High-silica high-grade daily-use fine porcelain with full glaze on the bottom and preparation method thereof

By forming shallow rounded edges inside the soles of high-silica high-grade daily-use fine porcelain, and firing them with high- and low-temperature glazes, the problem of smooth and delicate soles is solved, and the comfort of use and artistic expression of the product are improved. Suitable for mass production.

CN118420380BActive Publication Date: 2024-10-22SHANDONG GUIYUAN ADVANCED CERAMICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410896019.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-22
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

It is difficult to make the soles of existing high-silica high-grade daily-use fine porcelain smooth and delicate, resulting in easy scratches and residual stains during use, and lack of artistic expression.

Method used

Adopting the preparation method of full glaze on the base, by forming shallow round edges inside the base of the high-silica high-grade daily fine porcelain body, biscuit firing and multiple glaze firings are performed, combined with the use of high-temperature and low-temperature glazes to ensure The sole is fully glazed for smoothness, finesse and wear resistance.

Benefits of technology

It achieves smooth and wear-resistant soles, improves product comfort and artistic expression, solves the problem of rough soles, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118420380B_ABST
    Figure CN118420380B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation of ceramic products, and specifically relates to high-silica high-grade daily-use fine porcelain with full glaze on the bottom and a preparation method thereof. The preparation method of high-silica high-grade daily-use fine porcelain with full glaze on the bottom of the present invention comprises the following steps: sharpening the high-silica high-grade daily-use fine porcelain blank inside the bottom of the blank to form shallow round edges; bisque firing to obtain a blank; applying oil to the shallow round edges of the blank, glazing the entire blank with high-temperature glaze, and firing at high temperature to obtain high-temperature glazed white porcelain; glazing the shallow round edges of the high-temperature glazed white porcelain with low-temperature glaze, and firing at low temperature to obtain high-silica high-grade daily-use fine porcelain with full glaze on the bottom. The present invention provides a preparation method of high-silica high-grade daily-use fine porcelain with full glaze on the bottom, which has simple and stable process operation and can realize mass production; the prepared product has a smooth and wear-resistant bottom, and the fully glazed ceramic bottom is healthy and environmentally friendly, has strong comfort in use, and improves the artistic expression of high-silica high-grade daily-use fine porcelain products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of ceramic products, and in particular relates to high-silica high-grade daily-use fine porcelain with full glaze on the bottom and a preparation method thereof. Background Art

[0002] The water absorption rate of high-grade daily-use fine porcelain is less than 0.5%. The thermal stability is that it will not crack even if it is put into 20℃ water for heat exchange at 190℃. The glaze surface is moist and smooth, the glaze color and the picture are bright, and the hair feet are stable on the plane. The quality is higher than that of ordinary porcelain and fine porcelain. High silicon content is due to the SiO 2 It accounts for more than 70%.

[0003] As a representative of high-end porcelain, high-silica high-grade daily-use fine porcelain is becoming more and more popular. However, with the improvement of living standards and the upgrading of usage requirements, the quality requirements for high-silica high-grade daily-use fine porcelain have been raised. However, the glazing of the bottom of the existing high-silica high-grade daily-use fine porcelain still has great problems. The bottom is difficult to be smooth and delicate due to the special position. Smooth and delicate high-silica high-grade daily-use fine porcelain can prevent scratches on furniture such as dining tables during use, reduce the residual stains on the bottom, improve the comfort of holding, reduce friction on the skin, and improve the aesthetics of the product.

[0004] At present, some ceramic manufacturers will adopt fine polishing technology for the bottom of the product, but it is still impossible to achieve absolute smoothness and fineness. Therefore, the processing of the bottom foot becomes a key factor in whether high-silicon high-grade daily-use fine porcelain can be upgraded to a higher grade.

[0005] CN115784707A discloses a preparation process of a hidden-foot Jianzhan and the prepared hidden-foot Jianzhan, comprising the following steps: preparing a body and glaze slurry, wherein the body bottom foot is a double bottom foot, including an outer bottom foot and an inner bottom foot which are arranged at intervals, the inner bottom foot having a height smaller than the outer bottom foot, and the inner bottom foot is suspended; glazing: the inner bottom foot is not glazed, and other positions of the body are glazed; placing the glazed and air-dried body into a kiln for firing, the inner bottom foot is placed on a support pad, the width of the support pad is smaller than the outer bottom foot, and the outer bottom foot is suspended, and the body is prepared by the following method: mixing 2-2.5 parts by weight of red clay and 7-9 parts by weight of kaolin to obtain body clay, crushing and washing the body clay, passing through an 80-90 mesh sieve, filtering, refining mud, and aging to obtain body clay; throwing the body clay into shape, trimming, biscuit firing, and cooling to obtain a body. The glaze slurry is prepared by the following method: 150 parts by weight of glaze stone, 98-102 parts by weight of potassium feldspar, 48-51 parts by weight of limestone, 19-21 parts by weight of talc, 43-45 parts by weight of red clay and 365-375 parts by weight of water are weighed, added into a ball mill for grinding, and passed through a 100-110 mesh sieve to obtain the glaze slurry. The inner bottom foot of the prepared hidden-foot Jianzhan is not covered with a glaze layer, is relatively rough, easily retains stains, has skin friction when held by hand, and is less comfortable.

[0006] CN100548929C discloses a method for preparing a colored glaze ceramic wine bottle with a bottom that does not expose the body. Before applying the colored glaze, a three-time glazing and firing method is used to apply a layer of glossy base glaze, which greatly improves the quality of glaze decoration and completely eliminates defects such as pinholes and poor glossiness on the glaze. Although the firing temperature of the three-time glazing and firing mentioned above is gradually decreasing, the decreasing amplitude is relatively low. During the firing process, as long as the initial melting temperature of the glaze is exceeded, defects will be formed at the contact point between the glaze surface of the wine bottle and the support, which is not conducive to mass production. Moreover, the prepared colored glaze product adopts a suspended or inverted glaze firing method with a supporting kiln inserted in the bottle mouth, which is only suitable for the production of colored glaze ceramic wine bottles, and is not suitable for daily-use porcelain products such as bowls and plates. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the problem in the prior art of whether the bottom foot can be made glazed like other parts, and to provide a preparation method for high-silicon high-grade daily-use fine porcelain with a fully glazed bottom foot. The process operation is simple and stable, and mass production can be achieved. The prepared product has a smooth and wear-resistant bottom foot, and the fully glazed bottom foot ceramic is healthy and environmentally friendly, and has strong comfort in use, and the artistic expression of the high-silicon high-grade daily-use fine porcelain products is enhanced.

[0008] The method for preparing the high-silica high-grade daily-use fine porcelain with full glaze on the bottom of the present invention comprises the following steps:

[0009] (1) Sharpen the bottom of the high-silicon high-grade daily-use fine porcelain body to form a shallow round edge;

[0010] (2) biscuit firing to obtain a biscuit;

[0011] (3) Apply oil to the shallow round edges of the blank, glaze the entire blank with high-temperature glaze, and fire it at high temperature to obtain high-temperature glaze-fired white porcelain;

[0012] (4) Apply low-temperature glaze to the shallow round edges of high-temperature glazed white porcelain and fire it at low temperature to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom.

[0013] The biscuit firing temperature of step (2) is 1275-1305° C., and the biscuit firing time is 11-13 hours.

[0014] The high temperature glaze of step (3) is made of the following raw materials in percentage by weight: 15-22% quartz, 32-40% feldspar, 9-13% stalactite, 6-9% zirconium oxide, 3-6% raw talc, 8-12% kaolin, 4-8% ceramic powder, and 5-8% boron oxide. The solid content of the prepared high temperature glaze slurry is 61-65wt.%, and particles smaller than 10μm account for 70-80% of the total particles.

[0015] The high temperature sintering temperature of step (3) is 1180-1200° C., and the sintering time is 7-9 hours.

[0016] The low-temperature glaze of step (4) is made of the following raw materials in percentage by weight: quartz 10-18%, albite 38-45%, strontium carbonate 8-15%, Suzhou clay 12-20%, dolomite 5-9%, talc 3-5%, zinc oxide 2-6%. The solid content of the prepared low-temperature glaze slurry is 57-60wt.%, and particles smaller than 10μm account for 80-90% of the total number of particles.

[0017] The low-temperature sintering temperature of step (4) is 800-820°C, and the sintering time is 3-5 hours.

[0018] Step (3) apply oil to the shallow round edges of the blank, glaze the entire blank with high-temperature glaze, place it on a round support platform, and fire it at high temperature.

[0019] A high-silica high-grade daily-use fine porcelain with a full glaze on the bottom is prepared by the preparation method of the high-silica high-grade daily-use fine porcelain with a full glaze on the bottom.

[0020] Specifically, the method for preparing the high-silica high-grade daily-use fine porcelain with full glaze on the bottom foot comprises the following steps:

[0021] (1) Use a triangular tungsten steel blade to sharpen the bottom of a high-silicon, high-grade daily-use fine porcelain body, forming a shallow rounded edge inside the bottom that can be used for support firing.

[0022] (2) Use a shuttle kiln for bisque firing at a temperature of 1275-1305°C for 11-13 hours to obtain a bisque blank.

[0023] (3) Apply oil to the shallow round edge of the biscuit, apply high-temperature glaze to the entire biscuit, and leave the oiled shallow round edge unglazed. Place the shallow round edge of the glazed biscuit on a supporting round frame platform with a small top and a large bottom, and use a shuttle kiln to perform high-temperature firing at a temperature of 1180-1200°C for 7-9 hours to obtain high-temperature glazed white porcelain; the supporting round frame platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter, such as Figure 2 The term "slightly larger" refers to between 1 and 3 mm.

[0024] The high-temperature glaze is made of the following raw materials in percentage by weight: 15-22% quartz, 32-40% potassium feldspar, 9-13% stalactite, 6-9% zirconium oxide, 3-6% raw talc, 8-12% kaolin, 4-8% ceramic powder, and 5-8% boron oxide. The solid content of the prepared high-temperature glaze slurry is 61-65wt.%, and particles smaller than 10μm account for 70-80% of the total number of particles.

[0025] (4) Apply low-temperature glaze to the shallow round edges of high-temperature glaze-fired white porcelain, and use a shuttle kiln for low-temperature firing at a temperature of 800-820°C for 3-5 hours to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom;

[0026] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 10-18%, albite 38-45%, strontium carbonate 8-15%, Suzhou clay 12-20%, dolomite 5-9%, talc 3-5%, zinc oxide 2-6%. The solid content of the prepared low-temperature glaze slurry is 57-60wt.%, and particles smaller than 10μm account for 80-90% of the total number of particles.

[0027] In the preparation method of high-silica high-grade daily-use fine porcelain with full glaze on the bottom foot of the present invention, the addition of porcelain powder and zirconium oxide in the high-temperature glaze can increase the initial melting temperature of the glaze and enhance the hardness of the glaze surface. After the high-temperature glaze is glazed and fired on the bottom foot, the problem of smooth and delicate bottom foot can be solved essentially. The glaze surface has high hardness and strong wear resistance, which reduces the wear of the bottom foot glaze and enhances its practical performance. The high-temperature glaze on the bottom foot has a high initial melting temperature. During the low-temperature glaze firing at 800-820°C, the initial melting temperature of the glaze has not been reached, the glaze surface will not adhere to the firing plate, and its practical performance is retained.

[0028] In the method for preparing high-silica high-grade daily-use fine porcelain with full glaze on the bottom of the present invention, the addition of strontium carbonate in the low-temperature glaze greatly reduces the initial melting temperature and high-temperature viscosity of the glaze, allowing the glaze to be combined with the body of high-silica daily-use fine porcelain at 800-820°C to form a glass-phase glaze surface, thereby covering the shallow round edges with the glaze to achieve the effect of full glaze on the bottom.

[0029] The present invention adopts shallow round edges on the inner part of the bottom foot and cooperates with a supporting round frame platform, which effectively solves the process of high-temperature glaze-fired bottom foot with glaze. The supporting contact part is designed to be shallow round edges, which enhances the artistic sense of the bottom foot and makes the bottom foot more refined and beautiful without being obvious. The upper part of the supporting round frame platform made of alumina material is in contact with the shallow round edges to prevent adhesion and supporting firing, and the lower diameter is slightly larger than the product diameter to play a stabilizing role.

[0030] In the preparation method of the high-silica high-grade daily-use fine porcelain with full glaze on the bottom of the present invention, a combination of high-temperature glaze and low-temperature glaze is used to make the bottom of the product fully glazed, and the product as a whole is smooth and delicate, which prevents the porcelain from scratching the tabletop, reduces the residual stains, improves the comfort of the product, and improves the artistic beauty of the product. The preparation method fills the blank process of the high-silica high-grade daily-use fine porcelain with full glaze on the bottom, and the overall product yield is further improved, and the artistic added value of the product is also increased.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The method for preparing high-silica high-grade daily-use fine porcelain with a full glaze on the bottom of the present invention completely solves the problem of rough bottom. The bottom is smooth and wear-resistant, which greatly improves the practical performance of the product. The full glaze on the bottom of the ceramic is healthy and environmentally friendly, and is comfortable to use, and it also enhances the artistic expression of daily-use porcelain products.

[0033] (2) The method for preparing the full glaze of the bottom foot of high-silicon high-grade daily-use fine porcelain of the present invention has a simple and stable process operation and can realize mass production.

[0034] (3) The high-silica high-grade daily-use fine porcelain with a full glaze on the bottom prepared by the present invention adopts a high-temperature glaze firing process, which improves the glossiness of the high-silica high-grade daily-use fine porcelain and significantly improves the hardness of the glaze surface. The daily-use ceramic products fired three times have high regularity and high yield rate, which not only saves raw materials, but also improves the mechanical strength of the daily-use porcelain products, and further enhances the thermal shock resistance of the products. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Shape diagram of the product prepared for the present invention.

[0036] Figure 2 The utility model discloses a circular frame platform for supporting burning with a small top and a large bottom. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with specific embodiments.

[0038] The raw materials used in the following examples and comparative examples are all commercially available products.

[0039] Example 1

[0040] The method for preparing the high-silica high-grade daily-use fine porcelain with full glaze on the bottom comprises the following steps:

[0041] (1) Use a triangular tungsten steel blade to sharpen the bottom of a high-silicon, high-grade daily-use fine porcelain body, forming a shallow rounded edge inside the bottom for supporting firing.

[0042] (2) Use a shuttle kiln for bisque firing at a temperature of 1280°C for 12 hours to obtain a bisque body.

[0043] (3) Apply oil to the shallow round edge of the biscuit, apply high-temperature glaze to the entire biscuit, and leave the oiled shallow round edge unglazed. Place the shallow round edge of the glazed biscuit on a supporting round frame platform with a small top and a large bottom, and use a shuttle kiln to perform high-temperature firing at a temperature of 1200°C for 8 hours to obtain high-temperature glazed white porcelain; the supporting round frame platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter, such as Figure 2 shown.

[0044] The high-temperature glaze is made of the following raw materials in percentage by weight: 20% quartz, 35% potassium feldspar, 9% stalactite, 7% zirconium oxide, 5% raw talc, 10% kaolin, 6% ceramic powder, and 8% boron oxide. The solid content of the prepared high-temperature glaze slurry is 63wt.%, and particles smaller than 10μm account for 75% of the total number of particles.

[0045] (4) Apply low-temperature glaze to the shallow round edges of high-temperature glaze-fired white porcelain, and use a shuttle kiln for low-temperature firing at a temperature of 810°C for 4 hours to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom; Figure 1 As shown;

[0046] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 15%, albite 45%, strontium carbonate 10%, Suzhou clay 15%, dolomite 5%, talc 5%, and zinc oxide 5%. The solid content of the prepared low-temperature glaze slurry is 58wt.%, and particles smaller than 10μm account for 85% of the total number of particles.

[0047] Example 2

[0048] The method for preparing the high-silica high-grade daily-use fine porcelain with full glaze on the bottom comprises the following steps:

[0049] (1) Use a triangular tungsten steel blade to sharpen the bottom of a high-silicon, high-grade daily-use fine porcelain body, forming a shallow rounded edge inside the bottom that can be used for support firing.

[0050] (2) Use a shuttle kiln for bisque firing at a temperature of 1305°C and a firing time of 11 hours to obtain a bisque body.

[0051] (3) Apply oil to the shallow round edge of the biscuit, apply high-temperature glaze to the entire biscuit, and leave the shallow round edge unglazed. Place the shallow round edge of the glazed biscuit on a round support platform with a small top and a large bottom, and use a shuttle kiln to perform high-temperature firing at 1190°C for 9 hours to obtain high-temperature glazed white porcelain; the round support platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter, such as Figure 2 shown.

[0052] The high-temperature glaze is made of the following raw materials in percentage by weight: quartz 15%, potassium feldspar 40%, stalactite 12%, zirconium oxide 6%, raw talc 6%, kaolin 11%, ceramic powder 5%, boron oxide 5%. The solid content of the prepared high-temperature glaze slurry is 61wt.%, and particles smaller than 10μm account for 80% of the total number of particles.

[0053] (4) Apply low-temperature glaze to the shallow round edges of high-temperature glaze-fired white porcelain, and use a shuttle kiln for low-temperature firing at 800°C for 5 hours to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom;

[0054] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 18%, albite 40%, strontium carbonate 12%, Suzhou clay 18%, dolomite 5%, talc 3%, and zinc oxide 4%. The solid content of the prepared low-temperature glaze slurry is 57wt.%, and particles smaller than 10μm account for 90% of the total number of particles.

[0055] Example 3

[0056] The method for preparing the high-silica high-grade daily-use fine porcelain with full glaze on the bottom comprises the following steps:

[0057] (1) Use a triangular tungsten steel blade to sharpen the bottom of a high-silicon, high-grade daily-use fine porcelain body, forming a shallow rounded edge inside the bottom that can be used for support firing.

[0058] (2) Use a shuttle kiln for bisque firing at a temperature of 1275°C and a firing time of 13 hours to obtain a bisque body.

[0059] (3) Apply oil to the shallow round edge of the biscuit, apply high-temperature glaze to the entire biscuit, and leave the shallow round edge unglazed. Place the shallow round edge of the glazed biscuit on a round support platform with a small top and a large bottom, and use a shuttle kiln to perform high-temperature firing at 1180°C for 9 hours to obtain high-temperature glazed white porcelain; the round support platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter, such as Figure 2 shown.

[0060] The high-temperature glaze is made of the following raw materials in percentage by weight: 22% quartz, 35% potassium feldspar, 12% stalactite, 6% zirconium oxide, 5% raw talc, 9% kaolin, 6% ceramic powder, and 5% boron oxide. The solid content of the prepared high-temperature glaze slurry is 64wt.%, and particles smaller than 10μm account for 73% of the total number of particles.

[0061] (4) Apply low-temperature glaze to the shallow round edges of high-temperature glaze-fired white porcelain, and use a shuttle kiln for low-temperature firing at a temperature of 805°C for 4 hours to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom;

[0062] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 17%, albite 43%, strontium carbonate 11%, Suzhou clay 14%, dolomite 9%, talc 4%, and zinc oxide 2%. The solid content of the prepared low-temperature glaze slurry is 57wt.%, and particles smaller than 10μm account for 90% of the total number of particles.

[0063] Example 4

[0064] The method for preparing the high-silica high-grade daily-use fine porcelain with full glaze on the bottom comprises the following steps:

[0065] (1) Use a triangular tungsten steel blade to sharpen the bottom of a high-silicon, high-grade daily-use fine porcelain body, forming a shallow rounded edge inside the bottom that can be used for support firing.

[0066] (2) Use a shuttle kiln for bisque firing at a temperature of 1290°C and a firing time of 12 h to obtain a bisque blank.

[0067] (3) Apply oil to the shallow round edge of the biscuit, apply high-temperature glaze to the entire biscuit, and leave the oiled shallow round edge unglazed. Place the shallow round edge of the glazed biscuit on a round support platform with a small top and a large bottom, and use a shuttle kiln to perform high-temperature firing at a temperature of 1195°C for 7 hours to obtain high-temperature glazed white porcelain; the round support platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter, such as Figure 2 shown.

[0068] The high-temperature glaze is made of the following raw materials in percentage by weight: 20% quartz, 32% potassium feldspar, 12% stalactite, 9% zirconium oxide, 4% raw talc, 8% kaolin, 8% ceramic powder, and 7% boron oxide. The solid content of the prepared high-temperature glaze slurry is 65wt.%, and particles smaller than 10μm account for 76% of the total number of particles.

[0069] (4) Apply low-temperature glaze to the shallow round edges of high-temperature glaze-fired white porcelain, and use a shuttle kiln for low-temperature firing at a temperature of 810°C for 3 hours to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom;

[0070] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 10%, albite 44%, strontium carbonate 15%, Suzhou clay 12%, dolomite 8%, talc 5%, and zinc oxide 6%. The solid content of the prepared low-temperature glaze slurry is 60wt.%, and particles smaller than 10μm account for 80% of the total number of particles.

[0071] Example 5

[0072] The method for preparing the high-silica high-grade daily-use fine porcelain with full glaze on the bottom comprises the following steps:

[0073] (1) Use a triangular tungsten steel blade to sharpen the bottom of a high-silicon, high-grade daily-use fine porcelain body, forming a shallow rounded edge inside the bottom that can be used for support firing.

[0074] (2) Use a shuttle kiln for bisque firing at a temperature of 1300°C and a firing time of 13 h to obtain a bisque body.

[0075] (3) Apply oil to the shallow round edge of the biscuit, apply high-temperature glaze to the entire biscuit, and leave the shallow round edge unglazed. Place the shallow round edge of the glazed biscuit on a round support platform with a small top and a large bottom, and use a shuttle kiln to perform high-temperature firing at a temperature of 1185°C for 8 hours to obtain high-temperature glazed white porcelain; the round support platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter, such as Figure 2 shown.

[0076] The high-temperature glaze is made of the following raw materials in percentage by weight: quartz 19%, potassium feldspar 35%, stalactite 13%, zirconium oxide 8%, raw talc 3%, kaolin 12%, ceramic powder 4%, boron oxide 6%. The solid content of the prepared high-temperature glaze slurry is 62wt.%, and particles smaller than 10μm account for 70% of the total number of particles.

[0077] (4) Apply low-temperature glaze to the shallow round edges of high-temperature glaze-fired white porcelain, and use a shuttle kiln for low-temperature firing at 820°C for 4 hours to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom;

[0078] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 17%, albite 38%, strontium carbonate 8%, Suzhou clay 20%, dolomite 8%, talc 4%, and zinc oxide 5%. The solid content of the prepared low-temperature glaze slurry is 59wt.%, and particles smaller than 10μm account for 87% of the total number of particles.

[0079] Comparative Example 1

[0080] A method for preparing high-silicon high-grade daily-use fine porcelain comprises the following steps:

[0081] (1) The high-silica high-grade daily-use fine porcelain can be plastically molded to obtain a high-silica fine porcelain body, and a triangular tungsten steel blade is used to sharpen the bottom of the body to form a shallow round edge that can be used for support firing.

[0082] (2) Use a shuttle kiln for bisque firing at a temperature of 1280°C for 12 hours to obtain a bisque body.

[0083] (3) Apply oil to the shallow round edges of the blank, and glaze the entire blank with high-temperature glaze. Leave the shallow round edges unglazed. Place the shallow round edges of the glazed blank on a round support platform with a small top and a large bottom.

[0084] The high temperature glaze is made of the following raw materials in percentage by weight: quartz 18%, potassium feldspar 37%, stalactite 11%, zirconium oxide 8%, raw talc 4%, kaolin 10%, ceramic powder 5%, and boron oxide 7%.

[0085] The solid content of the high temperature glaze is 63wt.%, and particles smaller than 10μm account for 75% of the total number of particles.

[0086] The round frame platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter.

[0087] High-temperature glaze firing is carried out in a shuttle kiln with a firing temperature of 1190°C and a firing time of 8 hours to obtain high-temperature glaze-fired white porcelain.

[0088] (4) Apply low-temperature glaze to the shallow rounded edges of white porcelain.

[0089] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 17%, albite 43%, strontium carbonate 6%, Suzhou soil 16%, dolomite 8%, talc 5%, and zinc oxide 5%.

[0090] The solid content of the low-temperature glaze is 58wt.%, and particles smaller than 10μm account for 85% of the total number of particles.

[0091] The shuttle kiln is used for low-temperature glaze firing, with the firing temperature at 810°C and the firing time for 4 hours, to obtain high-silica, high-grade daily-use fine porcelain with a full glaze on the bottom.

[0092] Comparative Example 2

[0093] A method for preparing high-silicon high-grade daily-use fine porcelain comprises the following steps:

[0094] (1) The high-silica high-grade daily-use fine porcelain can be plastically molded to obtain a high-silica fine porcelain body, and a triangular tungsten steel blade is used to sharpen the bottom of the body to form a shallow round edge that can be used for support firing.

[0095] (2) Use a shuttle kiln for bisque firing at a temperature of 1300°C and a firing time of 12 h to obtain a bisque blank.

[0096] (3) Apply oil to the shallow round edges of the blank, and glaze the entire blank with high-temperature glaze. Leave the shallow round edges unglazed. Place the shallow round edges of the glazed blank on a round support platform with a small top and a large bottom.

[0097] The high temperature glaze is made of the following raw materials in percentage by weight: quartz 20%, potassium feldspar 39%, stalactite 12%, zirconium oxide 3%, raw talc 5%, kaolin 11%, ceramic powder 3%, and boron oxide 7%.

[0098] The solid content of the high temperature glaze is 64wt.%, and particles smaller than 10μm account for 75% of the total number of particles.

[0099] The round frame platform is made of alumina, with an upper diameter slightly larger than the diameter of the shallow round edge and a lower diameter slightly larger than the product diameter.

[0100] High-temperature glaze firing is carried out in a shuttle kiln with a firing temperature of 1190°C and a firing time of 8 hours to obtain high-temperature glaze-fired white porcelain.

[0101] (4) Apply low-temperature glaze to the shallow rounded edges of white porcelain.

[0102] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 16%, albite 41%, strontium carbonate 12%, Suzhou soil 16%, dolomite 7%, talc 4%, and zinc oxide 4%.

[0103] The solid content of the low-temperature glaze is 58wt.%, and particles smaller than 10μm account for 83% of the total number of particles.

[0104] The shuttle kiln is used for low-temperature glaze firing, with the firing temperature at 810°C and the firing time for 4 hours, to obtain high-silica, high-grade daily-use fine porcelain with a full glaze on the bottom.

[0105] Comparative Example 3

[0106] A method for preparing high-silicon high-grade daily-use fine porcelain comprises the following steps:

[0107] (1) The high-silica high-grade daily-use fine porcelain can be plastically molded to obtain a high-silica fine porcelain body, and a triangular tungsten steel blade is used to sharpen the bottom of the body to form a shallow round edge that can be used for support firing.

[0108] (2) Use a shuttle kiln for bisque firing at a temperature of 1290°C and a firing time of 12 h to obtain a bisque body.

[0109] (3) Apply oil to the shallow rounded edges of the blank, and glaze the blank with high-temperature glaze. If the shallow rounded edges are not glazed, wipe off the glaze on the bottom and place the glazed blank on the shelf.

[0110] The high temperature glaze is made of the following raw materials in percentage by weight: quartz 19%, potassium feldspar 36%, stalactite 12%, zirconium oxide 8%, raw talc 5%, kaolin 9%, ceramic powder 5%, and boron oxide 6%.

[0111] The solid content of the high temperature glaze is 64wt.%, and particles smaller than 10μm account for 75% of the total number of particles.

[0112] High-temperature glaze firing is carried out in a shuttle kiln with a firing temperature of 1195°C and a firing time of 8 hours to obtain high-temperature glaze-fired white porcelain.

[0113] (4) Apply low-temperature glaze to the shallow rounded edges of white porcelain.

[0114] The low-temperature glaze is made of the following raw materials in percentage by weight: quartz 15%, albite 42%, strontium carbonate 12%, Suzhou soil 15%, dolomite 8%, talc 4%, and zinc oxide 4%.

[0115] The solid content of the low-temperature glaze is 59wt.%, and particles smaller than 10μm account for 84% of the total number of particles.

[0116] Low-temperature glaze firing is carried out in a shuttle kiln, with a firing temperature of 810°C and a firing time of 5 hours to obtain high-silicon, high-grade daily-use fine porcelain.

[0117] The high-silica high-grade daily-use fine porcelain prepared in the above embodiments and comparative examples was tested for smoothness using a TR100 pocket roughness meter, and the glaze Vickers hardness was tested using a HV-1000ZDT automatic turret microhardness tester. The test results of the high-silica high-grade daily-use fine porcelain bottom are shown in Table 1.

[0118] Table 1 Test results

[0119]

[0120] As can be seen from Table 1 above, the bottom of the embodiment 1-5 of the present invention is glazed, the bottom foot is smooth and delicate, the bottom foot finish is 0.17-0.20 μm, and the Vickers hardness of the glaze reaches 600 kg / mm 2 , the product has good bottom smoothness, high glaze hardness, high mechanical strength and strong wear resistance. In Comparative Example 1, the amount of strontium carbonate added to the low-temperature glaze is reduced, resulting in a slight increase in the initial melting temperature and high-temperature viscosity of the low-temperature glaze. At the low-temperature firing temperature, the glass phase of the glaze is not fully formed, resulting in the glaze at the shallow round edge not being densely bonded, failing to ensure full glaze on the bottom, and poor performance in smoothness and glaze Vickers hardness. In Comparative Example 2, the amount of zirconium oxide and porcelain powder added to the high-temperature glaze is reduced, resulting in a decrease in the initial melting temperature of the high-temperature glaze, poor wear resistance of the bottom glaze, and during low-temperature firing, the bottom glaze and the firing plate are stained with the bottom, failing to ensure a smooth and delicate bottom. The bottom of Comparative Example 3 is not glazed, the bottom of the product is in a biscuit state, the bottom of the product is rough, the finish is poor, it is easy to have residual stains, rub the desktop and skin, and the mechanical strength of the product is also reduced.

Claims

1. A method for preparing high-silica high-grade daily-use fine porcelain with full glaze on the bottom, characterized in that: The following steps are involved: (1) Sharpen the bottom of the high-silicon high-grade daily-use fine porcelain body to form a shallow round edge; (2) biscuit firing to obtain a biscuit; (3) Apply oil to the shallow round edges of the biscuit, glaze the entire biscuit with high-temperature glaze, and fire at 1180-1200℃ for 7-9h to obtain high-temperature glaze-fired white porcelain; The high-temperature glaze is made of the following raw materials in percentage by weight: quartz 15-22%, potassium feldspar 32-40%, stalactite 9-13%, zirconium oxide 6-9%, raw talc 3-6%, kaolin 8-12%, ceramic powder 4-8%, boron oxide 5-8%; (4) Apply low-temperature glaze to the shallow round edges of high-temperature glaze-fired white porcelain, and fire at 800-820℃ for 3-5h to obtain high-silica high-grade daily-use fine porcelain with a full glaze on the bottom; The low-temperature glaze is made of the following raw materials in percentage by weight: 10-18% quartz, 38-45% albite, 8-15% strontium carbonate, 12-20% Suzhou clay, 5-9% dolomite, 3-5% talc and 2-6% zinc oxide.

2. The method for preparing high-silica high-grade daily-use fine porcelain with full glaze on the bottom according to claim 1, characterized in that: The biscuit firing temperature of step (2) is 1275-1305° C., and the biscuit firing time is 11-13 hours.

3. The method for preparing high-silica high-grade daily-use fine porcelain with full glaze on the bottom according to claim 1, characterized in that: The solid content of the prepared high-temperature glaze slurry is 61-65wt.%, and particles smaller than 10μm account for 70-80% of the total number of particles.

4. The method for preparing high-silica high-grade daily-use fine porcelain with full glaze on the bottom according to claim 1, characterized in that: The solid content of the prepared low-temperature glaze slurry is 57-60wt.%, and particles smaller than 10μm account for 80-90% of the total number of particles.

5. The method for preparing high-silica high-grade daily-use fine porcelain with full glaze on the bottom according to claim 1, characterized in that: Step (3) apply oil to the shallow round edges of the blank, glaze the entire blank with high-temperature glaze, place it on a round support platform, and fire it at high temperature.

6. A high-grade daily-use fine porcelain with a fully glazed bottom, characterized by: The porcelain is prepared by the method for preparing high-silica high-grade daily-use fine porcelain with full glaze on the bottom as described in any one of claims 1 to 5.