Transparent magnesium-aluminum-silicon glass-ceramics with high hardness and high-scar fracture toughness and its preparation
By introducing ZnO and B2O3 into magnesia-aluminum-silicon-ceramic glass, a two-step heat treatment method is used to control the precipitation of crystal phases and form a composite structure, which solves the problems of insufficient hardness and indentation fracture toughness of magnesium-aluminum-silicate glass-ceramics in the existing technology. It achieves a combination of high hardness, high mark fracture toughness and excellent optical properties, making it suitable for a variety of applications.
Patent Information
- Application Number
- CN202410840546.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-27
AI Technical Summary
It is difficult for existing magnesium-aluminum-silicon-ceramic glass to have high hardness, high mark fracture toughness and excellent optical properties at the same time, which limits its wide application in different fields.
By introducing ZnO and B2O3 as co-doping agents into magnesia-aluminosilicate-ceramic glass, a two-step heat treatment method is used to control the precipitation of MgAl2Si3O10 and cordierite crystal phases to form a mutually compounded twin-crystal phase structure, thereby enhancing the hardness and indentation of the glass. Fracture toughness, and by reasonably adjusting the content of B2O3 and ZnO to balance crystal phase precipitation and optimize the optical properties of the glass.
It achieves high hardness (Vickers hardness is above 7.9 GPa, modulus is above 104.1 GPa), high-mark fracture toughness (above 1.14 MPa·m1/2) and excellent visible light transmittance (above 74%), and reduces the time required for glass preparation cost, and avoids the coloring impact on the base glass.
Smart Images

Figure CN118388140B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of microcrystalline glass, and relates to a transparent magnesium aluminum silicon microcrystalline glass with high hardness and high pressure scratch fracture toughness and a preparation method thereof. Background Art
[0002] Glass-ceramics, also known as glass ceramics, is a polycrystalline material in which the crystal phase and the glass phase coexist by controlling the crystallization of some specific basic components of glass under program-controlled temperature conditions. The internal structural characteristics of glass-ceramics determine that glass-ceramics will have the advantages of both glass and ceramics, and have many advantages such as good mechanical properties, dielectric properties, chemical stability, etc.
[0003] In recent years, lithium aluminum silicon (Li2O-A12O3-SiO2, LAS) system glass-ceramics has been widely used due to its excellent thermal expansion properties, but its mechanical properties are average, such as Young's modulus is generally only 90~95GPa, indentation fracture toughness is 1~1.3MPa·m 1 / 2 , Vickers hardness is 6.5~7.5GPa. Although the Vickers hardness can be increased to 8.5GPa by ion exchange, the chemical stability of glass-ceramics is reduced due to the incorporation of alkali metals, which limits its application in more fields. And with the explosion of the new energy vehicle market, the lithium battery industry's demand for upstream raw materials has increased significantly, resulting in soaring prices of lithium carbonate and lithium-containing minerals, increasing the production cost of LAS system glass-ceramics.
[0004] At present, magnesium aluminum silicon (MgO-A12O3-SiO, MAS) system glass-ceramics is a hot topic in the research of transparent glass-ceramics. The mechanical properties of magnesium aluminum silicon system glass-ceramics are better than those of lithium aluminum silicon system glass-ceramics, and the basic components do not contain alkali metals. By adjusting the basic glass components and heat treatment process, glass-ceramics containing cordierite, aconite, mullite, sapphire, forsterite, enstatite and other phases can be obtained, which are suitable for different occasions. However, in the research of MAS glass-ceramics, it is difficult to prepare products with high transmittance, high hardness and high pressure scratch fracture toughness at the same time, which limits the widespread use of MAS glass-ceramics.
[0005] For example, patent CN113735450A discloses a method of using MgAl2Si4O 12The transparent MAS glass-ceramics with a main crystal phase and its preparation method, the glass components range from SiO2 58~65wt%, MgO 4~12.5wt%, Al2O3 12~18wt%, Li2O 0~2.5wt%, ZnO 0.5~8wt%, ZrO2 3~5wt%, P2O5 2~3wt%, CeO2 0.5~1wt%, SnO2 1~2wt%, Sb2O3 1~2wt%, after nucleation treatment at 750~830℃ for 2±0.2h, the transparent glass-ceramics are prepared, the Vickers hardness of the glass-ceramics is 7GPa, and the transmittance is 91%. However, the glass-ceramics prepared by this patent has no advantage in hardness compared with LAS glass-ceramics.
[0006] Patent CN110357435B discloses a magnesium-aluminum-silicon glass-ceramic, the glass components range from MgO 10~15wt%, Al2O3 25~35wt%, SiO2 40~50wt%, ZrO2 4~8wt%, B2O3 2~6wt%, CaO 1~5wt%, MnO 0.5~2wt%, the main crystal phase is MgAl2Si3O 10 The modulus of the glass-ceramics is 95 GPa, and its mechanical properties are relatively low. At the same time, since the preparation method is a powder sintering method, the sample is opaque.
[0007] Patent CN117466533A discloses a method for preparing magnesium aluminum silicon glass-ceramics. Magnesium aluminum silicon glass-ceramics include, by molar percentage, SiO2: 50~65%; Al2O3: 10~25%; P2O5: 0.01~5%; ZrO2: 0~3%; MgO: 4~25%; ZnO: 0.1~10%; Na2O: 6~30%; K2O: 0~3%. The main crystalline phase is cordierite, and the glass-ceramics is ion exchange strengthened. The maximum Vickers hardness after strengthening is only 7.05GPa, and the maximum indentation fracture toughness is only 1.18 MPa·m 1 / 2 The maximum visible light transmittance is 87%, and the hardness and indentation fracture toughness are not significantly higher than LAS glass-ceramics.
[0008] Therefore, it is of great significance to study a transparent magnesium-aluminum-silicon glass-ceramic with high hardness and high indentation fracture toughness and its preparation method, so as to prepare magnesium-aluminum-silicon glass-ceramic with high hardness, high indentation fracture toughness and excellent optical properties. Summary of the invention
[0009] The purpose of the present invention is to solve the problems existing in the prior art and to provide a transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness and a preparation method thereof.
[0010] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0011] A transparent magnesium aluminum silicon microcrystalline glass with high hardness and high indentation fracture toughness, wherein the microcrystalline glass has a Vickers hardness of 7.9 GPa or more, a modulus of 104.1 GPa or more, and an indentation fracture toughness of 1.14 MPa·m 1 / 2 Above, the visible light transmittance is above 74%;
[0012] The main crystalline phase of the microcrystalline glass is MgAl2Si3O 10 Crystal phase and cordierite crystal phase. The cordierite crystal phase is mainly distributed in MgAl2Si3O 10 Crystalline surface (the rest is distributed in the gaps between grains, or grows in clusters), MgAl2Si3O 10 The ratio (content ratio) of the crystal phase to the cordierite crystal phase is 2.9~9.9:1;
[0013] In terms of molar percentage, the glass raw materials of the microcrystalline glass include the following components:
[0014] SiO2 46~60%;
[0015] Al2O3 16~26%;
[0016] MgO 13~22%;
[0017] ZnO 1~10%;
[0018] B2O3 1~10%;
[0019] The molar ratio of ZnO to B2O3 is 1:3~3:1;
[0020] The glass raw materials are introduced from analytically pure silicon dioxide, aluminum oxide, basic magnesium carbonate pentahydrate, zinc oxide and boric acid respectively.
[0021] As the preferred technical solution:
[0022] As described above, in the transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness, the glass raw materials also include Sb2O3 as a clarifier, and the added amount of Sb2O3 is 1% of the total mass of the remaining glass raw materials.
[0023] The present invention also provides a method for preparing transparent magnesium aluminum silicon microcrystalline glass with high hardness and high high-scar fracture toughness. After the glass raw materials are cast to obtain basic glass, the basic glass is sequentially subjected to nucleation treatment and crystallization treatment to obtain the microcrystalline glass.
[0024] As the preferred technical solution:
[0025] The method for preparing the transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness as described above comprises the following specific steps:
[0026] (1) Mix the glass raw materials uniformly;
[0027] (2) The evenly mixed glass raw materials are placed in a quartz crucible and heated up with the furnace to melt and obtain glass liquid;
[0028] (3) pouring the glass liquid into a preheated mold to form it, and then placing it in an annealing furnace to anneal and eliminate stress, and obtaining the basic glass after cooling in the furnace;
[0029] (4) The base glass is subjected to nucleation treatment and crystallization treatment in sequence to obtain microcrystalline glass.
[0030] In the method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness as described above, the furnace heating rate in step (2) is 5-10°C / min, the melting temperature is 1550-1600°C, and the melting temperature is maintained for 2-4 hours.
[0031] In the method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness as described above, the preheating temperature of the mold in step (3) is 350-400°C, the annealing temperature is 650-720°C, and the annealing time is 2-4h.
[0032] In the method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness as described above, the process of nucleation treatment in step (4) is as follows: heating to 800-860°C at a rate of 5-10°C / min, and then nucleating for 8-12 hours.
[0033] The method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness as described above, wherein the crystallization process in step (4) is as follows: heating to 980-1100°C at a rate of 4-8°C / min, and then crystallizing for 20-60min. The short crystallization time allows the cordierite crystal phase and MgAl2Si3O 10 The size of the phase is smaller than the wavelength of visible light, which reduces the light scattering effect.
[0034] Invention mechanism:
[0035] The present invention uses a melting method to prepare a MAS system basic glass co-doped with ZnO and B2O3, and then controls the precipitation of MgAl2Si3O in the glass through a two-step heat treatment method. 10Of the two phases, the cordierite phase presents a six-membered ring crystal structure, with divalent metal ions and silicon or aluminum tetrahedrons connecting the six-membered rings. These tetrahedrons act like adhesives to assemble the hexahedrons into a three-dimensional skeleton. This three-dimensional skeleton structure can enhance the stability of the crystal, thereby improving the hardness and indentation fracture toughness of the microcrystalline glass. 10 It is a crystal phase in which magnesium ions are filled into the quartz solid solution. The Si in the quartz network structure 4+ The ions are partially replaced by Al 3+ Ion substitution, Mg 2+ The ions enter the hexagonal cavity composed of [SiO4] and [AlO4] tetrahedrons, maintaining the electrical neutrality of the structure as a whole and improving the stability of the structure. At the same time, the two crystals are different in morphology. Cordierite tends to form granular crystals, while MgAl2Si3O 10 In the process of crystallization, due to the MgAl2Si3O 10 The crystallization temperature of the crystal is lower than that of cordierite, so MgAl2Si3O 10 The crystal nucleus will precipitate first, and as MgAl2Si3O 10 The surface of the growing crystal provides nucleation sites for cordierite, promoting the heterogeneous nucleation process of cordierite, thereby further inducing the precipitation of cordierite and forming a new type of MgAl2Si3O 10 The microcrystalline glass grows on the surface of the nanocrystalline glass, eventually forming a twin phase that is composited with each other, which prolongs the path of crack propagation and strengthens the barrier to cracks, effectively hindering crack propagation and force transmission, thereby improving the hardness and indentation fracture toughness of the microcrystalline glass, making the microcrystalline glass scratch-resistant and not easy to break.
[0036] In addition, the precipitated cordierite phase and MgAl2Si3O 10 The refractive index of the phase is close to that of the base glass (both are around 1.54), which reduces the scattering effect of light. The final microcrystalline glass has good transparency.
[0037] In the prior art, MgAl2Si3O 10 The crystallization temperatures of the two crystal phases of Mg2Si3O and cordierite are quite different, so it is difficult to grow these two crystal phases in microcrystalline glass at the same time. The present invention solves this problem by introducing two additives, boron oxide (B2O3) and zinc oxide (ZnO), in addition to the ternary system of magnesium oxide, silicon oxide and aluminum oxide. The different contents of B2O3 in the system have different effects on the crystallization process, which may promote the precipitation of the cordierite crystal phase, or may inhibit the precipitation of the cordierite phase and promote the precipitation of MgAl2Si3O 10The introduced ZnO acts as a nucleating agent, promoting the precipitation of crystalline phases in the glass (including MgAl2Si3O 10 The present invention is based on the basic glass of magnesium aluminum silicon system. After introducing B2O3 and ZnO, an appropriate content of B2O3 and ZnO is adjusted to precipitate MgAl2Si3O in the system. 10 The effects of the crystal phase and the precipitated cordierite crystal phase are balanced, so that the glass still has a high content of MgAl2Si3O after crystallization. 10 Crystal phase and cordierite phase, by reasonably adjusting the addition amount of ZnO and B2O3, analyzing the change of crystallization peak temperature of the adjusted glass components, and selecting the appropriate crystallization temperature, finally transparent magnesium aluminum silicon microcrystalline glass with high hardness and high high pressure scratch fracture toughness was prepared.
[0038] Beneficial effects:
[0039] (1) The transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness of the present invention can effectively control the MgAl2Si3O 10 The precipitation of the cordierite crystal phase makes it more scratch-resistant and shatter-resistant than similar transparent glass-ceramics.
[0040] (2) The transparent magnesium aluminum silicon glass-ceramics of the present invention has high hardness and high indentation fracture toughness, is transparent and colorless, has high hardness, strong indentation fracture toughness, high visible light transmittance, and excellent comprehensive performance;
[0041] (3) The method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high high-scar fracture toughness of the present invention is that the raw materials for preparing the glass are easy to obtain and the cost is low, which is beneficial to industrial production; at the same time, the addition of ZnO and B2O3 in the present invention is beneficial to lowering the melting temperature of the glass, further reducing the cost of glass preparation;
[0042] (4) The method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high high-scratch fracture toughness of the present invention does not add a nucleating agent such as TiO2, thereby avoiding the coloring effect on the base glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 is the DSC curve of the base glass of Examples 4 to 5 of the present invention;
[0044] Figure 2 The crystal analysis spectrum of the glass-ceramics of Examples 4 and 5 of the present invention;
[0045] Figure 3 This is the surface crystal morphology of the glass-ceramics of Example 4;
[0046] Figure 4is the visible light transmittance spectrum of the glass-ceramics of Examples 4-5;
[0047] Figure 5 This is a comparison chart of the Vickers hardness of glass-ceramics of Examples 4 and 5;
[0048] Figure 6 This is a comparison chart of the modulus of glass-ceramics of Examples 4 and 5;
[0049] Figure 7 This is a comparison chart of the indentation fracture toughness of the glass-ceramics of Examples 4 and 5. DETAILED DESCRIPTION
[0050] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0051] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:
[0052] (1) Differential scanning calorimetry (DSC);
[0053] The test was carried out using a TGA / DSC3+ high-temperature synchronous thermal analyzer produced by Mettler, Switzerland. The heating rate during the test was 10°C / min and the maximum test temperature was 1200°C.
[0054] (2) X-ray diffraction (XRD);
[0055] The domestically produced DX2700B diffractometer was used for testing, and the test angle was in the range of 5°~85°.
[0056] (3) Crystal morphology (SEM);
[0057] The S-4800 scanning electron microscope produced by Hitachi of Japan was used for testing. The surface of the microcrystalline glass was treated with HF acid corrosion, and then the surface was sprayed with gold and observed under an electron microscope.
[0058] (4) Visible light transmittance;
[0059] The samples were ground and polished into 1 cm×1 cm blocks with a thickness of 4 mm, and the transmittance in the visible light wavelength range of 380~700 nm was measured using a UV-2600 ultraviolet-visible spectrometer produced by Shimadzu Corporation of Japan.
[0060] (5) Vickers hardness;
[0061] The hardness test was carried out using the FV-700 Vickers hardness tester produced by Shimadzu Corporation of Japan. A load of 9.8N was applied to the sample surface and the load was maintained for 10s to test the hardness value of the sample. Each sample was tested at least 5 times, and the final result was averaged.
[0062] (6) Indentation fracture toughness;
[0063] Using the FV-700 Vickers hardness tester produced by Shimadzu Corporation of Japan, pressure was applied on the surface to make a standard diamond indentation of the crack extending along the vertex angle, and the indentation fracture toughness of the sample was measured and calculated. The calculation formula is as follows: Each sample was tested at least 5 times, and the final result was averaged;
[0064] ;
[0065] Among them, F is the load applied by the indenter, unit N; Hv is the Vickers hardness, unit GPa; E is the Young's modulus, unit GPa; C is the average length of the indentation crack, unit μm.
[0066] (7) Modulus;
[0067] The modulus of the sample was tested by a nanoindenter. After the sample was polished, the modulus was tested by a G200X nanoindenter produced by KLA, USA. Each sample was tested at least 5 times, and the final result was averaged.
[0068] Example 1
[0069] A method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness, the specific steps are as follows:
[0070] (1) Preparation of raw materials:
[0071] The glass raw materials include glass raw material I and Sb2O3; the added amount of Sb2O3 is 1% of the total mass of the glass raw material I;
[0072] In terms of mole percentage, the glass raw material I includes the following components:
[0073] SiO2 52%;
[0074] Al2O3 22%;
[0075] MgO 18%;
[0076] ZnO 2%;
[0077] B2O3 6%;
[0078] (2) Evenly mix the glass raw materials;
[0079] (3) The uniformly mixed glass raw materials are placed in a quartz crucible and heated to 1600°C in a furnace at a rate of 10°C / min to melt to obtain glass liquid, and the melting temperature is maintained for 3 hours;
[0080] (4) Pour the glass liquid into a mold preheated to 380°C for forming, then place it in an annealing furnace at 680°C for 2 hours to eliminate stress, and cool it to room temperature in the furnace to obtain the basic glass;
[0081] Thermal analysis of the base glass was performed using differential scanning calorimetry (DSC), and the glass transition temperature (Tg) of the base glass was 798°C, and the crystallization peak temperature (Tc) was 1040°C;
[0082] (5) The base glass was heated to 840°C at a rate of 5°C / min, subjected to nucleation treatment for 10 h, and then heated to 1040°C at a rate of 5°C / min, subjected to crystallization treatment for 30 min. After cooling to room temperature, a transparent magnesium aluminum silicon microcrystalline glass with high hardness and high pressure scratch fracture toughness was obtained.
[0083] The final transparent magnesium aluminum silicon glass-ceramics with high hardness and high indentation fracture toughness has a Vickers hardness of 8.1 GPa, a modulus of 117.3 GPa, and an indentation fracture toughness of 1.14 MPa·m. 1 / 2 , the visible light transmittance at 550nm is 83.5%; the main crystal phase of the transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness is MgAl2Si3O 10 Crystal phase and cordierite crystal phase. The cordierite crystal phase is mainly distributed in MgAl2Si3O 10 Crystal phase surface, MgAl2Si3O 10 The ratio of the crystal phase to the cordierite crystal phase is 7.4:1.
[0084] The commercial boron-containing soda-lime glass of Schott, the commercial soda-lime slide glass of Suzhou Shenying Optics, the commercial high borosilicate glass of Schott, the high aluminum glass of Corning commercial mobile phone cover, and the lithium aluminum silicon system microcrystalline glass (main crystal phases of Li2Si2O5 and petalite) of commercial mobile phone cover were tested in the same manner as in the embodiment, and the measured Vickers hardnesses were 6.7 GPa, 6.1 GPa, 6.9 GPa, 6.6 GPa, and 8.3 GPa, respectively, and the indentation fracture toughness was 0.67 MPa·m 1 / 2 、0.84MPa·m 1 / 2 、1.15MPa·m 1 / 2 , 1.09MPa·m 1 / 2 , 1.19MPa·m 1 / 2 .
[0085] Comparative Example 1
[0086] A method for preparing transparent magnesium aluminum silicon glass-ceramics is basically the same as that of Example 1, except that: the glass raw material does not contain ZnO, that is: ZnO 0%; B2O3 8%.
[0087] The final transparent magnesium aluminum silicon glass-ceramics has a Vickers hardness of 8.0 GPa, a modulus of 102.9 GPa, and an indentation fracture toughness of 1.05 MPa·m 1 / 2 , the visible light transmittance at 550nm is 60.2%; the main crystal phase of transparent magnesium aluminum silicon glass-ceramics is MgAl2Si3O 10 Crystal phase.
[0088] By comparing Comparative Example 1 with Example 1, it can be found that the Vickers hardness, modulus, indentation fracture toughness and visible light transmittance of Comparative Example 1 are lower than those of Example 1. This is because the addition of zinc oxide can act as a nucleating agent to promote the crystallization of microcrystalline glass, prompting the microcrystalline glass to precipitate MgAl2Si3O 10 The zinc oxide crystal phase and the cordierite crystal phase improve the mechanical properties of the microcrystalline glass. However, since Comparative Example 1 only has a high content of boron oxide, the phase separation caused by boron oxide during the high-temperature crystallization process (there is no zinc oxide to adjust the composition of the glass to reduce the impact of the phase separation) ultimately reduces the visible light transmittance.
[0089] Example 2
[0090] A method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness is basically the same as that in Example 1, except that the contents of ZnO and B2O3 components in step (1) are different, namely: ZnO 4%; B2O3 4%.
[0091] The final transparent magnesium aluminum silicon glass-ceramics with high hardness and high indentation fracture toughness has a Vickers hardness of 9.0 GPa, a modulus of 122.9 GPa, and an indentation fracture toughness of 1.16 MPa·m. 1 / 2 , the visible light transmittance at 550nm is 75.5%; the main crystal phase of transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness is MgAl2Si3O 10 Crystal phase and cordierite crystal phase. The cordierite crystal phase is mainly distributed in MgAl2Si3O 10 Crystal phase surface, MgAl2Si3O 10 The ratio of the crystal phase to the cordierite crystal phase is 5.26:1.
[0092] Example 3
[0093] A method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high high-scratch fracture toughness is basically the same as that in Example 2, except that the contents of ZnO and B2O3 in step (1) are different, namely: ZnO 6%; B2O3 2%. The temperature of the crystallization treatment in step (5) is 1000°C.
[0094] The final transparent magnesium aluminum silicon glass-ceramics with high hardness and high indentation fracture toughness has a Vickers hardness of 8.4 GPa, a modulus of 108.7 GPa, and an indentation fracture toughness of 1.19 MPa·m 1 / 2 , the visible light transmittance at 550nm is 80.1%; the main crystal phase of the transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness is MgAl2Si3O 10 Crystal phase and cordierite crystal phase. The cordierite crystal phase is mainly distributed in MgAl2Si3O 10 Crystal phase surface, MgAl2Si3O 10 The ratio of the crystal phase to the cordierite crystal phase is 9.9:1.
[0095] Example 4
[0096] A method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high high-scratch fracture toughness is basically the same as that in Example 3, except that the temperature of the crystallization treatment in step (5) is 1020°C.
[0097] like Figures 4 to 7 As shown in the figure, the transparent magnesium aluminum silicon glass-ceramics with high hardness and high indentation fracture toughness finally obtained has a Vickers hardness of 9.2 GPa, a modulus of 130.2 GPa, and an indentation fracture toughness of 2.1 MPa·m 1 / 2 , the visible light transmittance at 550nm is 74%; the main crystal phase of transparent magnesium aluminum silicon microcrystalline glass with high hardness and high pressure scratch fracture toughness is MgAl2Si3O 10 Crystal phase and cordierite crystal phase. The cordierite crystal phase is mainly distributed in MgAl2Si3O 10 Crystal phase surface, MgAl2Si3O 10 The ratio of the crystal phase to the cordierite crystal phase is 2.9:1.
[0098] like Figure 2 As shown, the glass-ceramics of Example 4 has MgAl2Si3O 10 Crystal phase and cordierite crystal phase; such as Figure 3 As shown in the figure, two crystal phases appeared in Example 4, namely MgAl2Si3O 10 The crystal phase and cordierite crystal phase of the microcrystalline glass are consistent with the XRD display, and the MgAl2Si3O 10 Microcrystalline glass with crystalline phase and cordierite crystal phase.
[0099] Example 5
[0100] A method for preparing a transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness, the specific steps are as follows:
[0101] (1) Preparation of raw materials:
[0102] The glass raw materials include glass raw material I and Sb2O3; the added amount of Sb2O3 is 1% of the total mass of the glass raw material I;
[0103] In terms of mole percentage, the glass raw material I includes the following components:
[0104] SiO2 52%;
[0105] Al2O3 22%;
[0106] MgO 18%;
[0107] ZnO 4%;
[0108] B2O3 4%;
[0109] (2) Mix the glass raw materials uniformly;
[0110] (3) The uniformly mixed glass raw materials are placed in a quartz crucible and heated to 1600°C in a furnace at a rate of 10°C / min to melt to obtain glass liquid, and the melting temperature is maintained for 3 hours;
[0111] (4) Pour the glass liquid into a mold preheated to 380°C for forming, then place it in an annealing furnace at 680°C for 2 hours to eliminate stress, and cool it to room temperature in the furnace to obtain the basic glass;
[0112] (5) The base glass was heated to 840°C at a rate of 5°C / min, subjected to nucleation treatment for 10 h, and then heated to 1020°C at a rate of 5°C / min, subjected to crystallization treatment for 30 min. After cooling to room temperature, a transparent magnesium aluminum silicon microcrystalline glass with high hardness and high pressure scratch fracture toughness was obtained.
[0113] like Figures 4 to 7 As shown in the figure, the transparent magnesium aluminum silicon glass-ceramics with high hardness and high indentation fracture toughness finally obtained has a Vickers hardness of 9.1 GPa, a modulus of 110.2 GPa, and an indentation fracture toughness of 1.72 MPa·m 1 / 2 , the visible light transmittance at 550nm is 86%; the main crystal phase of transparent magnesium aluminum silicon microcrystalline glass with high hardness and high pressure scratch fracture toughness is MgAl2Si3O 10 Crystal phase and cordierite crystal phase. The cordierite crystal phase is mainly distributed in MgAl2Si3O 10 Crystal phase surface, MgAl2Si3O 10 The ratio of the crystal phase to the cordierite crystal phase is 3.23:1.
[0114] like Figure 1 As shown, the amount of zinc oxide added to the base glass of Example 5 is lower, and the glass transition temperature Tg and the crystallization peak temperature are both higher than those of Example 4.
[0115] like Figure 2 As shown, the glass-ceramics of Example 5 and Example 4 are compared with the standard PDF card ( Figure 2 The vertical line below) is found to have MgAl2Si3O 10 In Example 4, the diffraction intensity of cordierite is increased compared with that in Example 5, indicating that the crystalline phase composition of the microcrystalline glass can be controlled by regulating the content of boron oxide and zinc oxide.
Claims
1. A transparent magnesium aluminum silicon glass-ceramic with high hardness and high pressure scratch fracture toughness, characterized by: The microcrystalline glass has a Vickers hardness of 7.9 GPa or more, a modulus of 104.1 GPa or more, and an indentation fracture toughness of 1.14 MPa·m 1 / 2 Above, the visible light transmittance is above 74%; The main crystalline phase of the microcrystalline glass is MgAl2Si3O 10 Crystal phase and cordierite crystal phase. The cordierite crystal phase is mainly distributed in MgAl2Si3O 10 Crystal phase surface, MgAl2Si3O 10 The ratio of crystal phase to cordierite crystal phase is 2.9~9.9:1; In terms of molar percentage, the glass raw material components of the microcrystalline glass are as follows: SiO2 46~60%; Al2O3 16~26%; MgO 13~22%; ZnO 1~10%; B2O3 1~10%; The molar ratio of ZnO to B2O3 is 1:3~3:
1.
2. The method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high high-scar fracture toughness as claimed in claim 1, characterized in that: After the glass raw materials are cast to obtain the basic glass, the basic glass is subjected to nucleation treatment and crystallization treatment in sequence to obtain the microcrystalline glass.
3. The method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness according to claim 2, characterized in that: The specific steps are as follows: (1) Mix the glass raw materials uniformly; (2) The evenly mixed glass raw materials are placed in a quartz crucible and heated up with the furnace to melt and obtain glass liquid; (3) pouring the glass liquid into a preheated mold to form it, and then placing it in an annealing furnace to anneal and eliminate stress, and obtaining the basic glass after cooling in the furnace; (4) The base glass is subjected to nucleation treatment and crystallization treatment in sequence to obtain microcrystalline glass.
4. The method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness according to claim 3, characterized in that: In step (2), the furnace heating rate is 5-10°C / min, the melting temperature is 1550-1600°C, and the melting temperature is maintained for 2-4 hours.
5. The method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness according to claim 3, characterized in that: In step (3), the preheating temperature of the mold is 350-400°C, the annealing temperature is 650-720°C, and the annealing time is 2-4h.
6. The method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness according to claim 3, characterized in that: The process of the nucleation treatment in step (4) is as follows: heating to 800-860°C at a rate of 5-10°C / min, and then performing the nucleation treatment for 8-12 hours.
7. The method for preparing a transparent magnesium aluminum silicon glass-ceramics with high hardness and high pressure scratch fracture toughness according to claim 3, characterized in that: The process of the crystallization treatment in step (4) is: heating to 980-1100°C at a rate of 4-8°C / min, and then performing the crystallization treatment for 20-60 minutes.
Citation Information
Patent Citations
High-thermal-conductivity, low-expansion and low-dielectric glass ceramic and preparation method thereof
CN112939471A