Semiconductor device and method for manufacturing the same

By forming a doped epitaxial layer on a substrate and forming an associated diffusion layer in the manufacturing of semiconductor devices, the problems of uneven diffusion and limited depth are solved, the reliability and diversity of the device are improved, and the manufacturing process is simplified.

CN118398482BActive Publication Date: 2024-10-18BEIJING CRRC TIMES HUAISHI SEMICONDUCTOR CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410823716.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-18
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The existing diffusion doping process has problems such as uneven diffusion, low repetition rate and limited diffusion depth in the manufacturing of semiconductor devices, which affects the reliability and diversity of the device structure.

Method used

By forming an epitaxial layer with doping elements on the substrate, and forming a diffusion layer in the substrate based on the diffusion source structure, the concentration of the doping elements of the diffusion layer is related to the thickness of the epitaxial layer, using a metal organic chemical vapor deposition process and high temperature Diffusion process to control the uniformity and depth of the diffusion layer.

Benefits of technology

It improves the uniformity and repeatability of the diffusion layer, simplifies the manufacturing process, enhances the structural reliability and diversity of semiconductor devices, and meets the needs of deep junction diffusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118398482B_ABST
    Figure CN118398482B_ABST
Patent Text Reader

Abstract

The present application relates to a semiconductor device and a method for manufacturing the same, wherein the method for manufacturing the semiconductor device comprises: providing a substrate; forming a diffusion source structure on the substrate, wherein the diffusion source structure comprises at least one epitaxial layer having a doping element, wherein the epitaxial layer is formed on the substrate; forming a diffusion layer in the substrate based on the diffusion source structure, wherein the doping element of the diffusion layer is the same as the doping element of the epitaxial layer, and the concentration of the doping element of the diffusion layer is related to the thickness of the diffusion source structure. The semiconductor device and the method for manufacturing the same involved in the present application improve the diffusion uniformity and consistency of the diffusion layer, and can meet the diffusion requirements of semiconductor devices for different doping elements, as well as the requirements of deep junction diffusion of semiconductor devices. The present application simplifies the manufacturing process of semiconductor devices, improves the uniformity and repeatability of the diffusion layer, and thus improves the reliability and diversity of the semiconductor device structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a semiconductor device and a manufacturing method thereof. Background Art

[0002] In recent years, as the global demand for energy conservation and emission reduction has become more urgent, the application field of power semiconductors has moved from the traditional industrial control field to many industries such as new energy and smart grid, becoming a key module of high-voltage direct current transmission technology. Among them, the preparation step of PN junction is a key process step in the production of power electronic devices, and the diffusion doping process is a common method for making PN junction.

[0003] The diffusion doping process refers to the process of moving impurity atoms in the diffusion source to a specific depth in the semiconductor through atomic gaps or substitution at high temperatures to achieve special functions. During the diffusion doping process, the uniformity of impurity distribution, diffusion junction depth, and doping concentration are key factors that determine the performance of power semiconductor devices.

[0004] The general diffusion junction technology has problems such as uneven diffusion, low repetition rate and very limited diffusion depth, which to some extent affect the reliability of semiconductor device structure, limit the diversity of semiconductor device structure and make the preparation process of semiconductor devices more complicated. Summary of the invention

[0005] Based on this, it is necessary to provide a semiconductor device and a method for manufacturing the same, so as to simplify the manufacturing process of the semiconductor device, improve the uniformity and repeatability of the diffusion layer, and improve the diversity and reliability of the semiconductor device structure.

[0006] In a first aspect, the present application provides a method for manufacturing a semiconductor device, comprising:

[0007] providing a substrate;

[0008] forming a diffusion source structure on the substrate, wherein the diffusion source structure comprises at least one epitaxial layer having a doping element, and the epitaxial layer is formed on the substrate;

[0009] A diffusion layer is formed in the substrate based on the diffusion source structure, wherein the doping element of the diffusion layer is the same as the doping element of the epitaxial layer, and the concentration of the doping element of the diffusion layer is related to the thickness of the diffusion source structure.

[0010] In one embodiment, the diffusion source structure includes at least one first epitaxial layer, and the first epitaxial layer is doped with a first doping element; wherein forming the diffusion source structure on the substrate includes:

[0011] At least one first epitaxial layer is formed on the substrate.

[0012] In one embodiment, after forming at least one first epitaxial layer on the substrate, the method for manufacturing the semiconductor device further includes:

[0013] Performing a patterning process on each of the first epitaxial layers;

[0014] The step of forming a diffusion layer in the substrate based on the diffusion source structure includes:

[0015] A diffusion layer with a wavy junction is formed in the substrate based on each of the first epitaxial layers after the patterning process.

[0016] In one embodiment, the diffusion source structure includes at least one second epitaxial layer and at least one third epitaxial layer, the second epitaxial layer is doped with a second doping element, and the third epitaxial layer is doped with a third doping element; wherein forming the diffusion source structure on the substrate includes:

[0017] forming at least one second epitaxial layer on the substrate;

[0018] At least one third epitaxial layer is formed on the second epitaxial layer.

[0019] In one embodiment, after forming at least one third epitaxial layer on the second epitaxial layer, the method for manufacturing the semiconductor device further includes:

[0020] Performing a patterning process on each of the second epitaxial layers and each of the third epitaxial layers;

[0021] The step of forming a diffusion layer in the substrate based on the diffusion source structure includes:

[0022] A diffusion layer having a wavy junction is formed in the substrate based on each of the second epitaxial layers and each of the third epitaxial layers after the patterning process, and the diffusion layer is doped with the second doping element and the third doping element.

[0023] In one embodiment, a diffusion rate of the second doping element is lower than a diffusion rate of the third doping element.

[0024] In one embodiment, the conductivity type corresponding to the second doping element is the same as the conductivity type corresponding to the third doping element.

[0025] In one embodiment, before forming a diffusion layer in the substrate based on the diffusion source structure, the method for manufacturing the semiconductor device includes:

[0026] forming a passivation layer on a surface of the diffusion source structure facing away from the substrate;

[0027] After forming a diffusion layer in the substrate based on the diffusion source structure, the method for manufacturing the semiconductor device further includes:

[0028] The passivation layer is removed.

[0029] In one embodiment, the passivation layer comprises a silicon dioxide layer; wherein the forming of the passivation layer on the surface of the diffusion source structure facing away from the substrate comprises:

[0030] The silicon dioxide layer is formed on the side of the diffusion source structure away from the substrate by a thermal oxidation growth process or a chemical vapor deposition process.

[0031] In one embodiment, before forming a diffusion layer in the substrate based on the diffusion source structure, the method for manufacturing the semiconductor device includes:

[0032] A protection layer is formed on a surface of the substrate which is away from the diffusion source structure.

[0033] In one embodiment, the protective layer includes a silicon oxide layer or a silicon nitride layer; wherein the forming of the protective layer on a surface of the substrate facing away from the diffusion source structure includes:

[0034] The silicon oxide layer or the silicon nitride layer is formed on a surface of the substrate that is away from the diffusion source structure by using a chemical vapor deposition process.

[0035] In one embodiment, forming a diffusion source structure on the substrate includes:

[0036] A diffusion source structure is formed on the substrate based on a metal organic chemical vapor deposition process using preset process parameters; wherein the preset process parameters include: process temperature, process time and reaction gas, the process temperature ranges from 900°C to 1200°C, the process time ranges from 1h to 3h, the reaction gas includes silane gas and doping gas, and the ratio of the silane gas to the doping gas ranges from 100:1 to 300:1, wherein the doping gas includes at least the doping element, and the doping gas includes at least any one of arsine trihydride, phosphine trihydride, diborane and trimethylaluminum.

[0037] In one embodiment, forming a diffusion layer in the substrate based on the diffusion source structure includes:

[0038] A diffusion layer is formed in the substrate based on the diffusion source structure and a high-temperature diffusion process using preset diffusion parameters; wherein the preset diffusion parameters include: diffusion temperature and diffusion time, the diffusion temperature ranges from 1000°C to 1280°C, and the diffusion time ranges from 5h to 90h.

[0039] In one embodiment, before forming a diffusion source structure on the substrate, the method for manufacturing the semiconductor device includes:

[0040] The substrate is pre-processed, and the pre-processing at least includes a pre-cleaning process.

[0041] In a second aspect, the present application further provides a semiconductor device, comprising:

[0042] substrate;

[0043] A diffusion source structure, the diffusion source structure comprising at least one epitaxial layer having a doping element, the epitaxial layer being located on the substrate;

[0044] A diffusion layer is located in the substrate, wherein the diffusion layer is formed based on the diffusion source structure, the doping element of the diffusion layer is the same as the doping element of the epitaxial layer, and the concentration of the doping element of the diffusion layer is related to the thickness of the diffusion source structure.

[0045] In one embodiment, the diffusion source structure includes at least one first epitaxial layer, the first epitaxial layer is doped with a first doping element, and the first epitaxial layer covers the substrate.

[0046] In one embodiment, the first epitaxial layer includes a plurality of first epitaxial structures arranged at intervals, each of the first epitaxial structures being located on the substrate; wherein,

[0047] A surface of the diffusion layer facing away from the diffusion source structure is a wave surface.

[0048] In one embodiment, the diffusion source structure includes at least one second epitaxial layer and at least one third epitaxial layer, the second epitaxial layer is doped with a second doping element, the third epitaxial layer is doped with a third doping element, the second epitaxial layer covers the substrate, and the third epitaxial layer covers the second epitaxial layer.

[0049] In one embodiment, the second epitaxial layer includes a plurality of second epitaxial structures arranged at intervals, the third epitaxial layer includes a plurality of third epitaxial structures arranged at intervals, each of the second epitaxial structures is located on the substrate, and each of the third epitaxial structures is located on the second epitaxial structure; wherein,

[0050] A surface of the diffusion layer facing away from the diffusion source structure is a wave surface.

[0051] In one embodiment, the conductivity type corresponding to the second doping element is the same as the conductivity type corresponding to the third doping element.

[0052] In one embodiment, a diffusion rate of the second doping element is lower than a diffusion rate of the third doping element.

[0053] In one embodiment, the thickness of the epitaxial layer ranges from 0.5 μm to 10 μm.

[0054] In one embodiment, the diffusion layer has a thickness ranging from 1 μm to 180 μm.

[0055] In one embodiment, the impurity diffusion concentration of the diffusion layer ranges from 10 15 cm -3 ~10 22 cm -3 .

[0056] In one embodiment, the semiconductor device further includes:

[0057] The protective layer is located on a surface of the substrate that is away from the diffusion source structure.

[0058] In a third aspect, the present application also provides a semiconductor device manufactured using the semiconductor device manufacturing method.

[0059] The semiconductor device and the manufacturing method thereof provided by the embodiment of the present application can improve the diffusion uniformity and consistency of the diffusion layer by forming a diffusion source structure on the substrate, can meet the diffusion requirements of different doping elements by forming at least one epitaxial layer with doping elements in the diffusion source structure and forming the diffusion layer based on the diffusion source structure, and can meet the requirements of deep junction diffusion of the semiconductor device by making the concentration of the doping elements of the diffusion layer related to the thickness of the diffusion source structure. Therefore, the manufacturing process of the semiconductor device can be simplified by the above method, the uniformity and repeatability of the diffusion layer can be improved, and the reliability and diversity of the semiconductor device structure can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0061] Figure 1 A flowchart of a method for manufacturing a semiconductor device provided in one embodiment of the present application.

[0062] Figure 2 A schematic structural diagram of a step of providing a substrate in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0063] Figure 3 A schematic structural diagram of a step of forming a diffusion source structure on a substrate in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0064] Figure 4 A schematic structural diagram of a step of forming a diffusion layer in a substrate based on a diffusion source structure in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0065] Figure 5 A schematic structural diagram of the steps of forming a diffusion source structure on a substrate and performing patterning in a method for manufacturing a semiconductor device provided in one embodiment of the present application.

[0066] Figure 6 A structural schematic diagram of a step of forming a diffusion layer in a substrate based on a patterned diffusion source structure in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0067] Figure 7 A schematic structural diagram of a step of forming a diffusion source structure on a substrate in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0068] Figure 8 A schematic structural diagram of a step of forming a diffusion layer in a substrate based on a diffusion source structure in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0069] Fig. 9 A schematic structural diagram of a step of forming a diffusion source structure on a substrate in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0070] Fig.10 A structural schematic diagram of a step of forming a diffusion layer in a substrate based on a patterned diffusion source structure in a method for manufacturing a semiconductor device provided in an embodiment of the present application.

[0071] Explanation of the reference numerals: 100 - substrate; 101 - protective layer; 102 - diffusion layer; 110 - diffusion source structure; 111 - first epitaxial layer; 112 - second epitaxial layer; 113 - third epitaxial layer; 120 - passivation layer; X1 - first epitaxial structure; X2 - second epitaxial structure; X3 - third epitaxial structure. DETAILED DESCRIPTION

[0072] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0073] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0074] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present invention, the first element, component, region, layer, doping type or portion discussed below may be represented as a second element, component, region, layer or portion; for example, the first doping type may be referred to as the second doping type, and similarly, the second doping type may be referred to as the first doping type; the first doping type and the second doping type are different doping types, for example, the first doping type may be P-type and the second doping type may be N-type, or the first doping type may be N-type and the second doping type may be P-type.

[0075] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.

[0076] When used herein, the singular forms "a", "an" and " / the" may also include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include / comprise" or "have" and the like specify the presence of stated features, wholes, steps, operations, components, parts or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, wholes, steps, operations, components, parts or combinations thereof. At the same time, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.

[0077] In the diffusion bonding technology, the gas diffusion source process and the liquid diffusion source process are the most widely used. The aforementioned process generally includes pre-deposition of the diffusion source on the substrate to form a glass body with extremely high impurity concentration (such as phosphosilicate glass or borosilicate glass), and diffusion in a constant source manner at high temperature. The gas diffusion source process and the liquid diffusion source process have the advantages of simple equipment, convenient operation and easy large-scale production, but due to their inherent diffusion mode, they also face problems such as uneven surface diffusion and low repetition rate. At the same time, gaseous diffusion sources and liquid diffusion sources usually use highly toxic and explosive substances for diffusion, which poses certain safety hazards.

[0078] Compared with gas diffusion sources and liquid diffusion sources, solid diffusion sources have unique advantages in terms of uniformity and repetition rate. Solid diffusion sources can adjust the junction depth and doping concentration of the PN junction by regulating the amount of impurities doped in the solid diffusion source, and have fewer defects and are safe and non-toxic.

[0079] There are mainly two types of solid diffusion sources: one is to directly introduce a solid doping source (such as sheet-like boron nitride ceramic glass) close to the surface of the wafer, so that the solid diffusion source and the substrate are in contact with each other or maintain a specific distance, and the elements in the solid diffusion source silicon wafer are diffused into the substrate at high temperature. However, this type of solid diffusion source is in the form of a sheet and has a small diameter, which makes it difficult to accommodate the uniform diffusion of large-area wafers of 6 inches and above, and it is easy to warp at high temperatures, thus affecting the uniformity of diffusion and mass production. In addition, since the oxide layer on the surface of the sheet-like solid diffusion source is gradually consumed during the diffusion process, it will cause the loss of doping elements and affect the uniformity of diffusion. Therefore, the solid diffusion source needs to be activated after a period of diffusion.

[0080] Another solid-state diffusion source is the doped epitaxial layer grown directly onto the substrate, such as the zinc oxide film deposited by magnetron sputtering for the PN junction of solar cells. The uniformity and consistency of the element diffusion process are good, and the magnetron sputtering process at a lower temperature avoids the problem of premature diffusion of zinc atoms caused by high-temperature epitaxy. However, due to the limitations of the magnetron sputtering process, the thickness of the epitaxial film formed by the above process is very limited, and it is difficult to meet the requirements of power semiconductor devices for deep junction diffusion (the diffusion depth often reaches tens of microns). In addition, the epitaxial film deposited by magnetron sputtering is usually lightly doped, which is difficult to meet the continuous and sufficient doping requirements of impurity elements.

[0081] In view of this, the present application provides a method for manufacturing a semiconductor device to simplify the manufacturing process of the semiconductor device, improve the uniformity and repeatability of the diffusion layer, and thus improve the reliability and diversity of the semiconductor device structure.

[0082] Figure 1 A flowchart of a method for manufacturing a semiconductor device according to an embodiment of the present application. Figure 1 In one embodiment, the present application provides a method for manufacturing a semiconductor device, including the following contents.

[0083] Step S110: providing a substrate.

[0084] For example, see Figure 2 The substrate 100 is a silicon substrate. Optionally, the material of the substrate 100 may also be at least one of silicon carbide (SiC), gallium nitride (GaN) and gallium arsenide (GaAs).

[0085] Exemplarily, the substrate 100 may be pre-processed. The pre-processing includes at least a pre-cleaning process. Preferably, the substrate 100 is pre-cleaned by using an RCA cleaning process to remove particles or organic pollutants on the surface of the substrate 100.

[0086] Step S120: forming a diffusion source structure on the substrate, wherein the diffusion source structure includes at least one epitaxial layer having doping elements, and the epitaxial layer is formed on the substrate.

[0087] For example, see Figure 3 , forming a diffusion source structure 110 on a substrate 100, the diffusion source structure 110 including at least one epitaxial layer (for example, a first epitaxial layer 111) having doping elements, including: using preset process parameters, based on metal-organic chemical vapor deposition (MOCVD) technology, forming the diffusion source structure 110 on the substrate 100; wherein the preset process parameters include: process temperature, process time and reaction gas, the process temperature range includes 900°C~1200°C, the process time range includes 1h~3h, the reaction gas includes silane gas and doping gas, and the ratio of silane gas to doping gas ranges from 100:1 to 300:1, wherein the doping gas includes at least the doping element of the epitaxial layer. Optionally, the doping gas includes at least any one of arsine trihydride, phosphine trihydride, diborane and trimethylaluminum.

[0088] Specifically, the MOCVD process includes: introducing silane gas into a MOCVD high temperature furnace, depositing a uniform epitaxial layer (e.g., depositing the first epitaxial layer 111) on the surface of the substrate 100 at a high temperature (i.e., 900°C to 1200°C), and releasing hydrogen. During the reaction, the doping gas is injected into the reaction chamber to dope the epitaxial single crystal silicon while the epitaxial layer (e.g., the first epitaxial layer 111) is growing. At a high temperature (i.e., 900-1200°C), the thickness of the epitaxial layer (e.g., depositing the first epitaxial layer 111) is adjusted by adjusting the deposition time (e.g., 1h to 3h) (e.g., the thickness range is 0.5μm to 10μm) to adjust the thickness of the diffusion source structure 110, thereby adjusting the doping amount of impurity elements in the diffusion source structure 110. During the MOCVD process, several silicon wafers can be stacked in the high temperature furnace, thereby realizing mass production and improving production efficiency.

[0089] Optionally, a low-pressure chemical vapor deposition (LPCVD) process may be used to form the epitaxial layer. The relevant process parameters are the same as those of the MOCVD process. Those skilled in the art may also adaptively adjust the process parameters according to the process requirements, or use other process methods to form the epitaxial layer.

[0090] Step S130: forming a diffusion layer in the substrate based on the diffusion source structure, wherein the doping element of the diffusion layer is the same as the doping element of the epitaxial layer, and the concentration of the doping element of the diffusion layer is related to the thickness of the diffusion source structure.

[0091] For example, see Figure 4 , using preset diffusion parameters, based on high temperature diffusion process, based on the diffusion source structure 110, a diffusion layer 102 is formed in the substrate 100; wherein the preset diffusion parameters include: diffusion temperature and diffusion time, the diffusion temperature range includes 1000℃~1280℃, and the diffusion time range includes 5h~90h. At this time, a PN junction is formed at the junction of the diffusion layer 102 and the substrate 100. Preferably, the thickness of the diffusion layer 102 ranges from 1μm to 180μm. Preferably, the impurity diffusion concentration of the diffusion layer 102 ranges from 10 15 cm -3 ~10 22 cm -3 .

[0092] Exemplarily, the process of forming the diffusion layer 102 in the substrate 100 based on the diffusion source structure 110 includes: placing the substrate 100 in a high-temperature diffusion furnace, and continuously diffusing at a high temperature (i.e., 1000° C. to 1280° C.), so that the doping elements in the epitaxial layer (e.g., the first epitaxial layer 111) diffuse into the substrate 100 under vacuum or inert gas protection, and by adjusting the diffusion time (e.g., 5 h to 90 h) or adjusting the set thickness of the epitaxial layer (e.g., the first epitaxial layer 111) (the total amount of doping in the diffusion source structure is positively correlated with the set thickness), achieving impurity diffusion of different junction depths (e.g., 1 μm to 180 μm) or achieving different impurity diffusion concentrations (e.g., 10 15 cm -3 ~10 22 cm -3 ). Optionally, the thickness range includes 0.5 μm to 10 μm.

[0093] It should be noted that due to Figure 4 The thickness of the diffusion source structure 110 is equal to the thickness of the epitaxial layer (ie, the first epitaxial layer 111), so it can be adjusted directly according to the set thickness of the epitaxial layer. In other embodiments, the thickness of the diffusion source structure 110 is the sum of the thicknesses of all film layers in the diffusion source structure.

[0094] The manufacturing method of a semiconductor device provided by an embodiment of the present application can improve the diffusion uniformity and consistency of the diffusion layer by forming a diffusion source structure on the substrate, and can meet the diffusion requirements of different doping elements by forming at least one epitaxial layer with doping elements in the diffusion source structure and forming a diffusion layer based on the diffusion source structure, and can meet the requirements of deep junction diffusion of the semiconductor device by making the concentration of the doping elements in the diffusion layer related to the thickness of the diffusion source structure. Therefore, the above method can simplify the manufacturing process of the semiconductor device, improve the uniformity and repeatability of the diffusion layer, and thus improve the reliability and diversity of the semiconductor device structure.

[0095] Continue reading Figure 2 In one embodiment of the present application, a diffusion layer of a specific thickness (or a specific doping element concentration) can be formed according to the process requirements by using the relationship between the diffusion concentration formula of the substrate 100 and the thickness of the epitaxial layer in the diffusion source formed subsequently. The diffusion concentration formula of the finite surface source in the silicon substrate 100 is as follows:

[0096] .

[0097] in, represents the impurity concentration, represents the vertical distance from the surface of the substrate (i.e., diffusion thickness), represents the diffusion time, represents the diffusion coefficient, Indicates the total amount of doping.

[0098] Combined with the diffusion concentration formula of the substrate 100, it can be known that the total amount of doping can be controlled by adjusting the thickness of the epitaxial layer formed subsequently. As the thickness of the epitaxial layer increases (i.e. the total amount of doping With the increase of the thickness of the epitaxial layer, the concentration of the doping element (ie, the impurity concentration) of the diffusion layer at a specific depth of the substrate 100 is correspondingly increased, so that the concentration of the doping element of the diffusion layer can be flexibly controlled by the thickness of the epitaxial layer.

[0099] For example, see Figure 3 In one embodiment, the diffusion source structure 110 includes at least one first epitaxial layer 111, and the first epitaxial layer 111 is doped with a first doping element. Specifically, forming the diffusion source structure 110 on the substrate 100 includes: forming at least one first epitaxial layer 111 on the substrate 100. Optionally, the set thickness of the first epitaxial layer 111 ranges from 0.5 μm to 10 μm.

[0100] Continue reading Figure 3 In one embodiment, the method for manufacturing a semiconductor device further includes: forming a passivation layer 120 on a surface of the diffusion source structure 110 facing away from the substrate 100 to prevent the doping elements in the first epitaxial layer 111 from being precipitated in advance during the subsequent diffusion process, thereby affecting the diffusion uniformity. Optionally, the passivation layer 120 includes a silicon dioxide layer, and the silicon dioxide layer is formed on the side of the diffusion source structure 110 facing away from the substrate 100 by a thermal oxidation growth process or a chemical vapor deposition process.

[0101] Continue reading Figure 3In one embodiment, the method for manufacturing a semiconductor device further includes: forming a protective layer 101 on a surface of the substrate 100 that is away from the diffusion source structure 110 to prevent the back side of the substrate 100 (i.e., the surface of the substrate 100 that is away from the diffusion source structure 110) from being corroded. Optionally, the protective layer 101 includes a silicon oxide layer or a silicon nitride layer. Preferably, a chemical vapor deposition process is used to form a silicon oxide layer or a silicon nitride layer on a surface of the substrate 100 that is away from the diffusion source structure 110.

[0102] See also Figure 4 After forming the diffusion layer 102 in the substrate 100 based on the diffusion source structure 110, the method for manufacturing the semiconductor device further includes: removing the passivation layer 120. Optionally, the passivation layer 120 is removed using hydrofluoric acid.

[0103] In one embodiment, after forming a diffusion layer in the substrate based on the diffusion source structure, the method for manufacturing a semiconductor device may further include: removing the diffusion source structure to facilitate subsequent process flow (not shown in the figure). Optionally, wet etching may be used to remove the diffusion source structure, and the cleaning agent for the wet etching includes hydrofluoric acid and nitric acid.

[0104] See also Figure 5 In one embodiment, after forming at least one first epitaxial layer 111 on the substrate 100, the method for manufacturing a semiconductor device further includes: patterning each first epitaxial layer 111 (for example, the patterned first epitaxial layer 111 includes a first epitaxial structure X1). Optionally, a passivation layer 120 is formed on the diffusion source structure 110 to prevent the first doping element in the first epitaxial layer 111 from precipitating.

[0105] Exemplarily, each first epitaxial layer 111 is patterned, including: forming a mask (not shown in the figure) on the first epitaxial layer 111, sequentially performing exposure, development, water washing, drying and other processes, and then using dry etching or wet etching to form a patterned first epitaxial layer 111; removing the mask by hydrofluoric acid. Optionally, if there is a passivation layer 120 on the first epitaxial layer, a mask is formed on the passivation layer 120.

[0106] Accordingly, see Figure 6 After patterning each first epitaxial layer 111, a diffusion layer 102 having a wavy junction is formed in the substrate 100 based on the diffusion source structure 110. Figure 4 The difference between the diffusion layer 102 and the Figure 6The diffusion layer 102 in the substrate 100 is diffused based on the patterned first epitaxial layer 111, so the thickness of the portion of the diffusion layer 102 covered by the patterned first epitaxial layer 111 is greater than the thickness of the portion of the diffusion layer 102 not covered by the patterned first epitaxial layer 111, so that the bottom of the diffusion layer 102 is wavy. At this time, a wavy junction (i.e., a wavy PN junction, not marked in the figure) is formed at the junction of the diffusion layer 102 and the substrate 100.

[0107] Continue reading Figure 6 After forming the diffusion layer 102 in the substrate 100 based on the diffusion source structure 110 , the method for manufacturing the semiconductor device may further include: removing the passivation layer 120 .

[0108] Optionally, the method for manufacturing a semiconductor device may further include: removing the diffusion source structure to facilitate subsequent process flow (e.g., preparing other semiconductor structures on the surface of the diffusion layer away from the substrate). Optionally, the diffusion source structure may be removed by a planarization method, such as by a chemical mechanical polishing process.

[0109] See also Figure 2 and Figure 7 In one embodiment, a diffusion source structure 110 is formed on a substrate 100. The diffusion source structure 110 includes at least one second epitaxial layer 112 and at least one third epitaxial layer 113. The second epitaxial layer 112 is doped with a second doping element, and the third epitaxial layer 113 is doped with a third doping element.

[0110] Exemplarily, forming a diffusion source junction 110 on a substrate 100 includes: forming at least one second epitaxial layer 112 on the substrate 100; and forming at least one third epitaxial layer 113 on the second epitaxial layer 112. Preferably, the conductivity type corresponding to the second doping element is the same as the conductivity type corresponding to the third doping element, and the diffusion speed of the second doping element is lower than the diffusion speed of the third doping element, so as to prevent the second doping element in the second epitaxial layer 112 and the third doping element in the third epitaxial layer 113 from being precipitated in advance in the subsequent diffusion process, thereby affecting the uniformity of diffusion.

[0111] Then, see Figure 8 , a diffusion layer 102 is formed in the substrate 100 based on the diffusion source structure 110. The formation process of the diffusion layer 102 has been described above and will not be repeated here.

[0112] See also Figure 7 and Fig. 9In one embodiment, after forming at least one third epitaxial layer 113 on the second epitaxial layer 112, the method for manufacturing a semiconductor device further includes: performing a patterning process on each second epitaxial layer 112 and each third epitaxial layer 113 (for example, the second epitaxial layer 112 after the patterning process includes a second epitaxial structure X2, and the third epitaxial layer 113 after the patterning process includes a third epitaxial structure X3). The specific patterning process is similar to the process of performing a patterning process on each first epitaxial layer 111, and will not be described in detail herein.

[0113] Next, see Fig.10 , a diffusion layer 102 is formed in the substrate 100 based on the diffusion source structure 110, including: a diffusion layer 102 with a wavy junction is formed in the substrate based on each second epitaxial layer 112 and each third epitaxial layer 113 after patterning, and the diffusion layer 102 is doped with a second doping element and a third doping element.

[0114] A method for manufacturing a semiconductor device provided in an embodiment of the present application forms an epitaxial layer with a specific thickness on a substrate through MOCVD to prepare a uniform diffusion layer, thereby improving the diffusion uniformity and the repeatability of the diffusion process; the thickness range of the formed epitaxial layer is relatively large, so as to realize heavily doped epitaxy and deep junction diffusion doping for high-power semiconductor devices.

[0115] In addition, in the manufacturing method of the semiconductor device provided in one embodiment of the present application, the set thickness of the epitaxial layer can be set according to actual needs, so that doping structures with different junction depths and PN junctions with different doping concentrations can be prepared more flexibly. At the same time, the graphic processing of the epitaxial layer can achieve high-concentration doping at specific positions in the substrate, thereby completing the preparation of some complex structures, such as the development of a single-element wavy junction (i.e., a wavy PN junction corresponding to a diffusion layer containing only one doping element) or a double-element wavy junction (i.e., a wavy PN junction corresponding to a diffusion layer containing two doping elements).

[0116] Furthermore, the manufacturing method of the semiconductor device provided by the present application simplifies the core process steps of diffusion bonding, improves the stability, accuracy, controllability of the process and the consistency of the performance of the semiconductor device, thereby improving the preparation yield of the semiconductor device. In addition, the manufacturing method of the semiconductor device provided by the present application can provide solutions or technical inspiration for more types of semiconductor graphic structures, thereby greatly improving the electrical, thermal, mechanical and other properties of the semiconductor device.

[0117] Please continue to refer to Figure 4The present application also provides a semiconductor device, including: a substrate 100, a diffusion source structure 110 and a diffusion layer 102. The diffusion source structure 110 includes at least one epitaxial layer (for example, a first epitaxial layer 111) having a doping element, and the epitaxial layer is located on the substrate 100; the diffusion layer 102 is located in the substrate 100, wherein the diffusion layer 102 is formed based on the diffusion source structure 110, the doping element of the diffusion layer 102 is the same as the doping element of the epitaxial layer (for example, the first epitaxial layer 111), and the concentration of the doping element of the diffusion layer 102 is related to the thickness of the diffusion source structure 110.

[0118] The semiconductor device provided by an embodiment of the present application improves the diffusion uniformity and consistency of the diffusion layer by arranging a diffusion source structure on the substrate, and can meet the diffusion requirements of different doping elements by arranging at least one epitaxial layer with doping elements in the diffusion source structure and arranging a diffusion layer formed based on the diffusion source structure; and can meet the requirements of deep junction diffusion of the semiconductor device by arranging the concentration of the doping elements of the diffusion layer to be related to the thickness of the diffusion source structure. Therefore, the semiconductor device has excellent reliability and diversity, and the diffusion layer in the semiconductor device has excellent uniformity and repeatability.

[0119] Continue reading Figure 4 In one embodiment, the diffusion source structure 110 includes at least one first epitaxial layer 111, the first epitaxial layer 111 is doped with a first doping element, and the first epitaxial layer 111 covers the substrate 100. Optionally, the first epitaxial layer 111 has a set thickness, and the set thickness range includes 0.5μm~10μm. Optionally, the thickness range of the diffusion layer 102 includes 1μm~180μm, and the impurity diffusion concentration range of the diffusion layer 102 includes 10 15 cm -3 ~10 22 cm -3 .

[0120] For example, Figure 4 The semiconductor device shown further includes a PN junction (not shown in the figure), a protective layer 101 and a passivation layer 120, wherein the PN junction is located at the junction of the diffusion layer 102 and the substrate 100, the protective layer 101 is located on the surface of the substrate 100 facing away from the diffusion source structure 110; the passivation layer 120 is located on the surface of the diffusion source structure 110 facing away from the substrate 100, and the passivation layer 120 is located on the first epitaxial layer 111 ( Figure 4 The passivation layer has been removed. The specific location can be found in Figure 3 ).

[0121] See also Figure 6In one embodiment, the first epitaxial layer 111 includes a plurality of first epitaxial structures X1 arranged at intervals, each of which is located on the substrate 100; wherein the surface of the diffusion layer 102 facing away from the diffusion source structure 110 is a wavy surface. At this time, the PN junction at the junction of the diffusion layer 102 and the substrate 100 is a wavy junction.

[0122] See also Figure 8 In one embodiment, the diffusion source structure 110 includes at least one second epitaxial layer 112 and at least one third epitaxial layer 113, the second epitaxial layer 112 is doped with a second doping element, the third epitaxial layer 113 is doped with a third doping element, and the second epitaxial layer 112 covers the substrate 100, and the third epitaxial layer 113 covers the second epitaxial layer 112.

[0123] Preferably, the conductivity type corresponding to the second doping element is the same as the conductivity type corresponding to the third doping element, and the diffusion rate of the second doping element is less than the diffusion rate of the third doping element. Optionally, the diffusion source structure 110 has a set thickness, and the range of the set thickness includes 0.5μm~10μm. In other embodiments, the thickness of the second epitaxial layer 112 and the third epitaxial layer 113 can also be set separately, then the thickness of the diffusion source structure 110 is the sum of the thickness of all the second epitaxial layers 112 and all the third epitaxial layers 113. Optionally, the thickness range of the diffusion layer 102 includes 1μm~180μm, and the range of the impurity diffusion concentration of the diffusion layer 102 includes 10 15 cm -3 ~10 22 cm -3 .

[0124] For example, Figure 8 The semiconductor device shown further includes a PN junction (not shown in the figure), a protective layer 101 and a passivation layer 120, wherein the PN junction is located at the junction of the diffusion layer 102 and the substrate 100, the protective layer 101 is located on the surface of the substrate 100 facing away from the diffusion source structure 110, the passivation layer 120 is located on the surface of the diffusion source structure 110 facing away from the substrate 100, and the passivation layer 120 is located on the third epitaxial layer 113 ( Figure 8 The passivation layer has been removed. The specific location can be found in Figure 7 ).

[0125] See also Fig.10In one embodiment, the second epitaxial layer 112 includes a plurality of second epitaxial structures X2 arranged at intervals, the third epitaxial layer 113 includes a plurality of third epitaxial structures X3 arranged at intervals, each second epitaxial structure X2 is located on the substrate 100, and each third epitaxial structure X3 is located on the second epitaxial structure X2; wherein the surface of the diffusion layer 102 facing away from the diffusion source structure 110 is a wavy surface. At this time, the PN junction at the junction of the diffusion layer 102 and the substrate 100 is a wavy junction.

[0126] In one embodiment, the semiconductor device provided in the present application is prepared by the manufacturing method of the semiconductor device provided in the present application. Exemplarily, the semiconductor device provided in the present application can be an integrated gate-commutated thyristor (IGCT device), an insulated gate bipolar transistor (IGBT device) or a gate turn-off thyristor (GTO), or other power semiconductor devices, or other semiconductor devices with the same or similar structures, and the present application does not limit this.

[0127] The semiconductor device and the manufacturing method thereof provided by the embodiment of the present application can improve the diffusion uniformity and consistency of the diffusion layer by forming a diffusion source structure on the substrate, can meet the diffusion requirements of different doping elements by forming at least one epitaxial layer with doping elements in the diffusion source structure and forming the diffusion layer based on the diffusion source structure, and can meet the requirements of deep junction diffusion of the semiconductor device by making the concentration of the doping elements of the diffusion layer related to the thickness of the diffusion source structure. Therefore, the manufacturing process of the semiconductor device can be simplified by the above method, the uniformity and repeatability of the diffusion layer can be improved, and the reliability and diversity of the semiconductor device structure can be improved.

[0128] It should be understood that, although the steps in the above-mentioned flowcharts are shown in sequence according to the diagrams, these steps are not necessarily executed in sequence according to the order shown in the diagrams. Unless there is a clear description in this article, the execution of these steps is not strictly limited in order, and these steps can be executed in other orders. Moreover, at least a part of the steps in each figure may include multiple steps or multiple stages, and these steps or stages are not necessarily executed at the same time, but can be executed at different times, and the execution order of these steps or stages is not necessarily to be carried out in sequence, but can be executed in turn or alternately with other steps or at least a part of the steps or stages in other steps.

[0129] In the description of this specification, the description with reference to the terms "some embodiments", "other embodiments", "ideal embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic descriptions of the above terms do not necessarily refer to the same embodiment or example.

[0130] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features of the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0131] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for manufacturing a semiconductor device, characterized in that: include: providing a substrate; forming a diffusion source structure on the substrate, wherein the diffusion source structure comprises at least one epitaxial layer having a doping element, and the epitaxial layer is formed on the substrate; Based on the epitaxial layer of the diffusion source structure, a diffusion layer is formed in the substrate, wherein the doping element of the diffusion layer is the same as the doping element of the epitaxial layer, the concentration of the doping element of the diffusion layer is related to the thickness of the diffusion source structure, and the concentration of the doping element of the diffusion layer is controlled by adjusting the thickness of the epitaxial layer in the diffusion source structure in combination with the diffusion concentration formula of the substrate; Wherein, the diffusion concentration formula is as follows: ; in, represents the concentration of the doping element, represents the vertical distance from the surface of the substrate, represents the diffusion time, represents the diffusion coefficient, Indicates the total amount of doping.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The diffusion source structure includes at least one first epitaxial layer, and the first epitaxial layer is doped with a first doping element; wherein forming the diffusion source structure on the substrate includes: At least one first epitaxial layer is formed on the substrate.

3. The method for manufacturing a semiconductor device according to claim 2, wherein: After forming at least one first epitaxial layer on the substrate, the method for manufacturing the semiconductor device further includes: Performing a patterning process on each of the first epitaxial layers; The step of forming a diffusion layer in the substrate based on the diffusion source structure includes: A diffusion layer with a wavy junction is formed in the substrate based on each of the first epitaxial layers after the patterning process.

4. The method for manufacturing a semiconductor device according to claim 1, wherein: The diffusion source structure includes at least one second epitaxial layer and at least one third epitaxial layer, the second epitaxial layer is doped with a second doping element, and the third epitaxial layer is doped with a third doping element; wherein forming the diffusion source structure on the substrate includes: forming at least one second epitaxial layer on the substrate; At least one third epitaxial layer is formed on the second epitaxial layer.

5. The method for manufacturing a semiconductor device according to claim 4, wherein: After forming at least one third epitaxial layer on the second epitaxial layer, the method for manufacturing the semiconductor device further includes: Performing a patterning process on each of the second epitaxial layers and each of the third epitaxial layers; The step of forming a diffusion layer in the substrate based on the diffusion source structure includes: A diffusion layer having a wavy junction is formed in the substrate based on each of the second epitaxial layers and each of the third epitaxial layers after the patterning process, and the diffusion layer is doped with the second doping element and the third doping element.

6. The method for manufacturing a semiconductor device according to claim 4, wherein: A diffusion speed of the second doping element is lower than a diffusion speed of the third doping element.

7. The method for manufacturing a semiconductor device according to claim 4, wherein: The conductivity type corresponding to the second doping element is the same as the conductivity type corresponding to the third doping element.

8. The method for manufacturing a semiconductor device according to claim 1, wherein: Before forming a diffusion layer in the substrate based on the diffusion source structure, the method for manufacturing the semiconductor device includes: forming a passivation layer on a surface of the diffusion source structure facing away from the substrate; After forming a diffusion layer in the substrate based on the diffusion source structure, the method for manufacturing the semiconductor device further includes: The passivation layer is removed.

9. The method for manufacturing a semiconductor device according to claim 8, wherein: The passivation layer includes a silicon dioxide layer; wherein the passivation layer is formed on a surface of the diffusion source structure facing away from the substrate, comprising: The silicon dioxide layer is formed on the side of the diffusion source structure away from the substrate by a thermal oxidation growth process or a chemical vapor deposition process.

10. The method for manufacturing a semiconductor device according to claim 1, wherein: Before forming a diffusion layer in the substrate based on the diffusion source structure, the method for manufacturing the semiconductor device includes: A protection layer is formed on a surface of the substrate which is away from the diffusion source structure.

11. The method for manufacturing a semiconductor device according to claim 10, wherein: The protective layer comprises a silicon oxide layer or a silicon nitride layer; wherein the protective layer is formed on a surface of the substrate facing away from the diffusion source structure, comprising: The silicon oxide layer or the silicon nitride layer is formed on a surface of the substrate that is away from the diffusion source structure by using a chemical vapor deposition process.

12. The method for manufacturing a semiconductor device according to claim 1, wherein: The step of forming a diffusion source structure on the substrate comprises: A diffusion source structure is formed on the substrate based on a metal organic chemical vapor deposition process using preset process parameters; wherein the preset process parameters include: process temperature, process time and reaction gas, the process temperature ranges from 900°C to 1200°C, the process time ranges from 1h to 3h, the reaction gas includes silane gas and doping gas, and the ratio of the silane gas to the doping gas ranges from 100:1 to 300:1, wherein the doping gas includes at least the doping element, and the doping gas includes at least any one of arsine trihydride, phosphine trihydride, diborane and trimethylaluminum.

13. The method for manufacturing a semiconductor device according to claim 1, wherein: The step of forming a diffusion layer in the substrate based on the diffusion source structure includes: A diffusion layer is formed in the substrate based on the diffusion source structure and a high-temperature diffusion process using preset diffusion parameters; wherein the preset diffusion parameters include: diffusion temperature and diffusion time, the diffusion temperature ranges from 1000°C to 1280°C, and the diffusion time ranges from 5h to 90h.

14. The method for manufacturing a semiconductor device according to claim 1, wherein: Before forming the diffusion source structure on the substrate, the method for manufacturing the semiconductor device includes: The substrate is pre-processed, and the pre-processing at least includes a pre-cleaning process.

15. A semiconductor device, characterized in that: include: substrate; A diffusion source structure, the diffusion source structure comprising at least one epitaxial layer having a doping element, the epitaxial layer being located on the substrate; A diffusion layer, the diffusion layer is located in the substrate, wherein the diffusion layer is formed based on the diffusion source structure, the doping element of the diffusion layer is the same as the doping element of the epitaxial layer, the concentration of the doping element of the diffusion layer is related to the thickness of the diffusion source structure, and the concentration of the doping element of the diffusion layer is controlled by adjusting the thickness of the epitaxial layer in the diffusion source structure in combination with the diffusion concentration formula of the substrate; Wherein, the diffusion concentration formula is as follows: ; in, represents the concentration of the doping element, represents the vertical distance from the surface of the substrate, represents the diffusion time, represents the diffusion coefficient, Indicates the total amount of doping.

16. The semiconductor device according to claim 15, characterized in that The diffusion source structure includes at least one first epitaxial layer, the first epitaxial layer is doped with a first doping element, and the first epitaxial layer covers the substrate.

17. The semiconductor device according to claim 16, characterized in that The first epitaxial layer includes a plurality of first epitaxial structures arranged at intervals, each of the first epitaxial structures being located on the substrate; wherein, A surface of the diffusion layer facing away from the diffusion source structure is a wave surface.

18. The semiconductor device according to claim 15, characterized in that The diffusion source structure includes at least one second epitaxial layer and at least one third epitaxial layer, the second epitaxial layer is doped with a second doping element, the third epitaxial layer is doped with a third doping element, the second epitaxial layer covers the substrate, and the third epitaxial layer covers the second epitaxial layer.

19. The semiconductor device according to claim 18, characterized in that The second epitaxial layer includes a plurality of second epitaxial structures arranged at intervals, the third epitaxial layer includes a plurality of third epitaxial structures arranged at intervals, each of the second epitaxial structures is located on the substrate, and each of the third epitaxial structures is located on the second epitaxial structures; wherein, A surface of the diffusion layer facing away from the diffusion source structure is a wave surface.

20. The semiconductor device according to claim 18, wherein: The conductivity type corresponding to the second doping element is the same as the conductivity type corresponding to the third doping element.

21. The semiconductor device according to claim 18, wherein: A diffusion speed of the second doping element is lower than a diffusion speed of the third doping element.

22. The semiconductor device according to claim 15, characterized in that The thickness of the epitaxial layer ranges from 0.5 μm to 10 μm.

23. The semiconductor device according to claim 15, characterized in that The diffusion layer has a thickness ranging from 1 μm to 180 μm.

24. The semiconductor device according to claim 15, characterized in that The impurity diffusion concentration of the diffusion layer ranges from 10 15 cm -3 ~10 22 cm -3 .

25. The semiconductor device according to claim 15, characterized in that The semiconductor device further comprises: The protective layer is located on a surface of the substrate that is away from the diffusion source structure.

26. A semiconductor device, characterized in that: The semiconductor device is manufactured by the method for manufacturing a semiconductor device according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Formation method of deep PN junction and semiconductor device with deep PN junction

    CN104392907A

  • Method for preparing doped silicon of solar battery with low temperature vapor deposited solid diffusion source

    CN105702809A

  • Impurity diffusion method, solar cell and manufacturing method thereof

    CN116994945A