A UHMWPE fiber UD cloth and preparation method thereof
By adjusting the concentration of the spinning solution and the particle size of the UHMWPE resin, the consistency of the spinning solution is ensured, the problem of low fiber consistency is solved, the bulletproof performance of the UHMWPE fiber is improved, and excellent UD cloth bulletproof effect is achieved.
Patent Information
- Application Number
- CN202410847161.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing UHMWPE fiber production technology has low fiber consistency, resulting in a high fiber density coefficient of variation, which affects the ballistic performance of UD cloth.
By adjusting the concentration of the spinning solution and the particle size of the UHMWPE resin to ensure the consistency of the spinning solution, a twin-screw extruder is used for shearing and dissolving, combined with water bath cooling and post-spinning stretching, to prepare a linear density variation coefficient of less than 3%. UHMWPE fibers form excellent UD cloth.
The consistency and bulletproof performance of UHMWPE fiber are improved, and the prepared UD cloth shows a higher V50 value and better bulletproof effect in the target shooting test.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bulletproof substrates and relates to a UHMWPE fiber UD cloth and a preparation method thereof. Background Art
[0002] Traditional metal materials are heavy, inconvenient to wear, and lack flexibility. Bulletproof materials are developing towards lightweight, non-metallic, and composite. With the development and application of polymer materials, soft personal protection products made of high-performance fibers have basically replaced hard protection products in the military and police. The bulletproof substrate can be in the form of woven fabrics, knitted fabrics, UD fabrics, needle-punched felt, etc. The constituent fibers of the bulletproof substrate can be carbon fiber, aramid, aromatic heterocyclic fiber, ultra-high molecular weight polyethylene (UHMWPE) fiber, glass fiber, and artificial spider silk (a highly oriented fiber of amino acids) that has appeared in recent years.
[0003] Studies have shown that compared with woven fabrics, knitted fabrics, needle-punched felt, etc., UD fabrics have higher energy dispersion performance and fewer projectile penetration layers, can quickly absorb and diffuse bullet high-speed shock waves, and have significantly better anti-ballistic performance than other fabric forms. UD fabrics are also softer, which is beneficial to improving the comfort of personal protective equipment. Compared with carbon fiber, aromatic heterocyclic fiber, glass fiber, and artificial spider silk that has appeared in recent years, aramid and UHMWPE fibers have excellent properties such as ultra-high strength, high modulus, low density, and acid and alkali resistance. Compared with aramid, UHMWPE fibers have lower density, higher lightweight potential, higher specific strength and specific modulus, and better energy absorption characteristics. Under the same surface density, the bulletproof ability of the bulletproof substrate made of UHMWPE fibers is better than that of the bulletproof substrate made of aramid (about 25% higher). Therefore, it is necessary to use UHMWPE fibers to prepare UD fabrics.
[0004] All fibers in UD cloth are arranged in parallel and not interwoven, and the fibers between layers are staggered at vertical angles. This arrangement method enables UD cloth to disperse the energy generated by bullet impact faster and more effectively than ordinary fabrics, and has better bulletproof effect under the same conditions. However, this also requires that the consistency of the fibers used in UD cloth (fiber consistency refers to the degree of difference in performance indicators of different fiber rolls or the same roll of fibers, usually expressed as the coefficient of variation of the indicators) needs to be high, otherwise the prepared UD cloth may have gap defects, which will reduce the uniformity of the UD cloth and its bulletproof performance.
[0005] Affected by the particle size uniformity and structural stability of the UHMWPE resin raw materials, the coefficient of variation of the linear density of UHMWPE fiber products obtained by the existing UHMWPE fiber production technology is generally high, and the fiber consistency is low. For example, patent application CN111118615A discloses a method for processing ultra-high molecular weight polyethylene fiber spinning solution. This patent uses high-pressure emulsification and single-screw homogenization to reduce the adhesion and agglomeration caused by the partial dissolution of the PE surface layer, so that more solvent is dissolved into the PE powder, the dissolution temperature of the twin-screw is reduced, and the high-temperature degradation of the PE powder is reduced, thereby improving the fiber strength and the consistency of the strands. However, the patent does not specify the consistency data of the ultra-high molecular weight polyethylene fiber obtained by this method, and spinning aids including titanium dioxide, polyethylene glycol lipids, etc. are added during the dissolution process of the PE powder. The spinning aids are impurities, which are not conducive to the further improvement of the mechanical properties and consistency of the fiber.
[0006] From the above, it can be seen that the ballistic performance of UD cloth prepared by using UHMWPE fiber in the prior art needs to be further improved. Summary of the invention
[0007] The purpose of the present invention is to solve the problems existing in the prior art and to provide a UHMWPE fiber UD cloth and a preparation method thereof.
[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] A UHMWPE fiber UD cloth comprises two or more fiber layers, wherein the fibers in all the fiber layers are UHMWPE fibers, and the linear density variation coefficient CV value of the UHMWPE fibers (used to characterize the degree of difference in performance indicators of different fiber filament rolls) is less than 3%.
[0010] As the preferred technical solution:
[0011] As described above, the UHMWPE fiber UD cloth has a linear density of 800-1200D, a breaking strength of 36.9-39.5 cN / dtex, and an initial modulus of 1395-1752 cN / dtex.
[0012] As described above, the UHMWPE fiber UD cloth has a resin content of 12-25wt%.
[0013] As described above, the UHMWPE fiber UD cloth has a V50 value of 638-713 m / s in a target shooting test.
[0014] The present invention also provides a method for preparing a UHMWPE fiber UD cloth as described in any of the preceding items, wherein after the UHMWPE fibers are prepared, the UHMWPE fibers are sequentially spread, glued, and laminated to obtain the UHMWPE fiber UD cloth;
[0015] The preparation process of UHMWPE fiber is as follows: UHMWPE resin is swelled and dissolved in a solvent to prepare a spinning solution, and then spinning is performed to obtain UHMWPE fiber. When the average particle size d of the UHMWPE resin is in μm and the concentration C of the spinning solution is in wt%, Cd 2 <20000, which can ensure that the UHMWPE resin can swell and dissolve evenly, which is beneficial to improve the consistency of the spinning solution. The linear density coefficient of variation CV value of the obtained UHMWPE fiber is <3%. The specific principle is as follows:
[0016] The concentration of the spinning solution and the particle size of the UHMWPE resin are roughly inversely related, that is, the smaller the particle diameter, the higher the swelling concentration can be. This is because the smaller the particle diameter, the easier it is for the solvent to diffuse into the interior of the particle, and the shorter the time required for swelling. In this way, different particles can achieve the same swelling and dissolution effects in a shorter time, the consistency of the spinning solution is good, and a fiber product with high consistency can be obtained; on the contrary, if the particle diameter is larger, the time required for the solvent to diffuse into the interior of the particle is long, so there may be some larger particles that fail to achieve the effect of sufficient swelling and dissolution, and enter the next stage, resulting in poor consistency of the spinning solution; and when good swelling and dissolution consistency is achieved, the raw material particle diameter has a certain range, and the production situation also has certain requirements for the concentration of the spinning solution. Under the premise of satisfying good fiber consistency and taking into account the actual production situation, the present invention has obtained the relationship between the concentration of the above-mentioned spinning solution and the particle size of the UHMWPE resin through various explorations.
[0017] As the preferred technical solution:
[0018] In the method described above, the value range of d is 108~175μm. Within a certain range, a small particle size is conducive to the diffusion of the solvent into the UHMWPE resin, thereby improving the consistency of the spinning solution; the value range of C is 0.1~1.0wt%, and a low concentration is more conducive to the dispersion of UHMWPE resin particles and improves the consistency of the spinning solution; the Mw of the UHMWPE resin is 4~10 million, and the Mw / Mn is 1.5~5. The concentrated molecular weight of the UHMWPE resin is conducive to the consistency of the dissolution process, and the prepared primary fiber has better consistency.
[0019] As described above, the preparation steps of UHMWPE fiber are as follows:
[0020] (a) Fully mixing and swelling the UHMWPE resin and solvent (50-80# mineral oil) to obtain a uniform swelling material;
[0021] (b) feeding the swelling material into a twin-screw extruder for shearing and dissolving to obtain a spinning solution;
[0022] (c) after metering, the spinning solution enters a water bath for cooling and stretching to obtain nascent fibers;
[0023] (d) After the initial fiber phase equilibrium, UHMWPE fiber is obtained through post-spinning and stretching.
[0024] In the method described above, the swelling temperature is 60-120° C., the shear dissolution temperature is 100-300° C., the shear dissolution speed is 100-400 rpm, and the post-spinning stretching multiple is 50-100 times.
[0025] Beneficial effects:
[0026] The invention ensures that the coefficient of variation CV value of the linear density of the prepared UHMWPE fiber is less than 3% by adjusting the relationship between the concentration of the spinning solution and the particle size of the UHMWPE resin, thereby preparing a UD cloth with excellent ballistic performance, thereby making up for the shortcomings of the prior art. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0028] The testing methods of the relevant performance indicators in the following embodiments and comparative examples are as follows:
[0029] Linear density variation coefficient CV value: measured according to GB / T 14344-2008 “Test method for tensile properties of chemical fiber filaments”.
[0030] Breaking strength: measured according to GB / T19975-2005 “Test method for tensile properties of high-strength fiber filaments”.
[0031] Initial modulus: measured according to GB / T19975-2005 “Test method for tensile properties of high-strength fiber filaments”.
[0032] Target test V50 value: Determined according to GA950-2011 "V50 test method for bulletproof materials and products".
[0033] Sliver unevenness: measured according to GB / T 14346-1993 “Test method for electronic sliver unevenness of chemical filament yarns”.
[0034] The preparation steps of UHMWPE fiber UD cloth with two fiber layers are as follows:
[0035] (1) Fiber spreading;
[0036] The UHMWPE fiber package yarn is installed on the creel, and the UHMWPE fiber is drawn out from the creel, and passes through the regularly arranged threading holes and the fiber concentration plate in turn to enter the surface density control device. After the UHMWPE fiber bundle is accurately positioned in the width direction, it enters the fiber spreading module for uniform fiber spreading;
[0037] (2) Gluing;
[0038] The UHMWPE fibers evenly spread in step (1) are fed into a gluing device for even gluing;
[0039] (3) Lamination;
[0040] Spread the substrate evenly and compound it with the UHMWPE fiber evenly coated with glue in step (2);
[0041] (4) Dry and shape and then cool naturally;
[0042] The UHMWPE fiber after being compounded with the substrate in step (3) is heated and dried in a drying and shaping module, and then naturally cooled in the air through a cooling module;
[0043] (5) Fiber spreading;
[0044] The UHMWPE fiber is drawn out from the creel, and passes through regularly arranged threading holes and fiber concentration plates in turn to enter the surface density control device. After the UHMWPE fiber bundle is accurately positioned in the width direction, it enters the fiber spreading module for uniform fiber spreading;
[0045] (6) Gluing;
[0046] The UHMWPE fibers evenly spread in step (5) are fed into a gluing device for even gluing;
[0047] (7) Lamination;
[0048] The UHMWPE fibers uniformly coated with glue in step (6) are superimposed on the fiber surface of the UHMWPE fibers composited with the substrate obtained in step (4); wherein the fibers of two adjacent layers are arranged in a staggered manner at a vertical angle;
[0049] (8) Dry and shape and then cool naturally;
[0050] The UHMWPE fibers laminated in step (7) are then heated, dried and shaped in a drying and shaping module, and then naturally cooled in the air through a cooling module, and the substrate is removed to obtain a UHMWPE fiber UD cloth.
[0051] The preparation steps of UHMWPE fiber UD cloth with three fiber layers are as follows:
[0052] (1) Fiber spreading;
[0053] The UHMWPE fiber package yarn is installed on the creel, and the UHMWPE fiber is drawn out from the creel, and passes through the regularly arranged threading holes and the fiber concentration plate in turn to enter the surface density control device. After the UHMWPE fiber bundle is accurately positioned in the width direction, it enters the fiber spreading module for uniform fiber spreading;
[0054] (2) Gluing;
[0055] The UHMWPE fibers evenly spread in step (1) are fed into a gluing device for even gluing;
[0056] (3) Lamination;
[0057] Spread the substrate evenly and compound it with the UHMWPE fiber evenly coated with glue in step (2);
[0058] (4) Dry and shape and then cool naturally;
[0059] The UHMWPE fiber after being compounded with the substrate in step (3) is heated and dried in a drying and shaping module, and then naturally cooled in the air through a cooling module;
[0060] (5) Fiber spreading;
[0061] The UHMWPE fiber is drawn out from the creel, and passes through regularly arranged threading holes and fiber concentration plates in turn to enter the surface density control device. After the UHMWPE fiber bundle is accurately positioned in the width direction, it enters the fiber spreading module for uniform fiber spreading;
[0062] (6) Gluing;
[0063] The UHMWPE fibers evenly spread in step (5) are fed into a gluing device for even gluing;
[0064] (7) Lamination;
[0065] The UHMWPE fibers uniformly coated with glue in step (6) are superimposed on the fiber surface of the UHMWPE fibers composited with the substrate obtained in step (4); wherein the fibers of two adjacent layers are arranged in a staggered manner at a vertical angle;
[0066] (8) Dry and shape and then cool naturally;
[0067] The UHMWPE fibers laminated in step (7) are heated and dried in a drying and shaping module, and then naturally cooled in the air in a cooling module;
[0068] (9) Fiber spreading;
[0069] The UHMWPE fiber is drawn out from the creel, and passes through regularly arranged threading holes and fiber concentration plates in turn to enter the surface density control device. After the UHMWPE fiber bundle is accurately positioned in the width direction, it enters the fiber spreading module for uniform fiber spreading;
[0070] (10) Gluing;
[0071] The UHMWPE fibers evenly spread in step (9) are fed into a gluing device for even gluing;
[0072] (11) Lamination;
[0073] The UHMWPE fibers uniformly coated with glue in step (10) are superimposed on the fiber surfaces of the two layers of UHMWPE fiber layers obtained in step (8); wherein the fibers of the two adjacent layers are staggered at a vertical angle;
[0074] (12) Dry and shape and then cool naturally;
[0075] The UHMWPE fibers laminated in step (11) are heated, dried and shaped in a drying and shaping module, and then naturally cooled in the air through a cooling module, and the substrate is removed to obtain a UHMWPE fiber UD cloth.
[0076] UHMWPE fiber UD cloth with more than four fiber layers can be prepared by referring to the above method. According to the required number of layers, it can be prepared by stacking layers. It only needs to repeat the steps of yarn spreading, gluing, laminating, drying and shaping and then naturally cooling (removing the substrate is carried out during the natural cooling after the last drying and shaping), and then the UHMWPE fiber UD cloth with more than four fiber layers can be obtained.
[0077] Example 1
[0078] A method for preparing UHMWPE fiber, the specific steps are as follows:
[0079] (1) Preparation of raw materials;
[0080] UHMWPE resin: Mw is 5.5 million, Mw / Mn is 5.0, and the average particle size d is 152 μm;
[0081] Solvent: No. 68 mineral oil, the manufacturer is Zhejiang Zhengxin Petroleum Technology Co., Ltd., the brand is No. 68 industrial white oil;
[0082] (2) Preparation of UHMWPE fibers;
[0083] (2.1) Fully mixing and swelling the UHMWPE resin and the solvent to obtain a uniform swelling material; wherein the swelling temperature is 100°C;
[0084] (2.2) feeding the swollen material into a twin-screw extruder and dissolving the swollen material at 100°C and 350 rpm to obtain a spinning solution; wherein the concentration C of the spinning solution is 0.5 wt%;
[0085] (2.3) The spinning solution is metered and then placed in a water bath for cooling and drawing to obtain primary fibers;
[0086] (2.4) After the primary fiber reaches phase equilibrium, it is stretched by post-spinning to obtain UHMWPE fiber, where the stretching ratio is 57.8 times.
[0087] The final UHMWPE fiber has a linear density of 800D, a strand unevenness of 2.5%, a linear density variation coefficient CV value of 2.3%, a breaking strength of 36.9 cN / dtex, and an initial modulus of 1480 cN / dtex.
[0088] A method for preparing a UHMWPE fiber UD cloth is prepared by using the UHMWPE fiber prepared as above, the number of fiber layers is 25, the UHMWPE fibers in different fiber layers come from different silk rolls, the substrate used is a film with a thickness of 50 μm, and the manufacturer of the sizing agent used during gluing is Anqing Kechuang Chemical Co., Ltd., and the brand is PU 626S.
[0089] The resin content of the UHMWPE fiber UD cloth finally obtained is 12wt%, and the surface density of the UHMWPE fiber UD cloth is 5.73kg / m 2 , the target test V50 value is 642m / s.
[0090] Comparative Example 1
[0091] A method for preparing UHMWPE fiber is basically the same as that of Example 1, except that in step (2.2), the concentration C of the spinning solution is 1.2 wt%.
[0092] The final UHMWPE fiber had a strand unevenness of 4.4%, a linear density variation coefficient CV value of 4.0%, a breaking strength of 37.0 cN / dtex, and an initial modulus of 1468 cN / dtex.
[0093] A method for preparing a UHMWPE fiber UD cloth is basically the same as that in Example 1, except that the UHMWPE fiber used is the UHMWPE fiber prepared in this comparative example.
[0094] The target test V50 value of the UHMWPE fiber UD cloth finally obtained is 583m / s.
[0095] Comparing Comparative Example 1 with Example 1, it can be seen that due to the Cd 2 When the value is greater than 20,000, the linear density coefficient of variation of the UHMWPE fiber obtained is too high, which in turn leads to high coefficients of variation of the breaking strength and initial modulus of the UHMWPE fiber obtained, uneven distribution of the breaking work of the UHMWPE fiber, and defects and weak points in the prepared UD cloth. In the bulletproof process, the fiber is more likely to break and the bulletproof effect is poor. This is because when the average particle size of the UHMWPE resin is too large and the concentration of the spinning solution is too high, the space required for the UHMWPE particles to swell is insufficient, and the difficulty of the solvent to further penetrate into the interior of the UHMWPE particles after diffusion increases, resulting in a decrease in the consistency of the swelling and dissolution effects, and there may be insufficient dissolution, resulting in a decrease in the consistency of the UHMWPE fiber obtained, a high linear density coefficient of variation CV value, and then high coefficients of variation of the breaking strength and initial modulus, which reduces the performance of the UHMWPE fiber UD cloth prepared therefrom and leads to poor bulletproof effect.
[0096] Example 2
[0097] A method for preparing UHMWPE fiber, the specific steps are as follows:
[0098] (1) Preparation of raw materials;
[0099] UHMWPE resin: Mw is 4 million, Mw / Mn is 3.6, and the average particle size d is 175 μm;
[0100] Solvent: No. 50 mineral oil, the manufacturer is Zhejiang Zhengxin Petroleum Technology Co., Ltd., the brand is No. 50 industrial white oil;
[0101] (2) Preparation of UHMWPE fibers;
[0102] (2.1) The UHMWPE resin and the solvent are fully mixed and swelled to obtain a uniform swelling material; wherein the swelling temperature is 60°C;
[0103] (2.2) feeding the swollen material into a twin-screw extruder and dissolving the swollen material at 200° C. and 100 rpm to obtain a spinning solution; wherein the concentration C of the spinning solution is 0.2 wt %;
[0104] (2.3) The spinning solution is metered and then placed in a water bath for cooling and drawing to obtain primary fibers;
[0105] (2.4) After the primary fiber reaches phase equilibrium, it is stretched by post-spinning to obtain UHMWPE fiber; the stretching ratio after spinning is 50.2 times.
[0106] The final UHMWPE fiber has a linear density of 800D, a strand unevenness of 2.9%, a linear density variation coefficient CV value of 2.6%, a breaking strength of 37.5 cN / dtex, and an initial modulus of 1395 cN / dtex.
[0107] A method for preparing a UHMWPE fiber UD cloth is prepared by using the UHMWPE fiber prepared as above, the number of fiber layers is 28, the UHMWPE fibers in different fiber layers come from different silk rolls, the substrate used is a film with a thickness of 52 μm, and the manufacturer of the sizing agent used during gluing is Anqing Kechuang Chemical Co., Ltd., and the brand is PU 626S.
[0108] The resin content of the UHMWPE fiber UD cloth finally obtained is 18wt%, and the surface density of the UHMWPE fiber UD cloth is 6.03kg / m 2 , the target test V50 value is 638m / s.
[0109] Example 3
[0110] A method for preparing UHMWPE fiber, the specific steps are as follows:
[0111] (1) Preparation of raw materials;
[0112] UHMWPE resin: Mw is 8 million, Mw / Mn is 2.6, and the average particle size d is 108 μm;
[0113] Solvent: No. 68 mineral oil, the manufacturer is Zhejiang Zhengxin Petroleum Technology Co., Ltd., the brand is No. 68 industrial white oil;
[0114] (2) Preparation of UHMWPE fibers;
[0115] (2.1) Fully mixing and swelling the UHMWPE resin and the solvent to obtain a uniform swelling material; wherein the swelling temperature is 70°C;
[0116] (2.2) feeding the swollen material into a twin-screw extruder and dissolving the swollen material at 250°C and 250 rpm to obtain a spinning solution; wherein the concentration C of the spinning solution is 0.9 wt%;
[0117] (2.3) The spinning solution is metered and then placed in a water bath for cooling and drawing to obtain primary fibers;
[0118] (2.4) After the primary fiber reaches phase equilibrium, it is stretched by post-spinning to obtain UHMWPE fiber; the post-spinning stretching ratio is 79.4 times.
[0119] The final UHMWPE fiber has a linear density of 800D, a strand unevenness of 1.8%, a linear density variation coefficient CV value of 1.5%, a breaking strength of 39.5 cN / dtex, and an initial modulus of 1752 cN / dtex.
[0120] A method for preparing a UHMWPE fiber UD cloth is prepared by using the UHMWPE fiber prepared as above, the number of fiber layers is 25, the UHMWPE fibers in different fiber layers come from different silk rolls, the substrate used is a film with a thickness of 45 μm, and the manufacturer of the sizing agent used during gluing is Anqing Kechuang Chemical Co., Ltd., and the brand is PU 626S.
[0121] The resin content of the UHMWPE fiber UD cloth finally obtained is 22wt%, and the surface density of the UHMWPE fiber UD cloth is 5.28kg / m 2 , the target test V50 value is 713m / s.
[0122] Example 4
[0123] A method for preparing UHMWPE fiber, the specific steps are as follows:
[0124] (1) Preparation of raw materials;
[0125] UHMWPE resin: Mw is 6.6 million, Mw / Mn is 1.5, and the average particle size d is 126 μm;
[0126] Solvent: No. 68 mineral oil, the manufacturer is Zhejiang Zhengxin Petroleum Technology Co., Ltd., the brand is No. 68 industrial white oil;
[0127] (2) Preparation of UHMWPE fibers;
[0128] (2.1) Fully mixing and swelling the UHMWPE resin and the solvent to obtain a uniform swelling material; wherein the swelling temperature is 90°C;
[0129] (2.2) feeding the swollen material into a twin-screw extruder and dissolving it by shearing at 300°C and 300 rpm to obtain a spinning solution; wherein the concentration C of the spinning solution is 1.0 wt%;
[0130] (2.3) The spinning solution is metered and then placed in a water bath for cooling and drawing to obtain primary fibers;
[0131] (2.4) After the primary fiber reaches phase equilibrium, it is stretched by post-spinning to obtain UHMWPE fiber, where the stretching ratio is 98.5 times.
[0132] The final UHMWPE fiber has a linear density of 800D, a strand unevenness of 1.9%, a linear density variation coefficient CV value of 1.6%, a breaking strength of 38.3 cN / dtex, and an initial modulus of 1645 cN / dtex.
[0133] A method for preparing a UHMWPE fiber UD cloth is prepared by using the UHMWPE fiber prepared as above, the number of fiber layers is 25, the UHMWPE fibers in different fiber layers come from different silk rolls, the substrate used is a film with a thickness of 46 μm, and the manufacturer of the sizing agent used during sizing is Anqing Kechuang Chemical Co., Ltd., and the brand is PU 626S.
[0134] The resin content of the UHMWPE fiber UD cloth finally obtained is 20wt%, and the surface density of the UHMWPE fiber UD cloth is 5.68kg / m 2 , the target test V50 value is 672m / s.
[0135] Example 5
[0136] A method for preparing UHMWPE fiber, the specific steps are as follows:
[0137] (1) Preparation of raw materials;
[0138] UHMWPE resin: Mw is 6.6 million, Mw / Mn is 4.0, and the average particle size d is 134 μm;
[0139] Solvent: No. 68 mineral oil, the manufacturer is Zhejiang Zhengxin Petroleum Technology Co., Ltd., the brand is No. 68 industrial white oil;
[0140] (2) Preparation of UHMWPE fibers;
[0141] (2.1) The UHMWPE resin and the solvent are fully mixed and swelled to obtain a uniform swelling material; wherein the swelling temperature is 110°C;
[0142] (2.2) feeding the swollen material into a twin-screw extruder and dissolving the swollen material at 280° C. and 400 rpm to obtain a spinning solution; wherein the concentration C of the spinning solution is 0.7 wt %;
[0143] (2.3) The spinning solution is metered and then placed in a water bath for cooling and drawing to obtain primary fibers;
[0144] (2.4) After the primary fiber reaches phase equilibrium, it is stretched by post-spinning to obtain UHMWPE fiber; the post-spinning stretching ratio is 62 times.
[0145] The final UHMWPE fiber has a linear density of 1200D, a yarn unevenness of 2.3%, a linear density variation coefficient CV value of 2.1%, a breaking strength of 37.0 cN / dtex, and an initial modulus of 1550 cN / dtex.
[0146] A method for preparing a UHMWPE fiber UD cloth is prepared by using the UHMWPE fiber prepared as above, the number of fiber layers is 25, the UHMWPE fibers in different fiber layers come from different silk rolls, the substrate used is a film with a thickness of 55 μm, and the manufacturer of the sizing agent used during gluing is Anqing Kechuang Chemical Co., Ltd., and the brand is PU 626S.
[0147] The resin content of the UHMWPE fiber UD cloth finally obtained is 25wt%, and the surface density of the UHMWPE fiber UD cloth is 6.40kg / m 2 , the target test V50 value is 657m / s.
[0148] Example 6
[0149] A method for preparing UHMWPE fiber, the specific steps are as follows:
[0150] (1) Preparation of raw materials;
[0151] UHMWPE resin: Mw is 10 million, Mw / Mn is 3.1, and the average particle size d is 115 μm;
[0152] Solvent: No. 80 mineral oil, the manufacturer is Zhejiang Zhengxin Petroleum Technology Co., Ltd., the brand is No. 80 industrial white oil;
[0153] (2) Preparation of UHMWPE fibers;
[0154] (2.1) Fully mixing and swelling the UHMWPE resin and the solvent to obtain a uniform swelling material; wherein the swelling temperature is 120°C;
[0155] (2.2) feeding the swollen material into a twin-screw extruder and dissolving the swollen material at 180°C and 200 rpm to obtain a spinning solution; wherein the concentration C of the spinning solution is 0.8 wt%;
[0156] (2.3) The spinning solution is metered and then placed in a water bath for cooling and drawing to obtain primary fibers;
[0157] (2.4) After the primary fiber reaches phase equilibrium, it is stretched by post-spinning to obtain UHMWPE fiber; the post-spinning stretching ratio is 68 times.
[0158] The final UHMWPE fiber has a linear density of 1000D, a yarn unevenness of 2.1%, a linear density variation coefficient CV value of 1.7%, a breaking strength of 37.1 cN / dtex, and an initial modulus of 1600 cN / dtex.
[0159] A method for preparing a UHMWPE fiber UD cloth is prepared by using the UHMWPE fiber prepared as above, the number of fiber layers is 28, the UHMWPE fibers in different fiber layers come from different silk rolls, the substrate used is a film with a thickness of 48 μm, and the manufacturer of the sizing agent used during gluing is Anqing Kechuang Chemical Co., Ltd., and the brand is PU 626S.
[0160] The resin content of the UHMWPE fiber UD cloth finally obtained is 15wt%, and the surface density of the UHMWPE fiber UD cloth is 6.10kg / m 2 , the target test V50 value is 650m / s.
Claims
1. A UHMWPE fiber UD cloth, comprising two or more fiber layers, wherein the fibers in all the fiber layers are UHMWPE fibers, characterized in that: The coefficient of variation of the linear density of UHMWPE fiber is <3%; The preparation process of UHMWPE fiber is as follows: UHMWPE resin is swelled and dissolved in a solvent to prepare a spinning solution, and then spinning is performed to obtain UHMWPE fiber. When the average particle size d of the UHMWPE resin is in μm and the concentration C of the spinning solution is in wt%, Cd 2 <20000.
2. The UHMWPE fiber UD cloth according to claim 1, characterized in that: The linear density of UHMWPE fiber is 800~1200D, the breaking strength is 36.9~39.5cN / dtex, and the initial modulus is 1395~1752cN / dtex.
3. The UHMWPE fiber UD cloth according to claim 1, characterized in that: The resin content of UHMWPE fiber UD cloth is 12~25wt%.
4. The UHMWPE fiber UD cloth according to any one of claims 1 to 3, characterized in that: The V50 value of the UHMWPE fiber UD cloth target test is 638~713m / s.
5. The UHMWPE fiber UD cloth according to claim 1, characterized in that: The preparation method of the UHMWPE fiber UD cloth is as follows: after preparing the UHMWPE fiber, the UHMWPE fiber is sequentially spread, glued, and laminated to obtain the UHMWPE fiber UD cloth.
6. The UHMWPE fiber UD cloth according to claim 5, characterized in that: The value range of d is 108~175μm; the value range of C is 0.1~1.0wt%; the Mw of UHMWPE resin is 4~10 million, and Mw / Mn is 1.5~5.
7. The UHMWPE fiber UD cloth according to claim 5, characterized in that: The preparation steps of UHMWPE fiber are as follows: (a) Fully mixing and swelling the UHMWPE resin and the solvent to obtain a uniform swelling material; (b) feeding the swelling material into a twin-screw extruder for shearing and dissolving to obtain a spinning solution; (c) after metering, the spinning solution enters a water bath for cooling and stretching to obtain nascent fibers; (d) After the initial fiber phase equilibrium, UHMWPE fiber is obtained through post-spinning and stretching.
8. The UHMWPE fiber UD cloth according to claim 7, characterized in that: The swelling temperature is 60~120℃, the shear dissolution temperature is 100~300℃, the shear dissolution speed is 100~400rpm, and the post-spinning stretching multiple is 50~100 times.