A plasticized wear-resistant alloy material and preparation method thereof

Through mechanical alloying and powder metallurgy combined with surface deformation treatment, an alloy material with a double-layer heterogeneous structure is prepared, which solves the problem of hard phase and soft phase being difficult to dissolve in each other, and achieves both high wear resistance and plasticity. .

CN118422025BActive Publication Date: 2024-10-18SHANTOU UNIV
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410866112.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-18
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

During the preparation process of existing multi-principal alloy materials, due to the large difference in melting point between the hard phase and the soft phase and the difficulty in miscibility with each other, it is difficult to form a high-performance heterostructure, resulting in insufficient wear resistance of the material.

Method used

Mechanical alloying and powder metallurgy methods are used to prepare a heterostructure with a hard phase as the matrix and a soft phase as the second phase, and a nano-layered structure is formed through surface deformation treatment. Combined with the coupling effect of each step, plasticized resistance is obtained. Milled bilayer heterostructure.

Benefits of technology

While ensuring high hardness, it can significantly improve the plasticity and wear resistance of the material, reduce the wear rate, and alleviate the crack problem caused by stress concentration through the nano-layered structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118422025B_ABST
    Figure CN118422025B_ABST
Patent Text Reader

Abstract

The present invention discloses a plasticized wear-resistant alloy material and a preparation method thereof, wherein the alloy material has a double-layer heterogeneous structure, and the alloy material is composed of a hard matrix phase and a soft second phase; wherein: the hard matrix phase is at least two of Ta, Mo, Nb, Ti, Hf, Zr, W, and Re; and the soft second phase is at least one of Cu, Ag, Mg, and Zn. The present invention gives full play to the advantages of the hard matrix phase and the soft second phase, alleviates the crack problem caused by stress concentration caused by the inability of the hard matrix phase to coordinate deformation; while ensuring high hardness, the plasticity of the material is improved, and the wear resistance of the material is finally improved. And firstly, a heterogeneous structure is obtained by mechanical alloying and powder metallurgy; then, a surface deformation treatment is performed to obtain an adaptive plasticized wear-resistant double-layer heterogeneous structure of the surface and sub-surface of the material; while the hardness is slightly reduced, its wear resistance is greatly improved, and good plasticity is retained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials, and in particular relates to a plasticized wear-resistant alloy material and a preparation method thereof. Background Art

[0002] Sliding wear is a key factor that limits the life of metal parts in a wide range of functional and structural applications. In addition, a large amount of heat is generated during friction and wear, resulting in huge energy consumption. Among them, the factors that have a greater impact on the wear resistance of materials are: the hardness and plasticity of the material, and the microstructural evolution of the wear subsurface during friction. Generally speaking, the higher the hardness of the material and the stronger the ability of the wear subsurface to undergo coordinated deformation, the better the wear resistance. In recent years, multi-principal alloys have been widely used in the field of tribology due to their high strength, hardness, toughness and good wear resistance.

[0003] There are many kinds of existing multi-principal alloy materials. Among them, the hard phase structure can obtain a lower wear rate because of its high hardness and strength; while the soft phase structure has poor hardness, but it can slide more at room temperature, absorb stress, and has a certain lubrication effect. For some multi-principal alloys with hard phase as the matrix and soft phase as the second phase, during the sliding friction process, due to the high plasticity of the soft phase, high strain rate and strain gradient can cause severe plastic deformation of the sub-surface of the material, forming an adaptive nano-layered structure. Different from the traditional concept that the higher the hardness of the material, the better the wear resistance, this nano-layered structure provides a new strategy to improve the lack of plasticity of wear-resistant multi-principal cemented carbide. However, the melting points of the hard phase and the soft phase structure are generally different, and there is a problem of difficulty in miscibility. Traditional smelting requires repeated remelting and long-term homogenization treatment, with a long production cycle and difficult cost control; additive manufacturing is often difficult to achieve complete solid solution during the molding process for refractory hard metal elements such as high content of Ta and Mo. Therefore, it is difficult to prepare a heterogeneous structure of hard phase and soft phase by the above conventional process.

[0004] In response to the above problems, if we can combine the advantages of the hard phase's high hardness and strength with the soft phase's good plasticity, and through the regulation of the microstructure, we can develop a double-layer heterogeneous structure that has both high wear resistance and good plasticity while ensuring the hardness. This will have important guiding significance for the design of alloy materials serving in harsh environments. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a plasticized wear-resistant alloy material and a preparation method thereof, wherein the alloy material can have good hardness, wear resistance and plasticity at the same time.

[0006] The inventive concept of the present invention is as follows: the alloy material of the present invention has a double-layer heterogeneous structure, and the alloy material is composed of a hard matrix phase with high hardness and high strength and a soft second phase with high plasticity. By optimizing and reasonably compounding the hard matrix phase and the soft second phase, the advantages of the hard matrix phase and the soft second phase are fully utilized, and the crack problem caused by stress concentration due to the inability of the hard matrix phase to deform in a coordinated manner is alleviated; while ensuring high hardness, the plasticity of the material is improved, and ultimately the wear resistance of the material is improved. At the same time, when preparing the alloy material of the present invention, a heterogeneous structure with a hard phase as a matrix and a soft phase as a second phase is first obtained by mechanical alloying and powder metallurgy methods; then, a surface deformation treatment is performed to produce severe plastic deformation, so that the hard matrix phase and the soft second phase on the subsurface of the material are elongated, and the formation of a nano-layered structure on the subsurface of the material is spontaneously induced, thereby obtaining a self-adaptive plasticized wear-resistant double-layer heterogeneous structure of the surface-subsurface of the material; and the coupling effect between the steps is used to enable the double-layer heterogeneous structure to obtain a nanocrystalline organization and improve the density, so that while the hardness is slightly reduced, its wear resistance is greatly improved, and good plasticity is retained.

[0007] To solve the above technical problems, the first aspect of the present invention provides an alloy material, which has a double-layer heterogeneous structure and is composed of a hard matrix phase and a soft second phase; the hard matrix phase is at least two of Ta, Mo, Nb, Ti, Hf, Zr, W, and Re; and the soft second phase is at least one of Cu, Ag, Mg, and Zn.

[0008] Specifically, the alloy material of the present invention uses a hard phase as a matrix, and adds a certain amount of soft second phase to the hard matrix phase to form a double-layer heterogeneous structure of different components. Among them, the hard phase metals Ta, Mo, Nb, Ti, Hf, Zr, W, and Re all have high hardness and wear resistance, but at the same time, these metals have the problem of insufficient plasticity. The soft second phases Cu, Ag, Mg, or Zn all have a low melting point and are difficult to dissolve in the hard matrix phase, so it is easy to form a soft second phase, and the low shear strength is also conducive to improving the plastic deformation ability of the hard matrix phase; and at the same time, it alleviates the problem of cracks caused by stress concentration caused by the inability of the hard matrix phase to coordinate deformation.

[0009] As a further improvement of the above solution, the molar ratio of the hard matrix phase to the soft second phase is (90-99): (1-10).

[0010] Preferably, the molar ratio of the hard matrix phase to the soft second phase is (90-95):(5-10).

[0011] Specifically, by optimizing and reasonably compounding the hard matrix phase and the soft second phase, the high hardness and strength of the hard matrix phase and the plasticity of the soft second phase are fully utilized, effectively alleviating the crack problem caused by stress concentration due to the inability of the hard matrix phase to coordinate deformation. On the premise of ensuring the high hardness of the material, the plasticity of the material is further improved, thereby further improving the wear resistance of the material.

[0012] As a further improvement of the above solution, the grain size of the hard matrix phase is 190-220 nm.

[0013] Preferably, the grain size of the hard matrix phase is 192-213 nm.

[0014] As a further improvement of the above solution, the grain size of the soft second phase is 190-220 nm.

[0015] Preferably, the grain size of the soft second phase is 192-213 nm.

[0016] Specifically, by selecting metal powder with relatively small particle size (including hard matrix phase and soft second phase), it is beneficial to play the role of fine grain strengthening, thereby improving the hardness and wear resistance of the material.

[0017] As a further improvement of the above solution, the purity of the hard matrix phase is ≥98%.

[0018] As a further improvement of the above solution, the purity of the soft second phase is ≥98%.

[0019] Specifically, high-purity metal powder (including a hard matrix phase and a soft second phase) can reduce the introduction of impurities and ensure the comprehensive performance of the material.

[0020] A second aspect of the present invention provides a method for preparing the above alloy material, comprising the following steps:

[0021] (1) Mixing the metal powders of the hard matrix phase and the soft second phase, and then grinding and mechanically alloying them to obtain a solid solution alloy powder;

[0022] (2) sintering the solid solution alloy powder and performing powder metallurgy to obtain a bulk alloy material;

[0023] (3) Performing surface deformation treatment on the bulk alloy material to obtain the alloy material.

[0024] Specifically, since the melting points of the hard matrix phase and the soft second phase are quite different and they are difficult to dissolve in each other, it is difficult to prepare high-performance alloy materials through conventional processes. The present invention adopts a preparation process that combines mechanical alloying, powder metallurgy and surface deformation treatment to regulate the microstructure while forming a strong solid solution, precipitate a certain amount of soft second phase in the hard matrix phase, and control the grain size at the nanoscale, thereby improving the density and finally obtaining a block heterogeneous structure.

[0025] As a further improvement of the above scheme, in step (1), the grinding method is high-energy ball milling.

[0026] Preferably, in step (1), the grinding balls used for grinding are stainless steel grinding balls, and the ball-to-material mass ratio during grinding is (4-6):1.

[0027] Preferably, in step (1), the grinding speed is 600-1000 r / min.

[0028] Preferably, in step (1), the grinding time is 3-20 hours; more preferably, the grinding time is 6-12 hours.

[0029] As a further improvement of the above solution, in step (2), the sintering method is any one of spark plasma sintering, hot isostatic pressing sintering, and hot pressing sintering.

[0030] Preferably, in step (2), the sintering method is spark plasma sintering, and the spark plasma sintering is performed in a vacuum environment with a vacuum degree stabilized at 80-90 KPa.

[0031] Preferably, in step (2), the sintering temperature is 1100-1500° C. This temperature range is higher than the melting point of the soft second phases Cu, Ag, Mg, and Zn. Within this temperature range, the liquid soft phase can promote the sintering of the hard matrix phase, improve the material density, and avoid grain growth caused by excessively high temperature.

[0032] Preferably, in step (2), the heating rate of the sintering is 70-100° C. / min.

[0033] Preferably, in step (2), the sintering time is 3-8 minutes.

[0034] As a further improvement of the above solution, in step (3), the surface deformation treatment method is any one of rolling, shot peening, and laser shock strengthening.

[0035] Specifically, the present invention uses mechanical means to cause severe plastic deformation of the metal surface and subsurface through surface deformation treatment. Under the action of large shear deformation with high strain rate and strain gradient, the hard matrix phase and soft second phase of the material subsurface are elongated, which can induce the formation of high hardness and high stability of the material subsurface nano-layered structure, thereby obtaining an adaptive double-layer heterogeneous structure of the material surface-subsurface. While ensuring high hardness, the coordinated deformation mechanism between the hard matrix phase and the soft second phase can effectively improve the plasticity of the material and significantly improve the wear resistance.

[0036] Preferably, in step (3), the surface deformation treatment method is rolling, and the rolling is to use mechanical rolling to deform the surface.

[0037] Preferably, the rolling component is a ball, and the diameter of the ball is 2-4 mm.

[0038] Preferably, the rolling reduction amount is 0.1-0.2 mm.

[0039] Preferably, the rolling pressure is 1.0-2.0 MPa.

[0040] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:

[0041] (1) The present invention selects a specific hard phase as the matrix and a soft phase as the second phase, giving full play to the high hardness and strength of the hard matrix phase and the plasticity of the soft second phase, while ensuring high hardness, improving the plasticity of the material, and ultimately improving the wear resistance of the material. Different from the traditional principle that the higher the hardness of the material, the better the wear resistance, the present invention achieves a slight decrease in the hardness of the alloy material (14.1-29.6%) by adding a certain amount of soft second phase to the hard matrix phase, but the plastic strain is greatly increased (2.2-3.0 times), and the wear rate is also greatly reduced (33.9-67.8%); that is, while ensuring high hardness (HV>500), the plasticity and wear resistance of the material are significantly improved.

[0042] (2) The alloy material of the present invention is prepared by mechanical alloying and powder metallurgy process to control the microstructure, thus overcoming the problem that the hard matrix phase and the soft second phase have large melting point differences and are difficult to dissolve each other. The grain size of the prepared alloy material is nanocrystalline and the density is improved. Through surface deformation treatment, the severe plastic deformation can induce the formation of a sub-surface nano-layered structure of the material, forming a double-layer heterogeneous structure with the surface. The nano-layered structure alleviates the crack problem caused by stress concentration caused by the inability of the hard matrix phase to coordinate deformation, and improves the plasticity and wear resistance.

[0043] (3) When the alloy material of the present invention is used under sliding friction conditions, after the material surface is worn, under the continuous action of friction stress, the subsurface of the material will undergo severe plastic deformation again, the hard matrix phase and soft second phase of the subsurface will be elongated in the direction parallel to the sliding friction, and a nano-layered structure will be continuously formed. The adaptive double-layer heterogeneous structure can effectively play the role of plasticization and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 HAADF-STEM image of the ND-SD cross-sectional microstructure of the TaMoNb10Cu alloy prepared in Example 1 of the present invention under the friction track;

[0045] Figure 2 This is a HAADF-STEM image of the ND-SD cross-sectional microstructure of the TaMoNb alloy prepared in Comparative Example 1 of the present invention under the friction track. DETAILED DESCRIPTION

[0046] The present invention is described in detail below in conjunction with the examples, so that the technical personnel of the relevant technical field can understand the present invention. It is necessary to point out here that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The non-essential improvements and adjustments made to the present invention by the skilled person in the relevant field according to the above invention content should still belong to the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art.

[0047] Example 1

[0048] An alloy material consists of Cu powder (purity of 99.99%, grain size of 192-213nm) and equimolar TaMoNb alloy powder (purity of 99.99%, grain size of 192-213nm), and the molar ratio of TaMoNb alloy powder to Cu powder is 90:10.

[0049] A method for preparing an alloy material comprises the following steps:

[0050] (1) TaMoNb alloy powder and Cu powder were weighed in molar ratio, loaded into a high-energy ball mill, and stainless steel grinding balls with a diameter of 10 mm were added at a ball-to-material mass ratio of 5:1. The mixture was ball-milled at a speed of 875 r / min for 9 hours to mechanically alloy the powder and obtain a solid solution alloy powder.

[0051] (2) the solid solution alloy powder obtained in step (1) is loaded into a graphite grinding tool, and the grinding tool is placed in a spark plasma sintering furnace. Under a sintering pressure of 60 MPa, the temperature is raised to 1100°C at a rate of 100°C / min and sintered for 5 minutes to perform powder metallurgy. After the sintering, the furnace is cooled to room temperature to precipitate a certain amount of Cu-rich soft second phase in the hard phase TaMoNb matrix, and the grain size is controlled at the nanoscale to obtain a bulk alloy material TaMoNb10Cu;

[0052] (3) The bulk alloy material TaMoNb10Cu obtained in step (2) is subjected to surface deformation treatment by mechanical rolling. A ball with a diameter of 3 mm is placed in the ball. The rolling pass is 1 time, the reduction amount is 0.16 mm, and the rolling force is 1.5 MPa, thereby obtaining a TaMoNb10Cu alloy material with a double-layer heterogeneous structure.

[0053] Figure 1 This is the HAADF-STEM image of the ND-SD cross-sectional microstructure of the TaMoNb10Cu alloy material prepared in Example 1 under the friction track. The Pt layer is a protective layer during sample preparation. Figure 1 It can be seen that there is a severe plastic deformation area with a depth of 1.5μm below the wear surface. The grains are severely refined under the action of friction stress and are severely elongated in the direction parallel to the sliding friction (see the dotted box). The aspect ratio is generally greater than 10, showing good plasticity and forming a plasticized and wear-resistant double-layer heterogeneous structure; the general plastic deformation layer is about 1.5-4.5μm below the wear surface. The grains in this area are elongated along the sliding direction under the action of friction stress; the bottom area is subject to very little friction stress and is an undeformed layer.

[0054] Example 2

[0055] An alloy material consists of Cu powder (purity of 99.99%, grain size of 192-213nm) and equimolar TaMoNb alloy powder (purity of 99.99%, grain size of 192-213nm), and the molar ratio of TaMoNb alloy powder to Cu powder is 95:5.

[0056] A method for preparing an alloy material comprises the following steps:

[0057] (1) TaMoNb alloy powder and Cu powder were weighed in molar ratio, loaded into a high-energy ball mill, and stainless steel grinding balls with a diameter of 10 mm were added at a ball-to-material mass ratio of 5:1. The mixture was ball-milled at a speed of 875 r / min for 9 hours to mechanically alloy the powder and obtain a solid solution alloy powder.

[0058] (2) the solid solution alloy powder obtained in step (1) is loaded into a graphite grinding tool, and the grinding tool is placed in a spark plasma sintering furnace. Under a sintering pressure of 60 MPa, the temperature is raised to 1100°C at a rate of 100°C / min and sintered for 5 minutes to perform powder metallurgy. After the sintering, the furnace is cooled to room temperature to precipitate a certain amount of Cu-rich soft second phase in the hard phase TaMoNb matrix, and the grain size is controlled at the nanoscale to obtain a bulk alloy material TaMoNb5Cu;

[0059] (3) The bulk alloy material TaMoNb5Cu obtained in step (2) is subjected to surface deformation treatment by mechanical rolling. A ball with a diameter of 3 mm is placed in the ball. The rolling pass is 1 time, the reduction amount is 0.16 mm, and the rolling force is 1.5 MPa, thereby obtaining a TaMoNb5Cu alloy material with a double-layer heterogeneous structure.

[0060] Example 3

[0061] An alloy material consists of Ag powder (with a purity of 99.99% and a grain size of 192-213nm) and an equimolar amount of TiMo alloy powder (with a purity of 99.99% and a grain size of 192-213nm), and the molar ratio of the TiMo alloy powder to the Ag powder is 90:10.

[0062] A method for preparing an alloy material comprises the following steps:

[0063] (1) TiMo alloy powder and Ag powder were weighed in molar ratio, loaded into a high-energy ball mill, and stainless steel grinding balls with a diameter of 10 mm were added at a ball-to-material mass ratio of 5:1. The mixture was ball-milled at a speed of 875 r / min for 9 hours to mechanically alloy the powder and obtain a solid solution alloy powder.

[0064] (2) the solid solution alloy powder obtained in step (1) is loaded into a graphite mold, and the mold is placed in a spark plasma sintering furnace. Under a sintering pressure of 60 MPa, the temperature is raised to 1100° C. at a rate of 100° C. / min and sintered for 5 min to perform powder metallurgy. After the sintering, the furnace is cooled to room temperature to precipitate a certain amount of Ag-rich soft second phase in the hard phase TiMo matrix, and the grain size is controlled at the nanoscale to obtain a bulk alloy material TiMo10Ag;

[0065] (3) The bulk alloy material TiMo10Ag obtained in step (2) is subjected to surface deformation treatment by mechanical rolling. A ball with a diameter of 3 mm is placed therein. The number of rolling passes is 1, the reduction amount is 0.16 mm, and the rolling pressure is 1.5 MPa, thereby obtaining a TiMo10Ag alloy material with a double-layer heterogeneous structure.

[0066] Example 4

[0067] An alloy material consists of Ag powder (with a purity of 99.99% and a grain size of 192-213nm) and an equimolar amount of TiMo alloy powder (with a purity of 99.99% and a grain size of 192-213nm), and the molar ratio of the TiMo alloy powder to the Ag powder is 95:5.

[0068] A method for preparing an alloy material comprises the following steps:

[0069] (1) TiMo alloy powder and Ag powder were weighed in molar ratio, loaded into a high-energy ball mill, and stainless steel grinding balls with a diameter of 10 mm were added at a ball-to-material mass ratio of 5:1. The mixture was ball-milled at a speed of 875 r / min for 9 hours to mechanically alloy the powder and obtain a solid solution alloy powder.

[0070] (2) the solid solution alloy powder obtained in step (1) is loaded into a graphite mold, and the mold is placed in a spark plasma sintering furnace. Under a sintering pressure of 60 MPa, the temperature is raised to 1100° C. at a rate of 100° C. / min and the temperature is kept for 5 min to perform powder metallurgy. After the sintering, the furnace is cooled to room temperature to precipitate a certain amount of Ag-rich soft second phase in the hard phase TiMo matrix, and the grain size is controlled at the nanoscale to obtain a bulk alloy material TiMo5Ag;

[0071] (3) The bulk alloy material TiMo5Ag obtained in step (2) is subjected to surface deformation treatment by mechanical rolling. A ball with a diameter of 3 mm is placed therein. The number of rolling passes is 1, the reduction amount is 0.16 mm, and the rolling pressure is 1.5 MPa, thereby obtaining a TiMo5Ag alloy material with a double-layer heterogeneous structure.

[0072] Comparative Example 1

[0073] The only difference between Comparative Example 1 and Example 1 is that the alloy material of Comparative Example 1 is composed of 100% equimolar TaMoNb alloy powder (with a purity of 99.99% and a grain size of 192-213 nm), and does not contain Cu powder.

[0074] Figure 2 The HAADF-STEM image of the ND-SD cross-section microstructure of the TaMoNb alloy prepared in Comparative Example 1 under the friction track. The Pt layer is a protective layer during sample preparation. Figure 2It can be seen that there is a mechanical mixed layer with a thickness of about 200nm on the worn surface, which is mainly composed of wear debris formed by oxides and matrix; in the severe plastic deformation area with a depth of 1μm, the grains are severely elongated in the direction parallel to the sliding friction, forming lath-shaped nanocrystals almost parallel to the sliding direction; in the general deformation layer, this area is subject to less friction stress, but also undergoes certain plastic deformation, and the grains are elongated along the sliding direction; the bottom area is subject to very little friction stress and is an undeformed layer. For the severe plastic deformation area, due to the presence of the oxide second phase, the plastic deformation of the hard matrix phase is hindered, and stress concentration leads to the initiation of cracks (see the dotted box). As wear progresses, poor plasticity will cause the cracks to gradually expand, resulting in surface peeling and reducing the wear performance of the material.

[0075] Comparative Example 2

[0076] The only difference between Comparative Example 2 and Example 3 is that the alloy material of Comparative Example 2 is composed of 100% equimolar TiMo alloy powder (with a purity of 99.99% and a grain size of 192-213 nm), and does not contain Ag powder.

[0077] Comparative Example 3

[0078] The only difference between Comparative Example 3 and Example 1 is that the alloy material of Comparative Example 3 is composed of Cu powder (purity of 99.99%, grain size of 192-213 nm) and equimolar CoCr alloy powder (purity of 99.99%, grain size of 192-213 nm), and the molar ratio of CoCr alloy powder to Cu powder is 90:10.

[0079] Comparative Example 4

[0080] The only difference between Comparative Example 4 and Example 1 is that the alloy material of Comparative Example 4 is composed of Al powder (purity of 99.99%, grain size of 192-213 nm) and equimolar FeCo alloy powder (purity of 99.99%, grain size of 192-213 nm), and the molar ratio of FeCo alloy powder to Al powder is 90:10.

[0081] Comparative Example 5

[0082] The only difference between Comparative Example 5 and Example 1 is that the alloy material of Comparative Example 5 does not include the surface deformation treatment step (3) during the preparation process.

[0083] Comparative Example 6

[0084] The only difference between Comparative Example 6 and Example 3 is that the alloy material of Comparative Example 6 does not include the surface deformation treatment step (3) during the preparation process.

[0085] Performance Testing

[0086] The hardness, wear resistance, plasticity, grain size and density of the alloy materials prepared in Examples 1-4 and Comparative Examples 1-6 were tested, and the results are shown in Table 1.

[0087] Among them: a Vickers hardness tester is used to measure the Vickers hardness of the material; a ball-on-disc friction and wear testing machine is used, with a silicon nitride ball as the friction pair, a normal load of 5N, a sliding speed of 0.1m / s, and a sliding distance of 1000m to measure the friction and wear properties of the material; a universal testing machine is used to measure the plastic strain of the material; an electron backscatter diffraction probe is used to measure the grain size of the material; and a density balance is used to measure the density of the material.

[0088] Table 1:

[0089]

[0090] It can be seen from Table 1 that by comparing the test results of Examples 1-2 with Comparative Example 1 and Examples 3-4 with Comparative Example 2, it can be seen that after adding the soft second phase to the hard matrix phase, as the content of the soft second phase increases, the hardness of the material tends to gradually decrease, but can still maintain a relatively high hardness value (HV>500); the wear rate of the material tends to gradually decrease, and when the content of the soft second phase is 10%, the wear resistance is improved by about 3 times; the plastic strain of the material tends to gradually increase, and all have relatively high plastic strain values ​​(>26%).

[0091] Comparing the test results of Example 1 with those of Comparative Examples 3-4, it can be seen that Comparative Examples 3-4 use metal powders with a hard matrix phase and a soft second phase that are not used in Example 1. Due to the lack of a high-hardness hard phase, the hardness of the material is reduced by more than 170HV compared with Example 1, and the wear resistance is also reduced by more than 4 times. Although there is a large difference in hardness between the matrix phase and the second phase, the lack of coordinated deformation leads to a reduction in plasticity and wear resistance. At the same time, the problem of difficult solid solution between the matrix phase and the second phase causes the grain size to coarsen and reduces the density of the material. This shows that the present invention gives full play to the high hardness and strength of the hard matrix phase and the plasticity of the soft second phase by optimizing and reasonably compounding the material components, thereby improving the wear resistance of the material.

[0092] By comparing the test results of Example 1 with Comparative Example 5 and Example 3 with Comparative Example 6, it can be seen that the surface rolling treatment can effectively improve the wear resistance of the material.

[0093] Comparing the test results of Examples 1-4 and Comparative Examples 1-2 and 5-6, it can be seen that the grain size of Examples 1-4 and Comparative Examples 1-2 and 5-6 is 192-283nm, and the plastic deformation applied by the surface rolling treatment can promote grain refinement, and the grain size is reduced by more than 50nm, indicating that through the reasonable setting of the preparation process of the present invention, the growth of grains can be effectively avoided, and the obtained grains are all nanocrystalline. At the same time, the density of the alloy materials of Examples 1-4 and Comparative Examples 1-2 and 5-6 is >97%, and with the increase of the content of the soft second phase, the density of the material shows a gradually increasing trend, indicating that through the reasonable setting of the preparation process, the liquid soft phase can promote the sintering of the hard matrix phase and improve the density of the material.

[0094] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, without having to go through creative labor. Therefore, simple improvements made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the protection scope of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should belong to the protection scope of the present invention.

Claims

1. A plasticized wear-resistant alloy material, characterized in that: The alloy material has a double-layer heterogeneous structure, and the alloy material is composed of a hard matrix phase and a soft second phase; when the hard matrix phase is Ta, Mo, and Nb in equal moles, the soft second phase is Cu; when the hard matrix phase is Ti and Mo in equal moles, the soft second phase is Ag; The molar ratio of the hard matrix phase to the soft second phase is (90-95):(5-10); The grain size of the hard matrix phase is 190-220 nm, and the grain size of the soft second phase is 190-220 nm; The alloy material is prepared by a preparation method comprising the following steps: (1) mixing the metal powders of the hard matrix phase and the soft second phase, and then grinding them at a speed of 600-1000 r / min for 9-20 hours to mechanically alloy them to obtain a solid solution alloy powder; (2) Sintering the solid solution alloy powder at 1100-1500° C. for 3-8 minutes by spark plasma sintering to obtain a bulk alloy material; (3) Performing surface deformation treatment on the bulk alloy material to obtain the alloy material.

2. The plasticized wear-resistant alloy material according to claim 1, characterized in that: The purity of the hard matrix phase is ≥98%.

3. The plasticized wear-resistant alloy material according to claim 1, characterized in that: The purity of the soft second phase is ≥98%.

4. A method for preparing a plasticized wear-resistant alloy material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) mixing the metal powders of the hard matrix phase and the soft second phase, and then grinding them at a speed of 600-1000 r / min for 9-20 hours to mechanically alloy them to obtain a solid solution alloy powder; (2) Sintering the solid solution alloy powder at 1100-1500° C. for 3-8 minutes by spark plasma sintering to obtain a bulk alloy material; (3) Performing surface deformation treatment on the bulk alloy material to obtain the alloy material.

5. The method for preparing the plasticized wear-resistant alloy material according to claim 4, characterized in that: In step (3), the surface deformation treatment method is any one of rolling, shot peening, and laser shock strengthening.

6. The method for preparing the plasticized wear-resistant alloy material according to claim 5, characterized in that: The pressing amount of the rolling is 0.1-0.2 mm.

Citation Information

Patent Citations

  • High intensity low modulus in-situ synthesis ti-based composite material and preparation method thereof

    CN103194648A

  • Method of preparing tungsten-molybdenum-copper composite material by large current resistance sintering

    CN107937748A

  • Low modulus silver-containing anti-infection medical titanium alloy

    CN108300897A

  • Preparation method of antibacterial Ti-Nb-Zr-Ag alloy ingot

    CN109022853A

  • Tungsten-copper alloy unaffected by magnetic field as well as manufacturing method and application thereof

    CN111996430A