A method for rolling patterned plate without producing intermediate plate based on ESP process
By switching between four stands and five stands in the ESP process, and adjusting the thickness and cooling rate of the crystallizer outlet, the problem of continuous production of patterned plates in the ESP process was solved, efficient patterned steel plate rolling was achieved, and the cost was reduced. production costs and improved yield rate.
Patent Information
- Application Number
- CN202410853488.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing ESP process for rolling pattern plates cannot achieve continuous production, resulting in high production costs and low efficiency.
Using a method based on the ESP process, through the smelting, continuous casting, rough rolling, finish rolling, cooling and coiling processes, the switch between four and five stands is used to reduce the generation of intermediate plates and adjust the thickness and cooling rate of the crystallizer outlet. , combined with intelligent sector-section dynamic roll gap control, to achieve continuous rolling of patterned steel plates.
It reduces the production of intermediate plates, increases the yield rate to over 98%, saves production costs, and ensures uniform wear and service life of the work rolls.
Smart Images

Figure CN118385272B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel production, and relates to a method for rolling a patterned plate without producing an intermediate plate based on an ESP process. Background Art
[0002] Hot rolled patterned steel plates are widely used in various fields such as construction, machinery manufacturing, bridges, transportation, shipbuilding, etc. due to their beautiful appearance, good anti-skid effect, and easy cleaning. Patterned plates usually have no special requirements for product composition and performance, but the market demand is large and the price is high. Therefore, patterned plates are usually the most profitable products of hot rolling enterprises, and major steel mills are competing to develop and produce them.
[0003] At present, there are many studies on the rolling method of patterned steel plates based on the ESP thin slab continuous casting and rolling process, such as "Method for producing thin-gauge patterned steel plates based on ESP thin slab continuous casting and rolling process" (publication number CN 106077090 A). However, in the middle of the rolling process, the patterned roller surface is worn and the patterned roller needs to be replaced before continuing to roll, resulting in an intermediate plate, which makes continuous production impossible. Therefore, how to optimize and improve the production process of patterned steel plates is of great significance. Summary of the invention
[0004] The invention proposes a method for rolling a patterned plate based on an ESP process without producing an intermediate plate, which solves the problem in the prior art that the patterned plate rolled by the ESP process cannot be produced continuously and has a high production cost.
[0005] The technical solution of the present invention is achieved in this way:
[0006] A method for rolling a patterned plate without producing an intermediate plate based on an ESP process, comprising smelting, continuous casting of slabs, rough rolling, finish rolling, cooling and coiling;
[0007] The rough rolling process rolls out an intermediate plate with a thickness of 8 to 15 mm, and then heats the intermediate plate in an induction heating furnace at a temperature of 1080 to 1150° C. to remove phosphorus and obtain a semi-finished strip steel;
[0008] The finishing rolling process includes a five-stand finishing rolling mill unit. At the beginning of the casting, the four-stand mode is used to roll the steel to obtain a flat strip. When the thickness of the flat strip transitions to 2.0-3.5 mm, the F5 stand is put into use. The F5 stand is used to roll the patterned plate to obtain the patterned strip. The thickness of the obtained finished strip is 1.5-3.5 mm. When the bean-shaped meat loss defect occurs, the four-stand mode is switched to roll the flat strip, and the final rolling temperature is 810-850° C.
[0009] In the four-stand mode, the loads of the four-stand finishing mill are 21-31MN, 19-30MN, 16-26MN and 12-22MN respectively;
[0010] When the F5 stand is put into use, the loads of the five-stand finishing mill are 17~29MN, 15~27MN, 12~22MN, 10~20MN and 7~10MN respectively; the reduction rate of the F5 stand is 10~15%.
[0011] Preferably, the upper roll of the F5 stand in the five-stand finishing mill is a flat roll with a patterned roll, and the lower roll is a concave roll with a convexity of -25 to -50 μm.
[0012] Preferably, the smelting process forms molten steel, and the components of the molten steel include, by mass percentage, C: ≤0.05%, Si: 0.1-0.3%, Mn: 0.30-0.50%, S≤0.005%, P≤0.015%, and the rest are iron elements and unavoidable impurities.
[0013] Preferably, the dephosphorization process uses a pressure of 350 to 370 bar for dephosphorization.
[0014] Preferably, the continuous casting slab has a thickness of 95 mm.
[0015] Preferably, the continuous casting slab process adjusts the crystallizer outlet thickness to 100 mm, uses the intelligent sector segment dynamic roll gap control to reduce the thickness by 5 mm, and obtains a slab with a thickness of 95 mm after primary cooling and secondary cooling.
[0016] Preferably, the curling temperature in the curling process is 570-600°C.
[0017] The working principle and beneficial effects of the present invention are:
[0018] 1. The method for rolling patterned plates without producing intermediate plates based on the ESP process provided by the present invention adopts the ESP production line to produce 1.5-3.5 mm patterned steel plates, and reduces the production of intermediate plates by switching between four-frame and five-frame. Through the implementation of the present invention, 60-100 tons of intermediate plates can be produced less per pouring. The production cost is reduced, the yield rate is increased to more than 98%, and it is conducive to smooth production.
[0019] 2. The present invention adopts a thin slab continuous casting machine, adjusts the thickness of the crystallizer outlet, and utilizes intelligent sector segment dynamic roll gap control to produce a 95 mm slab after primary cooling and secondary cooling. The slab thickness is further reduced through the continuous casting process, and the internal heat of the slab is fully utilized. The slab enters a large reduction roughing mill and is directly rolled into an intermediate plate, thereby reducing the overall reduction of the roughing mill and further saving the energy consumption of the roughing mill.
[0020] 3. When the F5 stand of the present invention is pressed down, the thickness of the finished product corresponding to the F4 stand is 2.0-3.5 mm, the rolling load is 7-8 MN, and the reduction rate is 10-15%. It can achieve the stability of the rolling state when the last stand is put into use, prevent the occurrence of steel piling accidents and the impact on the working roll during pressing down, destroy the bean-shaped integrity of the working roll surface, and ensure the uniformity of the wear of the working roll during subsequent use.
[0021] 4. In the present invention, the mass percentage of C is ≤0.05%, wherein carbon is the main element for improving the strength of the material. By setting a lower curling temperature of 570-600°C and a faster cooling rate of 50-75%, a uniform and fine ferrite structure can be obtained at a lower carbon content, thereby obtaining a strength standard that meets the national standard requirements;
[0022] The mass percentage of Mn is 0.3-0.5%, and its main function is solid solution strengthening. The solid solution strengthening of manganese is very obvious, and it also plays a role in improving the strength of materials in ordinary carbon structural steel;
[0023] The mass percentage of Si is 0.1-0.3%, which is an important deoxidizer in steel and has a significant solid solution strengthening effect. However, Si is not good for welding and dendrite segregation and grain boundary segregation, so it should be controlled at ≤0.3%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0025] Figure 1 It is a schematic flow chart of the method for rolling a patterned plate without producing an intermediate plate by the ESP process of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] It should be noted that ESP (Endless Strip Production) is a thin slab continuous casting and rolling production line that can produce a whole strip of steel in one casting without frequent strip threading, so it is a fully continuous endless strip production line.
[0028] like Figure 1 The figure shows a schematic flow chart of a method for producing a patterned plate without producing an intermediate plate by the ESP process of the present invention.
[0029] Specifically, the present invention is a method for producing a patterned plate without an intermediate plate based on the ESP process, and uses an ESP headless rolling production line, including a high-speed continuous casting machine, a large-reduction rolling mill, an induction heating furnace, a high-pressure water dephosphorization device, a finishing mill, a laminar cooling device and a down coiler.
[0030] Specifically, it includes smelting, continuous slab casting, rough rolling, finishing rolling, cooling and coiling.
[0031] A. Smelting to form molten steel; the molten steel contains the following mass percentages: C: ≤0.05, Si: 0.1-0.3%, Mn: 0.30-0.50%, S≤0.005%, P≤0.015%, and the rest is iron and unavoidable impurities;
[0032] B. The continuous casting slab is cast by a high-speed continuous casting machine, and the thickness of the continuous casting slab is 95mm. It should be noted that the ESP production line is a rigid connection between the continuous casting machine and the rolling mill. The production line fully utilizes the waste heat of the continuous casting slab for rough rolling, omitting the gas heating furnace of the traditional rolling line. In order to fully utilize the waste heat of the slab for rolling and save the energy consumption of the rough rolling mill, the temperature of the continuous casting slab is not less than 980℃, the casting speed of the continuous casting machine is 4.0-5.5m / min, and then it directly enters the three-frame large-reduction rolling mill for rough rolling. In the large-reduction rolling mill, the continuous casting slab is rolled into an intermediate plate with a thickness of 8-15mm. After the large-reduction rolling mill A swing shear and scrap-pushing stand is arranged to remove the dummy rod and cut off the intermediate plate when problems occur in the subsequent equipment. The intermediate plate is then heated by an induction heating furnace at a temperature of 1080-1150°C. After high-pressure water dephosphorization to remove the surface oxide scale, a semi-finished strip is obtained, and then finished strip is obtained through finish rolling. The high-pressure water dephosphorization always maintains a pressure of 350-370 bar for dephosphorization. The nozzle angle and header height of the dephosphorization equipment are checked and adjusted after each shutdown. The production process only needs to stabilize the dephosphorization water pressure to meet the requirements of removing the oxide scale on the strip surface.
[0033] The induction heating furnace is installed before the high-pressure water dephosphorization of the finishing mill. Its function is to heat the strip and adjust the temperature of the intermediate plate. The purpose of the induction heating furnace temperature within the range of 1080-1150℃ is to ensure the final rolling temperature at the finishing exit, so that the strip can maintain good shaping during the rolling process of the F5 stand, and it is easy to form a full bean shape with a small load. It can also reduce the formation of iron oxide scale on the surface of the strip due to excessively high temperature during the heating process, and at the same time, it also reduces the energy consumption of the induction heating furnace;
[0034] C. The strip steel after descaling by high-pressure water is subjected to finish rolling to obtain the finished strip steel;
[0035] At the beginning of the casting, the four-stand mode is used to roll the steel to obtain flat strip steel. When the thickness of the flat strip steel transitions to 2.0-3.5mm, the F5 stand is used to roll the patterned plate to obtain the patterned strip steel. The thickness of the finished strip steel is 1.5-3.5mm. When bean-shaped meat loss defects occur, the four-stand mode is switched to roll the flat strip steel, and the final rolling temperature is 810-850℃.
[0036] The loads of the four-stand finishing mill are 21-31MN, 19-30MN, 16-26MN and 12-22MN respectively. It should be noted that the final rolling temperature of the four-stand is calculated based on the outlet temperature of the F4 stand. The temperature drop of each stand is about 50-70℃. The setting temperature of the four-stand induction furnace is lower than that of the five-stand mode, at 1080-1130℃. The low temperature setting reduces the power consumption cost of the induction furnace. When the rolling mileage of the four-stand is 40-60 kilometers or in the middle of the casting, the strip thickness transitions to 2.0-3. 5mm, the F5 stand is put into use, and the five-stand mode is started to roll the patterned plate to achieve the rolling of the patterned plate. It should be noted that the F5 stand is pressed down in the thickness range of 2.0 to 3.5mm to ensure the stability of the rolling state at the moment when the F5 last stand is pressed down, to prevent the occurrence of steel piling accidents and the impact on the working roll during pressing down, which will damage the bean-shaped integrity of the working roll surface, and at the same time ensure the uniformity of the working roll wear in the subsequent use process, improve the service life, and achieve the rolling of the patterned strip with a thickness of 1.5 to 3.5mm;
[0037] It should be noted that when the F5 stand is put into use, the loads of the five-stand finishing mill are 17-29MN, 15-27MN, 12-22MN, 10-20MN and 7-10MN respectively, and the reduction rate of the F5 final stand is in the range of 10-15%. After the F5 stand is put into use, it will share part of the load of other stands. At the same time, combined with the higher induction heating furnace temperature of 1100-1150℃, the deformation resistance of the strip during rolling is reduced, and the load of F1-F4 in the finishing stand is set to move forward, ensuring that the F5 stand rolls the patterned plate with a smaller load, and can reduce the grinding of the pattern roller and extend its service life;
[0038] The upper roll of the F5 stand is a flat roll with patterned rolls, and the lower roll is a concave roll with a convexity of -25~-50μm. It should be noted that the purpose of using a concave roll for the lower roll is to ensure that the strip is thin on both sides and thick in the middle after leaving the F5 finished product stand, forming a certain positive convex plate shape with a convexity of -25~-50μm. Combined with the bending roll control, the convexity of the finished strip plate can be controlled within 1% of the target finished product thickness, which is in line with the plate shape convexity control principle. The length of the roll is 1580mm, which is used to roll the patterned plate with a width of 1500mm.
[0039] D. When the strip steel exits the last stand finishing mill at the required final rolling temperature, it is cooled to a coiling temperature of 570-600°C by laminar cooling, and finally coiled into a hot rolled coil by a down coiler. It should be noted that the present invention combines the low-carbon design of molten steel smelting, sets a lower coiling temperature of 570-600°C and a faster cooling rate of 50-75%, and can obtain a uniform and fine ferrite structure at a lower carbon content, thereby obtaining a strength standard that meets the national standard requirements.
[0040] Example 1
[0041] In this embodiment, 2501 tons of coils were rolled, including 764.81 tons of flat strip steel and 1736.19 tons of patterned plates. The rolling specifications were 1.5-3.5 mm and the width was 1500 mm. The specific production parameters and steps are as follows:
[0042] A. Smelting to form molten steel, the composition of the molten steel in terms of mass percentage is shown in Table 1 below.
[0043]
[0044] B. The continuous casting slab is casted by a thin slab continuous casting machine with a thickness of 95 mm, and then directly enters three large-reduction rolling mills for rough rolling. The continuous casting slab is rolled into an intermediate plate in the large-reduction rolling mill with a thickness of 8 to 15 mm. A swing shear and a scrap pusher are arranged behind the large-reduction rolling mill to remove the dummy rod and remove the intermediate plate when problems occur in subsequent equipment. The intermediate plate is then heated by an induction heating furnace with a temperature between 1080 and 1150°C, and the surface iron oxide is removed by high-pressure water dephosphorization. The high-pressure water dephosphorization always maintains a pressure of 360 bar for dephosphorization;
[0045] The production parameters of each group are shown in Table 2 below.
[0046]
[0047] C. After being descaled by high-pressure water, the strip enters the five-stand finishing mill and is rolled to the final thickness; the final rolling temperature is 810~850℃;
[0048] The four-stand mode of F1~F4 was adopted to roll flat strip steel, with a total rolling of 764.81 tons and a rolling mileage of 40.6km. The thinnest specification was 1.8mm. When the flat strip steel specification transitioned to 3.5mm, the F5 stand was put into use. The five-stand mode was adopted to roll patterned plate, with a rolling mileage of 86.7km, a total rolling of 1736.19 tons, and the thinnest specification was 1.5mm. The total rolling was 2501 tons, with a yield rate of 98.14%. The five-stand mode rolled the patterned plate until the strip tail was thrown off and the pouring was stopped, completing the entire pouring rolling task.
[0049] The rolling force parameters of each finishing rolling stand are shown in Table 3.
[0050]
[0051] D. When the strip steel leaves the last stand finishing mill at the required final rolling temperature, it is cooled by laminar cooling front section, cooled to 580℃ at a cooling rate of 50%, and finally rolled into hot rolled coil by coiler. Among them, cooling rate = number of valves opened / total number of valves. The number of valves opened is calculated according to the cooling rate. If the result is not an integer, the water volume of the last valve is calculated according to the maximum water volume. If the cooling rate is 65% and the total number of valves is 8, the number of valves opened is 8×65%=5.2 valves. 5.2 valves means that 5 valves are opened first and the 6th valve is opened last, but the opening degree of the 6th valve (the percentage of the maximum water volume) is the percentage of the maximum water volume×0.2.
[0052] The inspection standards and performance indicators of the patterned plate of Example 1 are shown in Table 4 below.
[0053]
[0054] Comparative Example 1
[0055] Compared with Example 1, the only difference is that the five-stand mode is directly adopted in step C finishing rolling to produce patterned strip steel.
[0056] In step C, the finishing rolling adopts a five-stand mode to roll the patterned plate. When bean-shaped meat peeling defects appear, the patterned rollers are replaced. A total of 2472.2 tons are rolled, the thinnest specification is 1.5 mm, the yield rate is 95.37%, and the rolling force parameters of each stand are shown in Table 5.
[0057]
[0058] The comparison results of the casting production process of Example 1 and the comparative example are shown in Table 6 below.
[0059]
[0060] Note: Calculation method of yield rate: yield rate = (molten steel volume - tundish casting surplus - scale burnout - head and tail cuts at the beginning and end of pouring - accidental cuts during rolling) / molten steel volume * 100%
[0061] It can be seen from the above results that the production method of the present invention can realize flexible rolling of patterned plates, realize production continuity, reduce the production of 69.98 tons of intermediate plates, increase the yield rate by 2.77%, and increase the yield rate to more than 98%. The single-pass rolling mileage of patterned plates exceeds >85km, and the actual measurement of pattern height and mechanical property testing of patterned plates meet the national standard technical requirements.
[0062] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for rolling a patterned plate without producing an intermediate plate based on an ESP process, characterized in that: Including smelting, continuous slab casting, rough rolling, finishing rolling, cooling and coiling; The rough rolling process rolls out an intermediate plate with a thickness of 8 to 15 mm, and then heats the intermediate plate in an induction heating furnace at a temperature of 1080 to 1150° C. to remove phosphorus and obtain a semi-finished strip steel; The finishing rolling process includes a five-stand finishing rolling mill unit. At the beginning of the casting, the four-stand mode is used to roll the steel to obtain a flat strip. When the thickness of the flat strip transitions to 2.0-3.5 mm, the F5 stand is put into use. The F5 stand is used to roll the patterned plate to obtain the patterned strip. The thickness of the obtained finished strip is 1.5-3.5 mm. When the bean-shaped meat loss defect occurs, the four-stand mode is switched to roll the flat strip, and the final rolling temperature is 810-850° C. In the four-stand mode, the loads of the four-stand finishing mill are 21-31MN, 19-30MN, 16-26MN and 12-22MN respectively; When the F5 stand is put into use, the loads of the five-stand finishing mill are 17~29MN, 15~27MN, 12~22MN, 10~20MN and 7~10MN respectively; the reduction rate of the F5 stand is 10~15%.
2. A method for rolling a patterned plate without producing an intermediate plate based on an ESP process according to claim 1, characterized in that: The upper roll of the F5 stand in the five-stand finishing mill is a flat roll with a patterned roll, and the lower roll is a concave roll with a convexity of -25 to -50 μm.
3. A method for rolling a patterned plate without producing an intermediate plate based on an ESP process according to claim 1, characterized in that: The smelting process forms molten steel, and the components of the molten steel include C: ≤0.05%, Si: 0.1-0.3%, Mn: 0.30-0.50%, S≤0.005%, P≤0.015%, and the rest are iron elements and inevitable impurities.
4. A method for rolling a patterned plate without producing an intermediate plate based on an ESP process according to claim 1, characterized in that: The dephosphorization process uses a pressure of 350 to 370 bar to perform dephosphorization.
5. A method for rolling a patterned plate without producing an intermediate plate based on an ESP process according to claim 1, characterized in that: The thickness of the continuous casting slab is 95 mm.
6. A method for rolling a patterned plate without producing an intermediate plate based on an ESP process according to claim 1, characterized in that: The curling temperature in the curling process is 570-600°C.