Sealing structure and sealing material for gas storage
By using calcium ion solution and bacterial liquid combined with a bacterial reinforcement layer of gelling material in the gas storage, the problem of easy cracking of the rigid sealing layer is solved, the air tightness and stability of the gas storage are improved, and the service life is extended. , and reduces operating costs and maintenance requirements.
Patent Information
- Application Number
- CN202410884420.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-03
AI Technical Summary
The rigid sealing layer used in existing gas storages is prone to cracking in environments of high temperature, high internal pressure, and high-frequency alternating loads, resulting in high leakage rates and affecting the operating efficiency and safety of the power station.
The bacterial reinforcement layer is prepared by using a calcium ion solution and a bacterial liquid that can react with carbon-containing compounds and calcify and deposit after metabolism. Combined with gelling materials, a calcified structure is formed to cooperate with the sealing layer to enhance the air tightness and stability of the gas storage. , reduce the risk of leakage.
It can effectively prevent leakage, extend the service life of the gas storage, enhance the strength and toughness of the inner wall, reduce operating costs, and reduce the need for manual maintenance. It has the advantages of being environmentally friendly, pollution-free, and easy to operate.
Smart Images

Figure CN118423599B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sealing structures, and specifically discloses a sealing structure and a sealing material for a gas storage. Background Art
[0002] The gas storage reservoir of a compressed air energy storage power station is a key energy storage facility system. Its operating scenario is special (high temperature, high internal pressure, high-frequency alternating load and other stress characteristics), which is significantly different from traditional underground projects (hydropower, transportation). Therefore, more stringent requirements are placed on the sealing of the gas storage reservoir.
[0003] The sealing of the gas storage reservoir of a compressed air energy storage power station is a core factor affecting the operating efficiency of the power station. It plays a vital role in the success or failure of the operation of the compressed air energy storage power station. The size of its leakage rate has a significant impact on the operating efficiency of the power station.
[0004] In the existing technology, a rigid sealing layer is usually set on the lining of the gas storage to seal the gas storage to reduce the leakage rate. However, due to the special environment of high temperature, high internal pressure and high-frequency alternating load, the rigid sealing layer is easy to crack, and the density and width of the cracks are large, which seriously affects the operation efficiency of the power station and poses great safety hazards. Summary of the invention
[0005] The object of the present invention is to provide a sealing structure and a sealing material for a gas storage reservoir, so as to solve the technical problem that the rigid sealing layer used in the existing gas storage reservoir is prone to cracking.
[0006] A first aspect of the present invention provides a sealing structure for a gas storage, comprising a sealing layer and a bacteria enhancement layer;
[0007] The sealing layer is arranged on the lining of the gas storage reservoir;
[0008] The bacteria enhancement layer is disposed on the sealing layer;
[0009] The components of the bacterial enhancement layer include a calcium ion solution and a bacterial solution that can react with carbon-containing compounds and form calcification deposits after metabolism. The bacterial solution is obtained by culturing Gram-negative anaerobic sulfur-reducing bacteria in a sulfate-containing culture medium.
[0010] Preferably, the components of the bacteria-enhanced layer further include a gelling material;
[0011] The mass ratio of the bacterial cells in the bacterial liquid to the gelling material is 1:0.7-0.9.
[0012] Preferably, the gelling material is polyvinyl alcohol or alginate.
[0013] Preferably, the ratio of the concentration of sulfate in the sulfate to the concentration of Gram-negative anaerobic sulfur-reducing bacteria is 1:1;
[0014] The concentration of calcium ions in the calcium ion solution is greater than or equal to twice the concentration of sulfate radicals.
[0015] Preferably, the initial thickness of the bacteria-enhanced layer before calcification is 2 mm to 5 mm.
[0016] Preferably, the calcified thickness of the bacteria-enhanced layer is less than or equal to 1 cm.
[0017] Preferably, the sealing layer is a flexible sealing layer.
[0018] The second aspect of the present invention provides a sealing material for a gas storage, comprising a calcium ion solution and a bacterial solution that can react with carbon-containing compounds and calcify and deposit after metabolism, wherein the bacterial solution is obtained by culturing Gram-negative anaerobic sulfur-reducing bacteria in a sulfate-containing culture medium.
[0019] Preferably, a gelling material is also included, and the mass ratio of the Gram-negative anaerobic sulfur-reducing bacteria in the bacterial liquid to the gelling material is 1:0.7-0.9.
[0020] Preferably, the ratio of the concentration of sulfate in the sulfate to the concentration of Gram-negative anaerobic sulfur-reducing bacteria is 1:1;
[0021] The concentration of calcium ions in the calcium ion solution is greater than or equal to twice the concentration of sulfate radicals.
[0022] Compared with the prior art, the sealing structure and sealing material for gas storage of the present invention have the following beneficial effects:
[0023] The present invention uses a bacterial liquid that can react with carbon-containing compounds and calcify and deposit after metabolism to prepare a bacterial reinforcement layer. The calcified structure obtained after calcification cooperates with the original sealing layer and is not easy to crack, which can improve the air tightness and stability of the gas storage reservoir, effectively prevent leakage of the gas storage reservoir and the development of cracks in the concrete lining, extend the service life of the gas storage reservoir, and reduce operating costs. Furthermore, the calcified structure obtained after calcification cooperates with the original sealing layer to enhance the strength and toughness of the inner wall of the gas storage reservoir, help resist changes in the internal pressure of the gas storage reservoir, and improve the reliability of the operation of the gas storage reservoir. In addition, the calcified structure formed is a natural protective layer, therefore, the manual maintenance of the sealing layer can be reduced. Compared with the traditional manual maintenance method, it has the advantages of low cost, good effect, environmental protection, pollution-free, and easy operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic cross-sectional view of a gas storage before calcification of the bacteria-enhanced layer according to an embodiment of the present invention;
[0025] Figure 2This is a schematic cross-sectional view of a gas storage reservoir after the bacteria-enhanced layer is calcified according to an embodiment of the present invention.
[0026] In the figure: 1 is the lining; 2 is the sealing layer; 3 is the bacteria enhancement layer; 4 is the calcification structure. DETAILED DESCRIPTION
[0027] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present invention.
[0028] A first aspect of an embodiment of the present invention provides a sealing structure for a gas storage, such as Figure 1 and Figure 2 As shown, it includes a sealing layer 2 and a bacterial enhancement layer 3; wherein the sealing layer 2 is arranged on the lining 1 of the gas storage reservoir; the bacterial enhancement layer 3 is arranged on the sealing layer 2; wherein the components of the bacterial enhancement layer 3 include a calcium ion solution and a bacterial liquid that can react with carbon-containing compounds after metabolism and calcify and deposit, and the above-mentioned bacterial liquid is a bacterial liquid obtained by culturing Gram-negative anaerobic sulfur-reducing bacteria in a medium containing sulfate. The above-mentioned carbon-containing compound can be CH2O; the calcium ion solution can specifically be a calcium chloride solution, a calcium acetate solution, etc.
[0029] The present invention uses a bacterial liquid that can react with carbon-containing compounds and calcify and deposit after metabolism to prepare a bacterial reinforcement layer 3. The calcified structure 4 obtained after calcification cooperates with the original sealing layer 2, is not easy to crack, can improve the air tightness and stability of the gas storage, effectively prevent leakage of the gas storage and the development of cracks in the concrete lining, extend the service life of the gas storage, and reduce operating costs. Furthermore, the calcified structure 4 obtained after calcification cooperates with the original sealing layer 2, and can also enhance the strength and toughness of the inner wall of the gas storage, help resist changes in the internal pressure of the gas storage, and improve the reliability of the gas storage. In addition, the formed calcified structure 4 is a natural protective layer, therefore, it can reduce the manual maintenance of the sealing layer 2. Compared with the traditional manual maintenance method, it has the advantages of low cost, good effect, environmental protection, pollution-free, and easy operation.
[0030] The bacterial liquid used in the embodiment of the present invention is a bacterial liquid obtained by culturing Gram-negative anaerobic sulfur-reducing bacteria in a medium containing sulfate. The Gram-negative anaerobic sulfur-reducing bacteria can cause sulfate to undergo a reduction reaction with carbon-containing compounds to obtain hydrogen sulfide and bicarbonate, and the bicarbonate reacts with calcium ions to generate calcium carbonate deposition to form a calcified structure 4. The concentration ratio of sulfate in the above-mentioned sulfate to the concentration of Gram-negative anaerobic sulfur-reducing bacteria is 1:1, and the concentration of calcium ions in the calcium ion solution is greater than or equal to 2 times the concentration of sulfate, thereby ensuring the calcification deposition effect. Gram-negative anaerobic sulfur-reducing bacteria can withstand at least 15MPa of pressure and 90° of high temperature, so they can survive in a high temperature, high pressure and humid environment, and then react with carbon-containing compounds in the air through metabolism to cause calcium carbonate to be supersaturated and precipitate on its surface to form a calcified structure 4. At the same time, when the gas storage is a high-pressure gas storage of a compressed air energy storage power station, the 7-10MPa circulating humid environment of the gas storage can promote the division and metabolism of bacteria, thereby promoting the generation and accumulation of calcified substances. The principle of the calcified structure 4 formed by the calcified deposition of Gram-negative anaerobic sulfur-reducing bacteria in the embodiment of the present invention is as follows:
[0031] Under high temperature and high pressure, anaerobic sulfur-reducing bacteria reduce sulfate and carbon-containing compounds to generate hydrogen sulfide and bicarbonate through metabolic processes. At the same time, bicarbonate reacts with calcium ions to form calcium carbonate. The main reaction process is as follows:
[0032] Reduction reaction:
[0033] SO4 2− + 2CH2O → H2S + 2HCO3 −
[0034] Calcium carbonate deposition reaction:
[0035] HCO3 − + Ca 2+ → CaCO3 +H +
[0036] Overall reaction:
[0037] SO4 2− +2CH2O + 2Ca 2+ →H2S + 2CaCO3 + 2H +
[0038] In order to make the calcified structure 4 formed by the bacteria-enhanced layer 3 more uniform and improve the adhesion and biomineralization ability of bacteria in the bacteria-enhanced layer 3, the embodiment of the present invention further adds a gelling material to the components of the bacteria-enhanced layer 3; wherein the gelling material is polyvinyl alcohol or alginate.
[0039] In the embodiment of the present invention, the cultured bacterial liquid is mixed into the gelling material to form a bacterial gelling agent, and then the bacterial gelling agent is mixed with a calcium ion solution. The use of the gelling material as a carrier of bacteria can increase the adhesion and biomineralization ability of the bacteria.
[0040] In order to ensure the porosity of the bacterial gelling agent, thereby providing suitable growth and metabolism space for bacteria, the mass ratio of bacteria to gelling material in the bacterial liquid of the embodiment of the present invention is 1:0.7-0.9, for example, 1:0.7, 1:0.8, 1:0.9, etc. The high-concentration bacterial gelling agent has good fluidity and curability, and is easy to be evenly covered and fixed on the sealing layer 2.
[0041] In the embodiment of the present invention, the mixture of the bacterial liquid and the calcium ion solution or the mixture of the bacterial gelling agent and the calcium ion solution prepared above is evenly covered on the sealing layer 2 of the gas storage by spraying, smearing, pouring, etc., to form a bacterial enhancement layer 3. The initial thickness D1 of the bacterial enhancement layer 3 before calcification is 2 mm to 5 mm, which can ensure that it is closely combined with the sealing layer 2, and the bacterial enhancement layer is not too thick, resulting in flow and block falling on the top.
[0042] In order to prevent the thickness of the calcified structure 4 from affecting the volume of the gas storage reservoir and thus affecting the power generation efficiency, the thickness D2 of the calcified structure 4 in the embodiment of the present invention should be less than or equal to 1 cm. Specifically, according to the operation and maintenance conditions of the power station, the bacterial activity and the thickness of the calcified structure 4 are regularly detected, and the bacterial growth is controlled by adjusting the metabolic environment of the bacterial liquid to control the precipitation of its calcified substances, and the optimal living environment of the bacterial group is artificially and dynamically controlled to ensure the strength and density of the calcified structure 4.
[0043] The sealing layer 2 in the embodiment of the present invention can be a rigid sealing layer or a flexible sealing layer. Since the flexible sealing layer has the characteristics of good temperature adaptability and strong deformation adaptability, the embodiment of the present invention preferably uses a flexible sealing layer. Furthermore, the existing flexible sealing layer mostly contains polymer substances, such as polyurethane. Polymer substances will release organic pollutants under high temperature and high pressure environment, and the bacterial enhancement layer 3 in the embodiment of the present invention can react with carbon-containing compounds in organic pollutants during metabolism and calcification, thereby reducing the concentration of organic pollutants in the gas storage reservoir, improving the gas environment of the gas storage reservoir, and will not cause secondary pollution.
[0044] The second aspect of the present invention provides a sealing material for a gas storage, comprising a calcium ion solution and a bacterial liquid that can react with carbon-containing compounds and calcify and deposit after metabolism, wherein the bacterial liquid is a liquid obtained by culturing Gram-negative anaerobic sulfur-reducing bacteria in a medium containing sulfate. The sealing material uses fewer components, has low preparation difficulty, and has good sealing performance.
[0045] In order to make the calcification structure 4 formed by the bacteria-enhanced layer 3 more uniform and improve the adhesion and biomineralization ability of the bacteria in the bacteria-enhanced layer 3, the embodiment of the present invention further adds a gelling material to the components of the bacteria-enhanced layer 3, wherein the gelling material is polyvinyl alcohol or alginate, and the mass ratio of Gram-negative anaerobic sulfur-reducing bacteria in the bacterial liquid to the gelling material is 1:0.7~0.9.
[0046] The ratio of the concentration of sulfate in the sulfate to the concentration of Gram-negative anaerobic sulfur-reducing bacteria is 1:1, and the concentration of calcium ions in the calcium ion solution is greater than or equal to twice the concentration of sulfate, thereby ensuring the calcification deposition effect.
[0047] The effects of the sealing structure and sealing material for gas storage of the present invention will be verified by specific experiments below.
[0048] 1. Purpose of the experiment
[0049] The anaerobic sulfur-reducing bacteria were verified to cause sulfate to undergo reduction reaction with carbon-containing compounds at different temperatures and pressures to generate hydrogen sulfide and bicarbonate, while bicarbonate reacted with calcium ions to form calcium carbonate deposition.
[0050] 2. Materials and Equipment
[0051] Bacterial liquid, calcium ion solution, high-pressure reactor, CH2O, pH meter, thermometer, pressure gauge, microscope, X-ray diffractometer (XRD)
[0052] 3. Experimental steps
[0053] Bacterial culture: Gram-negative anaerobic sulfur-reducing bacteria are cultured in a sulfate-containing medium.
[0054] Reactor preparation: Inject the cultured bacterial solution, calcium ion solution and CH2O into the high-pressure reactor and seal the reactor.
[0055] Reaction conditions: different temperatures and pressures were set, and the reaction time was 48 hours.
[0056] Reaction monitoring: Use pH meter, thermometer and pressure gauge to monitor the reaction conditions in the reactor in real time.
[0057] Sample collection: After the reaction is completed, take out the samples in the reactor and use a microscope to observe the calcification deposition on the bacterial surface.
[0058] Result analysis: Calcium carbonate deposits in the product were extracted, and the structure of calcium carbonate deposits in the sample was analyzed using an X-ray diffractometer (XRD); its content was characterized by calcification concentration, and the unit of calcification concentration was mg / L, indicating the mass of calcium carbonate that can be generated per liter of solution when the above-prepared solution is uniformly covered on the sealing layer 2 of the gas storage to form a bacteria-enhanced layer 3 by spraying, smearing, pouring, etc.
[0059] 1) Strength analysis: The calcified sediment samples were placed in a standard mold to make standard size specimens. After curing to a stable state, the compressive strength test was performed. After multiple tests, the average value was taken as the compressive strength of the calcified structure 4. The compressive strength data of the calcified structure under different temperatures and pressures are recorded in Table 1 below.
[0060] 2) Leakage analysis: Connect the high-pressure gas storage tank to the sealing test device and set the initial pressure (e.g. 10MPa). Start the gas flow meter and pressure sensor, record the gas flow through the calcified sediment sample within a certain period of time (24 hours), and take the average value as the leakage of the calcified sediment after multiple tests. Calculate the leakage rate (%) of the calcified sediment based on the gas flow and test time.
[0061] Table 1 Experimental results
[0062]
[0063] 4. Conclusion
[0064] Through the above experimental results, the following conclusions can be drawn:
[0065] 1) Effect of temperature and pressure: With the increase of temperature and pressure, the concentration of calcification and the compressive strength of the obtained calcified structure 4 increased significantly, and the leakage rate in the sealing evaluation decreased significantly, indicating that the high temperature and high pressure environment is conducive to the metabolism of bacteria and the formation of calcification deposition.
[0066] 2) Influence of the mass ratio of Gram-negative anaerobic sulfur-reducing bacteria to cementitious materials: With the increase of the mass ratio of Gram-negative anaerobic sulfur-reducing bacteria to cementitious materials, the calcification concentration and the compressive strength of the resulting calcified structure 4 also increased significantly, and the leakage rate in the sealing evaluation was significantly reduced, indicating that the addition of cementitious materials can make the calcification structure formed by the bacteria-enhanced layer more uniform, enhance the adhesion and biomineralization ability of the bacterial structure, and significantly improve the sealing and strength of the sealing layer.
[0067] 3) Optimal conditions: At 90°C, 10MPa, and a mass ratio of anaerobic sulfur-reducing bacteria to cementitious materials of 1:0.9, the calcification concentration and the compressive strength of the resulting calcified structure 4 were the highest, the leakage rate in the sealing evaluation was the lowest, and the calcification effect was the most significant. The compressive strength and sealing evaluation of the calcified structure 4 in the experimental results also show that high temperature and high pressure are conducive to the formation of high-strength, low-leakage calcified deposits.
[0068] The sealing structure for gas storage of the present invention has good sealing performance, simple structure and convenient construction. The sealing material for gas storage of the present invention has few components, low preparation difficulty, convenient transportation and storage, and can be used in various gas storages with a wide range of applications.
[0069] The above are only several embodiments of the present invention and are not intended to limit the present invention in any form. Although the present invention is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, using the above disclosed technical content to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A sealing structure for a gas storage, characterized in that: Includes sealing layer and bacteria-enhancing layer; The sealing layer is arranged on the lining of the gas storage reservoir; The bacteria enhancement layer is arranged on the sealing layer, and the arrangement method is specifically: the bacteria enhancement layer is evenly covered on the sealing layer by spraying, painting or pouring; The components of the bacterial reinforcement layer include gelling material, calcium ion solution and bacterial liquid which can react with carbon-containing compounds and form calcification deposits after metabolism. The bacterial liquid is obtained by culturing Gram-negative anaerobic sulfur-reducing bacteria in a sulfate-containing culture medium.
2. The sealing structure for a gas storage according to claim 1, characterized in that: The mass ratio of the Gram-negative anaerobic sulfur-reducing bacteria in the bacterial liquid to the gelling material is 1:0.7-0.
9.
3. The sealing structure for gas storage according to claim 2, characterized in that: The gelling material is polyvinyl alcohol or alginate.
4. The sealing structure for a gas storage according to any one of claims 1 to 3, characterized in that: The ratio of the concentration of sulfate in the sulfate to the concentration of Gram-negative anaerobic sulfur-reducing bacteria is 1:1; The concentration of calcium ions in the calcium ion solution is greater than or equal to twice the concentration of sulfate radicals.
5. The sealing structure for a gas storage according to claim 1, characterized in that: The initial thickness of the bacterial reinforcement layer before calcification is 2 mm to 5 mm.
6. The sealing structure for a gas storage according to claim 1, characterized in that: The calcified thickness of the bacteria enhanced layer is less than or equal to 1 cm.
7. The sealing structure for a gas storage according to claim 1, characterized in that: The sealing layer is a flexible sealing layer.
8. A sealing material for a gas storage, characterized in that: The bacterial reinforcement layer used for preparing the sealing structure for gas storage as claimed in any one of claims 1 to 7 comprises a gelling material, a calcium ion solution and a bacterial liquid which can react with carbon-containing compounds and form calcification deposits after metabolism, wherein the bacterial liquid is obtained by culturing Gram-negative anaerobic sulfur-reducing bacteria in a sulfate-containing culture medium.
9. The sealing material for gas storage according to claim 8, characterized in that: The mass ratio of the Gram-negative anaerobic sulfur-reducing bacteria in the bacterial liquid to the gelling material is 1:0.7-0.
9.
10. The sealing material for gas storage according to claim 8, characterized in that: The ratio of the concentration of sulfate in the sulfate to the concentration of Gram-negative anaerobic sulfur-reducing bacteria is 1:1; The concentration of calcium ions in the calcium ion solution is greater than or equal to twice the concentration of sulfate radicals.
Citation Information
Patent Citations
Method for preventing leakage in geological storage process of carbon dioxide
CN117533695A
Underground gas storage based on partitioned lining structure
CN117569870A