A Fe-W 18 O 49 / NH2-MIL-125 (Ti) composite photocatalyst and its preparation method and application in nitrogen fixation

By constructing Fe-W18O49/NH2-MIL-125(Ti) composite photocatalyst, the problem of low ammonia generation rate of Fe-W18O49 in the photocatalytic nitrogen fixation reaction was solved, and efficient photocatalytic nitrogen fixation activity and stability were achieved. The generation rate is significantly improved.

CN118416951BActive Publication Date: 2024-10-18JILIN TEACHERS INST OF ENG & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311214652.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-20
Publication Date
2024-10-18
Estimated Expiration
2043-09-20

AI Technical Summary

Technical Problem

The ammonia generation rate of Fe-W18O49 in the photocatalytic nitrogen fixation reaction is low, and there are problems such as low light energy utilization, slow charge transfer, and rapid carrier recombination, resulting in low nitrogen fixation reaction efficiency.

Method used

Construct Fe-W18O49/NH2-MIL-125(Ti) composite photocatalyst. Fe-W18O49 nanowires are uniformly loaded on the surface of NH2-MIL-125(Ti) metal organic framework material to form a composite catalyst and change the carrier distribution. migration path, expand the light absorption range, promote the separation of photogenerated electrons and holes, and improve the nitrogen fixation reaction efficiency.

Benefits of technology

The photocatalytic nitrogen fixation activity is significantly improved, and the ammonia generation rate reaches 128.2 μmol·g-1·h-1. The composite catalyst has good stability, and the generation rate does not change significantly after multiple cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118416951B_ABST
    Figure CN118416951B_ABST
Patent Text Reader

Abstract

The present invention provides a Fe-W 18 O 49 / NH2‑MIL‑125(Ti) composite photocatalyst, preparation method thereof and application in nitrogen fixation, Fe‑W 18 O 49 The nanowires are evenly distributed on the surface of the NH2-MIL-125(Ti) three-dimensional metal organic framework material. 18 O 49 Compared with the NH2-MIL-125(Ti) single-phase catalyst, there are more photogenerated electron-hole pairs that can separate and participate in the photocatalytic reaction. The photocurrent intensity response is significantly improved, the photocatalytic nitrogen fixation activity is high, and the ammonia generation rate can reach 128.2 μmol·g ‑1 ·h ‑1 , and the generation rate of ammonia does not change significantly after multiple cycles of use, and has good stability; the composite photocatalyst is Fe-W 18 O 49 The obtained product can be obtained by stirring a mixed solution of NH2-MIL-125(Ti). The preparation method has low cost, simple process and easy controllable parameters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photocatalysis technology, and specifically relates to Fe-W 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst, its preparation method and application in nitrogen fixation. Background Art

[0002] Ammonia's high energy density makes it an important chemical substance that can be used as a carbon-free fuel and energy storage medium to provide electricity and heat for humans. At present, the synthesis of ammonia mainly relies on the high temperature and high pressure Haber-Bosch method, which consumes about 1.8% of the world's energy. Using inexhaustible solar energy to achieve nitrogen fixation under mild conditions is an effective alternative to solve the current technical problems of nitrogen fixation.

[0003] Among many semiconductor materials, W 18 O 49 It has good photocatalytic activity, a band gap energy of about 2.9 eV, and exhibits low toxicity, good stability, and high redox potential. It is considered to be an n-type semiconductor material with excellent photocatalytic activity. 18 O 49 The outer surface contains abundant oxygen vacancies, which provide sufficient active sites for adsorption and activation of reactants and are widely used in the field of photocatalysis. At the same time, ion doping can adjust the local coordination environment of the metal center to promote the donation of electrons to the N2 antibonding orbit and N2 adsorption / activity, further improving the nitrogen fixation activity. Inspired by the fact that nitrogenase is composed of iron-molybdenum protein, Fe and Mo elements have natural advantages in nitrogen fixation, and the content of Fe in the earth's crust ranks fourth. Researchers use Fe-doped W 18 O 49 Various studies have been conducted, such as patent CN113318751A discloses a sea urchin-shaped Fe-doped W 18 O 49 , in order to reduce the requirements for the reaction conditions of synthetic ammonia, but the sea urchin-like Fe-W 18 O 49 Fe-doped W nanowires 18 O 49 In comparison, the urchin-like morphology is not conducive to the defects in the catalyst being completely exposed to the outer surface for N2 adsorption and activation; for example, patent CN114669307A improves the preparation method and uses the impregnation method and thermal reduction method to prepare Fe-W containing oxygen vacancies. 18 O 49Nanowires have improved the activity of photocatalytic nitrogen fixation and have been applied in the field of photocatalytic nitrogen fixation. However, this process is prone to uneven impregnation, and the H2 / Ar gas flow rate is difficult to control during high-temperature reduction, resulting in different oxygen vacancy contents in samples prepared from different batches. 18 O 49 (Fe-W 18 O 49 )'s catalytic activity is often affected by low light energy utilization, slow charge transfer, and rapid carrier recombination, resulting in a low ammonia production rate in the nitrogen fixation reaction.

[0004] Therefore, how to improve Fe-W 18 O 49 To improve the photocatalytic nitrogen fixation performance and increase the rate of ammonia production, and to explore a more reasonable catalyst and its preparation method are still technical problems to be solved in this field.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] As mentioned above, the single-phase catalyst Fe-W 18 O 49 There is a problem of low ammonia generation rate. Constructing a heterojunction catalyst to produce a synergistic effect among the components can not only expand the light absorption range and promote the generation of photogenerated electrons and photogenerated holes, but also change the migration path of carriers, reduce the recombination of electron-hole pairs, and enable more photogenerated electrons to migrate to the catalyst surface to participate in the nitrogen fixation reaction. NH2-MIL-125(Ti) metal organic framework material is a three-dimensional metal organic framework material with an orthogonal face-centered cubic topological structure constructed by Ti8O8(OH)4 clusters and 2-aminoterephthalic acid ligands. NH2-MIL-125(Ti) contains cyclic octamers shared by corners or edges. The octamers are connected to other 12 cyclic octamers through 2-aminoterephthalic acid ligands to form a porous 3D structure. It has the characteristics of non-toxicity, multifunctionality, biocompatibility, and excellent redox activity. At the same time, amino modification can reduce the band gap energy of MIL-125(Ti), adjust its band structure, and the light absorption boundary can be extended to 550nm. In addition, NH2-MIL-125(Ti) contains regular porosity, which can promote mutual mass transfer between the outside and the inside, and is widely used in the field of photocatalysis.

[0007] Therefore, in order to solve the Fe-W 18 O 49 There is a problem of low ammonia generation rate in the photocatalytic nitrogen fixation reaction. The present invention provides a Fe-W18 O 49 / NH2-MIL-125(Ti) composite photocatalyst and its preparation method and application in nitrogen fixation. The composite photocatalyst has low preparation cost and high photocatalytic nitrogen fixation activity.

[0008] In order to achieve the above purpose, the present invention adopts the following technical solutions:

[0009] A Fe-W 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst, the composite photocatalyst includes Fe-W 18 O 49 Nanowires and NH2-MIL-125(Ti) metal organic framework materials, Fe-W 18 O 49 The nanowires are uniformly loaded on the surface of NH2-MIL-125(Ti) metal organic framework material.

[0010] In some embodiments, the Fe-W 18 O 49 The mass ratio of nanowires to NH2-MIL-125(Ti) metal organic framework material is 10:(1-5).

[0011] Preferably, in some embodiments, the Fe-W 18 O 49 The mass ratio of the nanowires to the NH2-MIL-125 (Ti) metal organic framework material is 10:(2-5), and the most preferred ratio is 10:2.

[0012] In another aspect, the present invention provides the Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst specifically comprises the following steps:

[0013] (1) WCl6 and FeCl3·6H2O are added to an ethanol solution. The mixed solution is first stirred at room temperature, then heated in a polytetrafluoroethylene-lined autoclave for 12-25 h, centrifuged, washed, and dried to obtain Fe-W containing oxygen vacancies. 18 O 49 Nanowires;

[0014] (2) Mixing the NH2-MIL-125(Ti) solution with the Fe-W obtained in step (1) 18 O 49 The nanowire solutions are ultrasonically dispersed separately, and the two solutions are mixed and stirred. After the solvent is completely evaporated, Fe-W 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst.

[0015] In some embodiments, the mass ratio of WCl6 and FeCl3·6H2O in step (1) is 10:(0.5-2); preferably, in some embodiments, the mass ratio of WCl6 and FeCl3·6H2O in step (1) is 10:1.

[0016] In some embodiments, the mass volume ratio of WCl6 and solvent ethanol in step (1) is (0.1-0.15) : 70, wherein the mass of WCl6 is measured in g and the volume of ethanol is measured in mL; preferably, in some embodiments, the mass volume ratio of WCl6 and solvent ethanol in step (1) is 0.1 : 70, wherein the mass of WCl6 is measured in g and the volume of ethanol is measured in mL.

[0017] In some embodiments, the mixed solution of WCl6 and FeCl3·6H2O in step (1) is stirred at room temperature at a speed of 1000-1200 rpm.

[0018] In some embodiments, the centrifugation process in step (1) is: centrifugation at a speed of 8000-10000 rpm for 3-5 minutes; the washing is: washing with ethanol as a reagent to remove residual raw materials and other by-products in the product; the drying conditions are: maintaining in a vacuum drying oven at 60-70°C for 8-10 hours.

[0019] In some embodiments, the temperature of the polytetrafluoroethylene-lined high-pressure reactor in step (1) is 180-200°C; the polytetrafluoroethylene-lined high-pressure reactor is heated in an electric blast drying oven, and the heating rate of the electric blast drying oven is 2-3°C / min, and the cooling rate is 1-2°C / min.

[0020] In some embodiments, the heating time of the tetrafluoroethylene-lined high-pressure reactor in step (1) in the electric heated forced air drying oven is 20 hours.

[0021] In some embodiments, the preparation of the NH2-MIL-125(Ti) three-dimensional metal organic framework material in step (2) specifically comprises the following steps:

[0022] Add 2-aminoterephthalic acid to the mixed solution of N,N-dimethylformamide and methanol and stir thoroughly. Add tetrabutyl titanate and continue stirring for 30 minutes. Transfer the mixed solution to a polytetrafluoroethylene-lined high-pressure reactor, heat at 140-160°C for 18-22 hours, cool to room temperature, wash with DMF and methanol, and heat and dry to obtain NH2-MIL-125(Ti).

[0023] In some embodiments, in step (2), Fe-W 18 O 49 Add ethanol to dissolve and obtain Fe-W 18 O 49 solution, and adding NH2-MIL-125(Ti) into ethanol to dissolve to obtain NH2-MIL-125(Ti) solution; the Fe-W 18 O 49 The nanowire solution and the NH2-MIL-125 (Ti) solution are ultrasonically dispersed for 20-40 min. The Fe-W 18 O 49 After the nanowire solution is mixed with the NH2-MIL-125(Ti) solution, the stirring time is 8-10 h.

[0024] In some embodiments, the step (2) may also be carried out by mixing Fe-W 18 O 49 The nanowire powder and NH2-MIL-125(Ti) powder are mixed and ball-milled or ground to obtain Fe-W 18 O 49 / NH2-MIL-125(Ti) composite catalyst.

[0025] In a third aspect, the present invention provides a Fe-W 18 O 49 Application of / NH2-MIL-125(Ti) composite photocatalyst in photocatalytic nitrogen fixation.

[0026] In some embodiments, the Fe-W 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst is used in photocatalytic nitrogen fixation, and the photocatalytic nitrogen fixation reaction comprises the following steps: 18 O 49 The / NH2-MIL-125(Ti) composite photocatalyst was dissolved in water, and Na2SO3 was added. In the dark, high-purity N2 was bubbled in, and the nitrogen fixation reaction was carried out under full light irradiation and stirring.

[0027] In some embodiments, in the nitrogen fixation reaction, Fe-W 18 O 49 The mass ratio of / NH2-MIL-125(Ti) composite photocatalyst to water is 1:(1000-4000);

[0028] In some embodiments, the Fe-W 18 O 49The mass ratio of / NH2-MIL-125(Ti) composite photocatalyst to Na2SO3 is 50:(1-50);

[0029] In some embodiments, the high-purity N2 bubbling time is 30-40 min;

[0030] In some embodiments, the full light source is a 300W xenon lamp.

[0031] The beneficial effects of the present invention are:

[0032] 1. Fe-W provided by the present invention 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst, Fe-W 18 O 49 The nanowires are evenly distributed on the surface of NH2-MIL-125(Ti) three-dimensional metal organic framework materials; the composite photocatalyst is relatively 18 O 49 Compared with the NH2-MIL-125(Ti) single-phase catalyst, there are more photogenerated electron-hole pairs that can separate and participate in the photocatalytic reaction. The photocurrent intensity response is significantly improved, the photocatalytic nitrogen fixation activity is high, and the ammonia generation rate in the photocatalytic nitrogen fixation reaction can reach 128.2 μmol·g -1 ·h -1 , and the ammonia generation rate did not change significantly after multiple cycles of use, with good stability.

[0033] 2. The present invention prepares Fe-W by a two-step solvothermal method 18 O 49 Nanowires and NH2-MIL-125(Ti) three-dimensional metal organic framework materials, and then Fe-W 18 O 49 Mix with NH2-MIL-125(Ti) solution and stir to obtain Fe-W 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst, the preparation method has low cost, simple process and easy controllable parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Example 1Fe-W 18 O 49 SEM image of / NH2-MIL-125(Ti) composite photocatalyst;

[0035] Figure 2 Example 1Fe-W 18 O 49High-resolution transmission electron microscopy image of / NH2-MIL-125(Ti) composite photocatalyst;

[0036] Figure 3 The Fe-W of Examples 1-3 18 O 49 / NH2-MIL-125(Ti), Comparative Example 1Fe-W 18 O 49 and X-ray diffraction pattern of comparative example 2NH2-MIL-125(Ti);

[0037] Figure 4 Example 1Fe-W 18 O 49 / NH2-MIL-125(Ti), Comparative Example 1Fe-W 18 O 49 and the photoluminescence spectrum of the comparative example 2NH2-MIL-125(Ti) photocatalyst;

[0038] Figure 5 The Fe-W of Examples 1-3 18 O 49 / NH2-MIL-125(Ti), Fe-W of Comparative Example 1 18 O 49 and the photocurrent spectrum of NH2-MIL-125(Ti) of Comparative Example 2;

[0039] Figure 6 Example 1Fe-W 18 O 49 Photocatalytic cycle test of / NH2-MIL-125(Ti) composite catalyst. DETAILED DESCRIPTION

[0040] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0041] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0042] The instruments, reagents and their sources used in the examples are as follows:

[0043] The structure and morphological characteristics of the synthesized samples were observed using a scanning electron microscope (SEM) of model Hitachi SU-8000FE-SEM, and the internal morphology of the samples was observed using a transmission electron microscope (TEM) JEM-2100PLUS. The composition and crystal form of the prepared samples were analyzed by an X-ray diffractometer (XRD) of model Siemens D5005. The photoluminescence (PL) spectrum of the samples was detected by an F-7000 fluorescence spectrophotometer, and the photocurrent of the samples was estimated by a three-electrode (CHI661D electrochemical workstation) system. The UV-visible diffuse reflectance spectrum of the samples was measured using a varian cary 700 spectrophotometer.

[0044] Tungsten hexachloride (WCl6), ferric chloride hexahydrate (FeCl3·6H2O), 2-aminoterephthalic acid (NH2-BDC) and tetrabutyl titanate (C 16 H 36 O4Ti) was purchased from Aladdin Reagent Co., Ltd., N,N-dimethylformamide (DMF), methanol (MeOH), and ethanol (C2H6O) were purchased from Sinopharm Chemical Reagent Co., Ltd. All chemicals were used directly without further purification.

[0045] The NH2-MIL-125(Ti) metal organic framework material was prepared by the following method: 1.08 g of 2-aminoterephthalic acid was added to a mixed solution of 25 mL of N,N-dimethylformamide and 2.7 mL of methanol and stirred thoroughly, and then 0.52 mL of tetrabutyl titanate was added and stirred for 30 min. The mixed solution was transferred to a polytetrafluoroethylene-lined autoclave and heated at 150°C for 20 h. After cooling to room temperature, it was washed with DMF and methanol and heated to dryness to obtain NH2-MIL-125(Ti).

[0046] Example 1

[0047] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst comprises the following steps:

[0048] (1) 0.1 g WCl6 and 0.01 g FeCl3·6H2O were added to 70 mL ethanol, respectively, and stirred at 1000 rpm for 30 min. The mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave and heated in an electric blast drying oven at 200 °C for 20 h at a heating rate of 2 °C / min. The mixture was then cooled to room temperature at a cooling rate of 1 °C / min. The product Fe-W was collected by centrifugation at 10000 rpm for 3 min. 18 O 49, washed with ethanol and then dried in a drying oven at 60°C for 10 h.

[0049] (2) 0.1 g Fe-W 18 O 49 and 0.02gNH2-MIL-125(Ti) were added to 20mL of ethanol and ultrasonically treated for 30min to be fully dispersed. The two solutions were mixed and stirred for 10h. After the solvent was completely evaporated, Fe-W was obtained. 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst.

[0050] Example 2

[0051] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst specifically comprises the following steps:

[0052] Same as Example 1, except that the amount of NH2-MIL-125(Ti) added in step (2) is 0.01 g.

[0053] Example 3

[0054] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst specifically comprises the following steps:

[0055] Same as Example 1, except that the amount of NH2-MIL-125(Ti) added in step (2) is 0.03 g.

[0056] Example 4

[0057] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst specifically comprises the following steps:

[0058] Same as Example 1, except that the amount of NH2-MIL-125 added in step (2) is 0.05 g.

[0059] Example 5

[0060] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst specifically comprises the following steps:

[0061] The same as Example 1, except that in step (1), the polytetrafluoroethylene-lined high-pressure reactor is heated in an electric heated forced air drying oven at 200° C. for 12 h.

[0062] Example 6

[0063] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst specifically comprises the following steps:

[0064] The same as Example 1, except that in step (1), the polytetrafluoroethylene-lined high-pressure reactor is heated in an electric heated forced air drying oven at 200° C. for 25 h.

[0065] Example 7

[0066] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite photocatalyst specifically comprises the following steps:

[0067] Same as Example 1, except that the amount of FeCl3·6H2O added in step (1) is 0.005 g.

[0068] Example 8

[0069] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125 composite photocatalyst specifically comprises the following steps:

[0070] Same as Example 1, except that the amount of FeCl3·6H2O added in step (1) is 0.02 g.

[0071] Example 9

[0072] Fe-W 18 O 49 The preparation method of the / NH2-MIL-125(Ti) composite catalyst specifically comprises the following steps:

[0073] (1)Fe-W 18 O 49 The preparation method of nanowires is the same as step (1) of Example 1.

[0074] (2) 0.1 g Fe-W 18 O 49 The nanowire powder and 0.02 g NH2-MIL-125 (Ti) powder were placed in a ball mill and the ball mill was operated for 30 min to obtain Fe-W 18 O 49 / NH2-MIL-125(Ti) composite catalyst.

[0075] Comparative Example 1 Single-phase catalyst Fe-W 18 O49 Preparation

[0076] According to the preparation method of step (1) of Example 1, a single-phase catalyst Fe-W 18 O 49 Nanowires.

[0077] Comparative Example 2 Preparation of single-phase catalyst NH2-MIL-125 (Ti)

[0078] 1.08 g of 2-aminoterephthalic acid was added to a mixed solution of 25 mL of N,N-dimethylformamide and 2.7 mL of methanol and stirred thoroughly. Then 0.52 mL of tetrabutyl titanate was added and stirred for 30 min. The mixed solution was transferred to a polytetrafluoroethylene-lined autoclave and heated at 150 ° C for 20 h. After cooling to room temperature, it was washed with DMF and methanol and heated to dryness to obtain NH2-MIL-125 (Ti).

[0079] Verification Example

[0080] 1. Scanning electron microscopy and transmission electron microscopy characterization

[0081] The Fe-W prepared in step 1 18 O 49 The / NH2-MIL-125(Ti) composite photocatalyst was characterized by scanning electron microscopy and transmission electron microscopy. Figure 1 The Fe-W prepared in Example 1 18 O 49 SEM image of the / NH2-MIL-125(Ti) composite photocatalyst. It can be seen from the image that Fe-W 18 O 49 The nanowires are uniformly loaded on the surface of the NH2-MIL-125(Ti) three-dimensional metal organic framework material, and the interfaces are tightly connected and in contact with each other. Figure 2 The Fe-W prepared in Example 1 18 O 49 High-resolution transmission electron microscopy image of the / NH2-MIL-125(Ti) composite material. From the image, we can observe that Fe-W 18 O 49 The lattice fringe is 0.37nm.

[0082] 2. X-ray diffraction test

[0083] The Fe-W prepared in Example 1, Example 2 and Example 3 18 O 49 / NH2-MIL-125(Ti) composite photocatalyst, and comparative example 1Fe-W 18 O 49, Comparative Example 2NH2-MIL-125(Ti) was subjected to X-ray diffraction test, and the test results are as follows Figure 3 As shown. Figure 3 It can be seen that in Fe-W 18 O 49 In the spectrum, there is an obvious characteristic peak at 23.3°, which can be attributed to the W corresponding to JCPDS 5-0392. 18 O 49 Monoclinic form of Fe-W 18 O 49 / NH2-MIL-125(Ti) composite catalyst can be observed 18 O 49 The characteristic peaks of NH2-MIL-125(Ti) can also be observed at 6.8°, 9.5°, 11.5°, 16.5° and 17.9°, indicating that the composite catalyst was successfully prepared.

[0084] 3. Photoluminescence test

[0085] Figure 4 Example 1Fe-W 18 O 49 / NH2-MIL-125(Ti), Comparative Example 1Fe-W 18 O 49 The photoluminescence spectrum of NH2-MIL-125(Ti) prepared in Example 2 and the Fe-W prepared in Example 1 18 O 49 / NH2-MIL-125(Ti) peak intensity is significantly lower than that of Fe-W 18 O 49 and NH2-MIL-125(Ti), which means Fe-W 18 O 49 / NH2-MIL-125(Ti) has more photogenerated electron-hole pairs that can separate and participate in the photocatalytic reaction.

[0086] 4. Photocurrent test

[0087] Figure 5 The Fe-W prepared in Example 1, Example 2 and Example 3 18 O 49 / NH2-MIL-125(Ti), Fe-W prepared in Comparative Example 1 18 O 49 Compared with the photocurrent spectrum of NH2-MIL-125(Ti) prepared in Comparative Example 2, it can be found that the Fe-W prepared in Example 1 18 O 49The photocurrent intensity response of the / NH2-MIL-125(Ti) composite catalyst is significantly higher than that of other catalysts, indicating that the composite catalyst has more photogenerated electrons that can be transferred to the catalyst surface to participate in the photocatalytic reaction, thereby significantly improving the photocatalytic effect.

[0088] 5. Photocatalytic cycle test

[0089] The Fe-W prepared in Example 1 18 O 49 / NH2-MIL-125(Ti) composite material was tested for photocatalytic cycle. The test results Figure 6 As shown, from Figure 6 It can be observed that the generation rate of ammonia does not change significantly after multiple cycles. 18 O 49 / NH2-MIL-125(Ti) composite catalyst has good stability.

[0090] 6. Photocatalytic nitrogen fixation reaction

[0091] The photocatalysts prepared in Examples 1-9 and Comparative Examples 1-2 were used to perform photocatalytic nitrogen fixation, and the specific steps were as follows:

[0092] Take 0.05g of photocatalyst in a photocatalytic reactor, add 100mL of deionized water, add 0.01g of Na2SO3, stir evenly, and bubble high-purity nitrogen for 30 minutes in the dark to exhaust the air in the reaction device. Use a 300W xenon lamp to simulate full-spectrum irradiation. Centrifuge the catalytic solution to remove the catalyst, and detect the ammonia content in the supernatant. The light intensity of the xenon lamp is 200mW·cm -2 The results are shown in Table 1.

[0093] The photocatalytic nitrogen fixation performance of the catalysts prepared in Examples 1-9 and Comparative Examples 1-2 was tested. The model of the UV-Vis spectrophotometer used was Varian Cary 700. The test was carried out in a quartz cuvette. The test results of the ammonia generation rate are shown in Table 1.

[0094] Table 1 Ammonia generation rate of photocatalysts prepared in different embodiments / comparative examples in nitrogen fixation reaction

[0095] Specific embodiments <![CDATA[Ammonia production rate (μmol·g -1 ·h -1 )]]> Example 1 128.2 Example 2 96.7 Example 3 112.5 Example 4 100.1 Example 5 105.9 Example 6 110.6 Example 7 104.3 Example 8 98.7 Example 9 102.7 Comparative Example 1 74.4 Comparative Example 2 9.8

[0096] It can be seen from Table 1 that the Fe-W prepared by the present invention 18 O 49 The nitrogen fixation activity of the / NH2-MIL-125(Ti) composite catalyst was significantly improved, and the maximum ammonia generation rate could reach 128.2 μmol·g -1 ·h-1 , much higher than the Fe-W in Comparative Example 1 18 O 49 The ammonia generation rate when catalyzed by -1 ·h -1 , and the ammonia generation rate of 9.8 μmol·g -1 ·h -1 The composite catalyst prepared by the present invention has a synergistic effect produced by close interface contact between the two, which changes the carrier migration path, is beneficial to the separation of photogenerated electron-hole pairs, and enables the composite catalyst to exhibit good photocatalytic nitrogen fixation activity.

[0097] From the ammonia generation rate of the catalysts prepared in Examples 1-4 in the nitrogen fixation reaction, it can be seen that Fe-W 18 O 49 The ratio of nanowires and NH2-MIL-125(Ti) three-dimensional metal organic framework materials affects the nitrogen fixation activity of the composite catalyst. 18 O 49 When the mass ratio of nanowires to NH2-MIL-125 (Ti) metal organic framework material is 10:2, the nitrogen fixation activity of the prepared composite catalyst is significantly higher than that of the composite catalysts prepared in other ratios.

[0098] From the ammonia generation rate of the catalysts prepared in Examples 1, 5, and 6 in the nitrogen fixation reaction, it can be seen that the solvothermal method in step (1) for preparing Fe-W 18 O 49 When the nanowires are prepared, the difference in heating time can affect the nitrogen fixation activity of the samples.

[0099] From the ammonia generation rate of the catalysts prepared in Examples 1, 7, and 8 in the nitrogen fixation reaction, it can be seen that the solvothermal method in step (1) for preparing Fe-W 18 O 49 When the nanowires are prepared, the mass ratio of WCl6 and FeCl3·6H2O will also affect the nitrogen fixation activity of the samples.

[0100] From the ammonia generation rate of the catalysts prepared in Examples 1 and 9 in the nitrogen fixation reaction, it can be seen that in step (2), Fe-W 18 O 49 The method used when compounding with NH2-MIL-125(Ti) catalyst also affects the nitrogen fixation activity of the sample.

Claims

1. A Fe-W for photocatalytic nitrogen fixation 18 O 49 / NH2-MIL-125 (Ti) composite photocatalyst, characterized in that: The composite photocatalyst includes Fe-W 18 O 49 Nanowires and NH2-MIL-125 (Ti) metal organic framework materials, Fe-W 18 O 49 The nanowires are uniformly loaded on the surface of the NH2-MIL-125 (Ti) metal organic framework material; the Fe-W 18 O 49 The mass ratio of nanowires to NH2-MIL-125 (Ti) metal organic framework material is 10: (1-5).

2. The composite photocatalyst according to claim 1, characterized in that: The Fe-W 18 O 49 The mass ratio of nanowires to NH2-MIL-125 (Ti) metal organic framework material is 10:(2-5).

3. The composite photocatalyst according to claim 1, characterized in that: The Fe-W 18 O 49 The mass ratio of nanowires to NH2-MIL-125 (Ti) metal organic framework material is 10:

2.

4. A Fe-W according to claim 1 18 O 49 / NH2-MIL-125 (Ti) composite photocatalyst preparation method, characterized in that, The following steps are involved: (1) WCl6 and FeCl3•6H2O are added to an ethanol solution. The mixed solution is first stirred at room temperature and then reacted in a polytetrafluoroethylene-lined autoclave. The polytetrafluoroethylene-lined autoclave is heated in an electric blast drying oven for 12-25 hours, centrifuged, washed, and dried to obtain Fe-W containing oxygen vacancies. 18 O 49 Nanowires; (2) Mix the NH2-MIL-125 (Ti) solution with the Fe-W obtained in step (1) 18 O 49 The nanowire solutions are ultrasonically dispersed separately, and the two solutions are mixed and stirred. After the solvent is completely evaporated, Fe-W 18 O 49 / NH2-MIL-125 (Ti) composite photocatalyst.

5. The method for preparing the composite photocatalyst according to claim 4, characterized in that: The mass ratio of WCl6 and FeCl3•6H2O in step (1) is 10:(0.5-2).

6. The method for preparing the composite photocatalyst according to claim 4, characterized in that: The mass ratio of WCl6 and FeCl3•6H2O in step (1) is 10:

1.

7. The method for preparing the composite photocatalyst according to claim 4, characterized in that: The mass volume ratio of WCl6 and solvent ethanol in step (1) is (0.1-0.15) : 70, wherein the mass of WCl6 is measured in g and the volume of ethanol is measured in mL.

8. The method for preparing the composite photocatalyst according to claim 4, characterized in that: In step (1), the heating time of the polytetrafluoroethylene-lined high-pressure reactor in the electric heated blast drying oven is 20 hours.

9. The method for preparing the composite photocatalyst according to claim 4, characterized in that: In step (1), the centrifugation process is: centrifugation at a speed of 8000-10000 rpm for 3-5 minutes; the washing is: washing with ethanol as a reagent to remove the residual raw materials and other by-products in the product; the drying condition is: maintaining in a vacuum drying oven at 60-70°C for 8-10 hours.

10. The method for preparing the composite photocatalyst according to claim 4, characterized in that: In step (2), the Fe-W 18 O 49 The ultrasonic dispersion time of the nanowire solution and the NH2-MIL-125 (Ti) solution is 20-40 minutes; the Fe-W 18 O 49 After the nanowire solution is mixed with the NH2-MIL-125 (Ti) solution, the mixing and stirring time is 8-10 hours.

11. A Fe-W according to any one of claims 1 to 3 18 O 49 / NH2-MIL-125 (Ti) composite photocatalyst or Fe-W prepared by the preparation method according to any one of claims 4 to 10 18 O 49 Application of / NH2-MIL-125 (Ti) composite photocatalyst in photocatalytic nitrogen fixation.

12. The use according to claim 11, characterized in that: The photocatalytic nitrogen fixation reaction steps include: 18 O 49 The / NH2-MIL-125 (Ti) composite photocatalyst was dissolved in water, and Na2SO3 was added. In the dark, high-purity N2 was bubbled in, and the nitrogen fixation reaction was carried out under full light irradiation and stirring.

Citation Information

Patent Citations

  • Application of titanium based metal organic framework material in photocatalytic nitrogen fixation

    CN110548545A

  • Sea urchin-shaped Fe-doped W18O49 composite photocatalyst, and preparation method and application thereof

    CN113318751A