; and it is placed in a vacuum environment of 10Pa for 1 to 2 hours to remove excess bubbles in the PDMS mixed solution while ensuring that the PDMS mixed solution completely fills the array needle cover plate mold; and then it is placed in a vacuum oven at 60 to 85°C for 2 to 4 hours to obtain a cured array needle cover plate blank.
5. The method for manufacturing an array nanospray needle based on pressing molding according to claim 4, characterized in that: In step b.2, the PDMS mixed solution is a mixed solution of PDMS and a curing agent in a volume ratio of 4:1 to 10:
1.
6. The method for manufacturing an array nanospray needle based on pressing molding according to any one of claims 1 to 5, characterized in that: The photoresist is AZ703, AZ5214E, AZ701, BP212, BN308, or SU-8 photoresist; And / or, the silicon dioxide layer is replaced by an Al, Cr, Au, Ag, or Ni metal thin film layer.
Citation Information
Patent Citations
Nanofilter devices using elastomeric micro to nanochannel interfaces and methods based thereon
US20120196376A1