A method for preparing polyester for high-viscosity bottles using a final polycondensation reactor
By using a differential rotating cage stirrer and a ring stirrer combination in the final polycondensation reactor, combined with a vacuum system and temperature control, the problems of low mass transfer and devolatilization efficiency and large reactor volume are solved, and efficient preparation is achieved High-viscosity polyester for bottles improves melt quality and efficiency.
Patent Information
- Application Number
- CN202410897720.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-05
AI Technical Summary
When preparing polyester for high-viscosity bottles, the existing final polycondensation reactor has problems such as low mass transfer and devolatilization efficiency, excessive reactor volume, high cost, and uneven molecular weight distribution, and the combined polymerization reactor has problems such as increased viscosity. The final melt has poor fluidity and easily adheres to the spindle, affecting the devolatilization efficiency.
A final polycondensation reactor is designed, which uses a combination of a cage stirrer and a ring stirrer with differential rotation. The first and second power systems drive the cage stirrer and the ring stirrer to perform differential rotation respectively. The combination Vacuum system and temperature control, adjust the rotation speed and viscosity sensor in real time to improve film forming efficiency, and improve space utilization through the transfer stirrer.
It achieves efficient mass transfer and devolatilization, reduces the polycondensation reaction time, improves melt quality and overall efficiency, reduces energy and material consumption, and the intrinsic viscosity of the melt reaches 0.70dL/g~1.0dL/g, which meets the requirements of high Preparation requirements for polyester for sticky bottles.
Smart Images

Figure CN118437258B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester processing, in particular to a method for preparing polyester for high-viscosity bottles using a final polycondensation reactor. Background Art
[0002] Bottle polyester is made of raw materials ethylene glycol (EG), terephthalic acid (PTA), and isophthalic acid (IPA) mixed into slurry at a certain molar ratio. The slurry completes esterification reaction at a certain temperature and pressure to produce ethylene terephthalate (BHET) and ethylene isophthalate (BHEI), and then undergoes pre-polycondensation and final polycondensation to produce isophthalic acid-modified polyethylene terephthalate (PET). The intrinsic viscosity of basic bottle PET is generally 0.62dL / g, and then the intrinsic viscosity of PET is increased to more than 0.80dL / g through solid phase viscosity increase. At present, the production process of bottle polyester is mainly divided into two types: solid phase viscosity enhancement and liquid phase viscosity enhancement. Among them, the solid phase viscosity enhancement technology is relatively mature. Representative enterprises include Buhler of Switzerland, Xingke of Italy, Chemtex of the United States, and Yizheng Chemical Fiber of China. Hot nitrogen / air is used to remove small molecules in PET solid particles to increase the intrinsic viscosity of PET. However, this technology has problems such as high energy consumption and material consumption, uneven molecular weight distribution of PET products, and high dust. The liquid phase viscosity enhancement technology is to make PET reach a higher intrinsic viscosity (generally above 0.78dL / g) in the final polycondensation reactor, and then realize the preparation of bottle PET through low-temperature formaldehyde removal. This technology has the advantages of low energy consumption and material consumption, uniform viscosity inside and outside the particles, and less dust, but it puts forward higher requirements on the structural form of the final polycondensation reactor.
[0003] The final polycondensation reactor used in the conventional final polycondensation reaction process mostly adopts a horizontal disc reactor. The working principle of this reactor is to make the PET melt adhere to the surface of the disc with the help of the rotation of the disc installed inside the reactor after the pre-polycondensation treatment, and form a sagging film of a certain thickness under the action of gravity and the scraper installed on the inner wall of the cylinder. As the liquid film continues to slide down, new interfaces are continuously generated inside the reactor disc, forming an interface renewal phenomenon, so that the ethylene glycol molecules released from the PET can escape at the interface and the sagging film, so that the molecular chain gradually grows. Under the action of the rotation of the disc and the replacement of the liquid level, the polycondensation reaction continues to proceed, and polyethylene terephthalate is obtained.
[0004] However, since the liquid film formed in the conventional final polycondensation reactor is perpendicular to the driving axis of the disc, that is, the liquid film is formed only in the plane of the disc, the melt surface area used for evaporation of ethylene glycol in PET is small. In order to increase the evaporation area and the gas phase flow area, a commonly used method is to increase the volume of the cylinder and add multiple sets of discs inside the cylinder. However, the final polycondensation reactor using this method has the problems of not being able to fully utilize the internal space of the reactor, the reactor volume is too large, the space occupied is too large, and the cost is too high.
[0005] With the innovation of technology, combined polymerization reactors combining cage reactors and disc reactors have emerged in the market, such as a combined polymerization reactor in the field of polyester production equipment disclosed in Chinese Patent No. CN201684605U (CN201020175319.5), and a polymerization reactor and a polyester production method disclosed in Chinese Patent No. CN106268591A (CN201610848575.8). However, the viscosity of the melt in the existing combined polymerization reactor gradually increases with the reaction process, and the fluidity becomes poor. The high-viscosity melt at the rear end is easy to adhere to the main shaft, affecting the mass transfer and devolatilization efficiency of the melt. The front and rear rotation speeds of the cage reactor part are consistent. Since the viscosity of this part varies greatly, when the front and rear rotation speeds are consistent, the difference in the film formation of the melt before and after will be large. The melt at the rear end may not be able to form a film at a higher rotation speed, resulting in a low devolatilization efficiency, thereby affecting the overall mass transfer and devolatilization efficiency. Summary of the invention
[0006] In order to overcome the deficiencies of the prior art, the object of the present invention is to provide a method for preparing high-viscosity bottle polyester using a final polycondensation reactor, which has the advantages of forming differential rotation and improving mass transfer and devolatilization efficiency.
[0007] The purpose of the present invention is achieved by the following technical solutions:
[0008] According to an embodiment of the present disclosure, a method for preparing high-viscosity bottle polyester in a final polycondensation reactor is provided. The method is implemented based on a final polycondensation reactor, and the final polycondensation reactor comprises:
[0009] A cylinder, wherein the front end of the cylinder is provided with a feed inlet, the rear end is provided with a discharge outlet, and the middle part and the top of the rear end of the cylinder are both provided with gas phase outlets connected to the vacuum system;
[0010] A first power system and a second power system are respectively arranged at the front and rear sides of the cylinder, the first power system is connected to a first main shaft, and the second power system is connected to a second main shaft;
[0011] A cage stirrer connected to the first main shaft, the cage stirrer comprising: at least two cage frames arranged in sequence along the axial direction of the cylinder, and a transmission arranged between adjacent cage frames for reducing the rotation speed of each cage frame in sequence according to a predetermined ratio, and a first viscosity sensor and a second viscosity sensor are respectively arranged on the front side and the rear side of the cage stirrer;
[0012] A transfer stirrer fixed at the end of the cage stirrer, the transfer stirrer comprising: an inner fixed ring, an outer support ring, and a plurality of reaction disks fixed between the inner fixed ring and the outer support ring, the inner wall of the cylinder being rotatably connected to a plurality of support rollers that abut and support the outer support ring; and
[0013] a circular agitator connected to the second main shaft and rotatably connected to the intermediate agitator;
[0014] The method comprises: continuously feeding a polyester melt material for bottles having an IPA content of (0.25-3.0)% and an intrinsic viscosity of 0.15 dL / g-0.40 dL / g into the final polycondensation reactor, adjusting the output speed of the first power system according to the viscosity value detected by the first viscosity sensor and / or the second viscosity sensor, reacting for 50 min-150 min under the conditions of a temperature of 265° C.-290° C. and an absolute pressure of 0 Pa-2000 Pa, and preparing a high-viscosity polyester melt for bottles having an intrinsic viscosity of 0.70 dL / g-1.0 dL / g.
[0015] To implement the above technical solution, during the polycondensation reaction, the pre-polycondensation melt is fed into the cylinder from the feed port, the cage stirrer is driven to rotate by the first power system through the first main shaft, the cage stirrer synchronously drives the transfer stirrer to rotate during the rotation process, and the annular stirrer is driven to rotate by the second power system through the second main shaft. Since the annular stirrer is rotatably connected with the transfer stirrer, the two can rotate at different speeds respectively, thereby meeting the differential stirring requirements of the front and rear melts in different viscosity states;
[0016] In the initial state, the first power system is controlled to rotate at a predetermined speed to provide power according to the pre-detected viscosity value of the pre-condensation melt. During the rotation of the cage stirrer, the melt viscosity at the front and rear sides of the cage stirrer is detected by the first viscosity sensor and the second viscosity sensor respectively, and the output speed of the first power system is adjusted according to the real-time measured viscosity value, so that the cage stirrer can be adjusted to rotate at a more reasonable speed according to the viscosity state of the melt, so that the melt can be efficiently devolatilized by film formation. The melt located in the annular stirrer part is in a high viscosity state, and the second power system is usually controlled to rotate at a predetermined low speed.
[0017] Meanwhile, the cage stirrer is composed of a plurality of cage frames, and the adjacent cage frames are connected in a transmission form to rotate at a differential speed with the rotation speed decreasing in sequence, so that the film-forming states at the front section and the rear section of the cage stirrer are similar, and the mass transfer and devolatilization efficiency at the front section and the rear section are kept similar, which is beneficial to improving the overall mass transfer and devolatilization efficiency; and the transfer stirrer arranged between the cage stirrer and the annular stirrer, on the one hand, can replace the supporting structure in the existing technology to provide support for the rotating free ends of the cage stirrer and the annular stirrer, and on the other hand, can also stir the melt to form a film through the reaction disk, and can further improve the utilization rate of the internal space of the cylinder to further improve the devolatilization efficiency;
[0018] By controlling the temperature in the cylinder to 265℃~290℃ and the absolute pressure to 0Pa~2000Pa, and evacuating the cylinder by the vacuum system at the gas phase outlet, the cylinder is in a high vacuum state. When the pre-condensation melt is fed into the cylinder, the melt is lifted up by the cage frame during the rotation of the cage frame stirrer, and forms a film under the action of gravity during the rising and falling process, and undergoes a condensation reaction. Low molecular substances and alcohol reaction products are extracted from the gas phase outlet, the molecular chains of the polymer increase, the degree of polymerization increases, and the content of ethylene glycol in the melt and the ethylene glycol produced by the condensation reaction are uniform. The melt viscosity is relatively high under the action of vacuum and increases rapidly. Through the differential rotation of different cage bodies, the melt in the front section and the rear section of the cage stirrer can be effectively filmed, and then the melt is filmed in turn through the transfer stirrer and the ring stirrer, so that the characteristic viscosity of the melt finally reaching the discharge port is 0.70dL / g-1.0dL / g, and the preparation of the polyester melt for high-viscosity bottles can be completed. The final polycondensation reactor and the preparation method of the present invention have high film-forming efficiency, can effectively improve the mass transfer and devolatilization efficiency, reduce the polycondensation reaction time, and improve the melt quality.
[0019] In some exemplary embodiments, the cage frame includes: a frame portion, and mounting plates fixed to both sides of the frame portion, the mounting plates are provided with a transmission shaft, and the transmission shaft can be connected to the power input end / power output end of the transmission.
[0020] To implement the above technical solution, the cage frame is connected and fixed to the first main shaft and the transmission through the mounting plate, and the frame part is hollow as a whole, which can effectively prevent high-viscosity melt from sticking to the shaft, prevent the melt from coking due to long-term heating, and improve the melt quality.
[0021] In some exemplary embodiments, reinforcing ribs are provided inside the frame portion, and a plurality of cage spokes with trapezoidal cross sections are provided around the outer periphery of the frame portion, and the minimum gap between the highest point of the cage spokes and the inner wall of the cylinder is 5 to 20 mm.
[0022] To implement the above technical scheme, the structural strength of the frame portion can be improved by arranging reinforcing ribs, thereby ensuring that the frame portion does not deform during rotation. The cage frame spokes are provided to help the cage frame agitator scrape off the melt attached to the inner wall of the cylinder during rotation, thereby preventing the melt from coking due to long-term heating after hanging on the wall. The frame portion can perform parallel film drawing on the melt, and the reinforcing ribs and cage frame spokes can perform vertical film formation on the melt, thereby improving the film forming effect and devolatilization efficiency.
[0023] In some exemplary embodiments, the transmission includes: a housing, a driving gear and a driven gear rotatably connected to the housing and coaxially arranged, and a transmission gear set arranged between the driving gear and the driven gear for speed conversion, the driving gear and the driven gear are respectively connected to the transmission shaft of the adjacent cage frame, and the transmission is fixed to the cylinder through supporting feet.
[0024] To implement the above technical solution, power transmission between adjacent cage frames is achieved through the driving gear, the driven gear and the transmission gear set. By setting a reasonable transmission ratio between the driving gear, the transmission gear set and the driven gear, the rotation speed of each cage frame can be reduced in sequence.
[0025] In some exemplary embodiments, the cage frame is provided in three groups, and the speed ratios of the three groups of cage frames are 1: (0.75-0.9): (0.5-0.7) respectively. Adjusting the output speed of the first power system according to the viscosity value detected by the first viscosity sensor and / or the second viscosity sensor specifically includes:
[0026] If the viscosity value measured by the first viscosity sensor is 0.15 dL / g to 0.25 dL / g, the output speed of the first power system is controlled to be 6 rpm to 10 rpm;
[0027] If the viscosity value measured by the first viscosity sensor is 0.25 dL / g to 0.35 dL / g, the output speed of the first power system is controlled to be 4.5 rpm to 6 rpm;
[0028] If the viscosity value measured by the first viscosity sensor is 0.35 dL / g to 0.40 dL / g, the output speed of the first power system is controlled to be 3 rpm to 4.5 rpm; or,
[0029] If the viscosity value measured by the second viscosity sensor is 0.55 dL / g to 0.70 dL / g, the output speed of the first power system is controlled to be 5 rpm to 6.5 rpm.
[0030] To implement the above technical solution, since when the viscosity value increases, if the rotation speed is too fast, it will make it difficult to form a film in time or the thickness of the liquid film will be too large. Therefore, when the melt viscosity increases, the rotation speed needs to be appropriately reduced. According to the above strategy, the output speed of the first power system is adjusted according to the viscosity value detected by the first viscosity sensor and / or the second viscosity sensor, so that reasonable speed control can be performed corresponding to different viscosity gradients.
[0031] In some exemplary embodiments, the inner side of the reaction disk is fixed to the inner fixed ring, and the outer side is fixed to the outer support ring. The reaction disk is provided with a plurality of reaction grooves and / or reaction holes. The support rollers are arranged near the middle of the cylinder and at least two groups are symmetrically arranged.
[0032] To implement the above technical solution, reaction grooves and / or reaction holes are arranged on the reaction disk to facilitate the passage of the melt and film formation. The height of the melt in the cylinder is usually not higher than half of the height of the cylinder. Therefore, the support plate is arranged close to the middle of the cylinder to avoid immersing the support roller in the melt and affecting its rotation.
[0033] In some exemplary embodiments, a stepped mounting section is provided at one end of the inner fixed ring close to the annular agitator, and the stepped mounting section is used for being rotatably connected to the annular agitator.
[0034] The implementation of the above technical solution facilitates the rotational connection between the transfer agitator and the annular agitator.
[0035] In some exemplary embodiments, the annular agitator includes: two oppositely arranged faceplates, a plurality of annular spokes arranged between the two faceplates, and a plurality of annular agitating elements fixed to the annular spokes and arranged along the axial direction of the cylinder, wherein one of the faceplates is fixed to the second main shaft, and the other faceplate is fixed with a linkage shaft rotatably connected to the step mounting section.
[0036] To implement the above technical scheme, the second main shaft and the transfer agitator are installed and connected through the flower disc, and the connection and fixation of each ring agitator are achieved through the ring spokes. The melt is pulled into a film in parallel by the ring stirring piece and the melt is pulled into a film vertically by the ring spokes, thereby improving the film forming effect and the devolatilization efficiency. The ring agitator is hollow as a whole, which can effectively prevent high-viscosity melt from sticking to the shaft, prevent the melt from coking due to long-term heating, and improve the melt quality.
[0037] In some exemplary embodiments, the annular stirring element includes: a plurality of connecting ribs fixed to each of the annular spokes, an outer ring body fixed to the ends of the connecting ribs, and a plurality of inner ring bodies fixed to the connecting ribs, and the minimum gap between the outer ring body and the inner wall of the cylinder is 2 to 10 mm.
[0038] To implement the above technical solution, the molten metal can be effectively film-formed on the annular stirring element by connecting the ribs, the outer ring body and the inner ring body, and the appropriate gap between the outer ring body and the inside of the cylinder body can be controlled to help the annular stirring element scrape off the melt adhering to the inner wall of the cylinder during rotation, thereby avoiding coking caused by prolonged heating after the melt adheres to the wall.
[0039] In some exemplary embodiments, a plurality of porous discs are fixed inside the connecting ribs, and the ratio of the number of the porous discs to the number of the annular stirring elements is 1:(1-10).
[0040] To implement the above technical solution, the provision of a porous disc can further assist in parallel film drawing of the melt, further increase the film forming area, and further improve the devolatilization efficiency.
[0041] In summary, compared with the prior art, the present invention has the following beneficial effects:
[0042] The embodiment of the present invention provides a method for preparing high-viscosity bottle polyester by a final polycondensation reactor, wherein the temperature in the cylinder is controlled to be 265° C. to 290° C., the absolute pressure is 0 Pa to 2000 Pa, and the cylinder is in a high vacuum state by a vacuum system at the gas phase outlet. When the pre-polycondensation melt is supplied into the cylinder, the melt is lifted up by the cage frame during the rotation of the cage frame stirrer, and forms a film under the action of gravity during the rising and falling process, and undergoes a polycondensation reaction. Low molecular weight substances and alcohol reaction products are extracted from the gas phase outlet, the molecular chains of the polymer increase, the degree of polymerization increases, and the melt is The contents of ethylene glycol and ethylene glycol produced by polycondensation are both high. The viscosity of the melt increases rapidly under the action of vacuum. Through the differential rotation of different cage bodies, the melt in the front section and the rear section of the cage stirrer can be effectively filmed, and then filmed through the transfer stirrer and the ring stirrer in sequence, so that the characteristic viscosity of the melt finally reaching the discharge port is 0.70dL / g-1.0dL / g, and the preparation of the polyester melt for high-viscosity bottles can be completed. The final polycondensation reactor and the preparation method of the present invention have high film-forming efficiency, can effectively improve the mass transfer devolatilization efficiency, reduce the polycondensation reaction time, and improve the melt quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a schematic structural diagram of the final polycondensation reactor in an embodiment of the present invention.
[0044] Figure 2 Schematic diagram of the cage frame structure in an embodiment of the present invention.
[0045] Figure 3 It is a schematic structural diagram of a transmission in which part of the case is removed in an embodiment of the present invention.
[0046] Figure 4It is a schematic diagram of the structure of the cooperation between the transfer stirrer and the support roller in an embodiment of the present invention, which shows a schematic diagram of the structure of the reaction tank arranged on the reaction disk.
[0047] Figure 5 It is a schematic diagram of the structure of the cooperation between the transfer stirrer and the support roller in an embodiment of the present invention, which shows a schematic diagram of the structure of the reaction holes arranged on the reaction disk.
[0048] Figure 6 It is a schematic diagram of the structure of the installation disk in an embodiment of the present invention.
[0049] Figure 7 Schematic diagram of the structure of the annular stirring element in an embodiment of the present invention.
[0050] Figure 8 Schematic diagram of the structure in which a porous disc is arranged inside the circular spokes in an embodiment of the present invention.
[0051] The numbers and letters in the figure represent the corresponding component names:
[0052] 10. Cylinder; 11. Feed inlet; 12. Discharge outlet; 13. Gas phase outlet; 20. First power system; 21. First main shaft; 30. Second power system; 31. Second main shaft; 40. Cage stirrer; 41. Cage frame; 411. Frame portion; 412. Mounting plate; 413. Transmission shaft; 414. Reinforcement rib; 415. Cage spoke; 42. Transmission; 421. Box; 422. Driving gear; 423. Driven gear; 424. Transmission gear group; 43, first viscosity sensor; 44, second viscosity sensor; 50, transfer agitator; 51, inner fixing ring; 511, step installation section; 52, outer support ring; 53, reaction disk; 531, reaction tank; 532, reaction hole; 54, support roller; 60, annular agitator; 61, flower disk; 62, annular spokes; 63, annular stirring element; 631, connecting ribs; 632, outer ring body; 633, inner ring body; 64, linkage shaft; 65, porous disc. DETAILED DESCRIPTION
[0053] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0054] like Figures 1 to 8As shown, the present invention provides a method for preparing high-viscosity bottle polyester by a final polycondensation reactor, and the method is implemented based on a final polycondensation reactor, wherein the final polycondensation reactor comprises: a cylinder 10, a feed port 11 is provided at the front end of the cylinder 10, a discharge port 12 is provided at the rear end, and a gas phase outlet 13 connected to a vacuum system is provided at the top of the middle and rear end of the cylinder 10; a first power system 20 and a second power system 30 are respectively arranged on the front and rear sides of the cylinder 10, the first power system 20 is connected to a first main shaft 21, and the second power system 30 is connected to a second main shaft 31; a cage agitator 40 connected to the first main shaft 21; a transfer agitator 50 fixed to the end of the cage agitator 40; and a ring agitator 60 connected to the second main shaft 31 and rotatably connected to the transfer agitator 50.
[0055] Specifically, the feed port 11 and the discharge port 12 are both arranged at the bottom of the cylinder 10. An interlayer is usually arranged inside the cylinder 10. A plurality of heat medium inlets and heat medium outlets are also arranged on the cylinder 10. The heat medium such as heat transfer oil is supplied into the interlayer through the heat medium inlet by the heating equipment, and the heat medium is returned to the heating equipment through the heat medium outlet, thereby forming a circulation of the heat medium. The cylinder 10 is heat-conducted and heated by the heat medium, so that the inside of the cylinder 10 forms a high-temperature state.
[0056] The first power system 20 and the second power system 30 are used to provide the power required for stirring. Usually, the first power system 20 and the second power system 30 both include a stirring motor, a transmission box and a differential connected in sequence. Of course, in some embodiments, they can also be replaced by a combined structure of a motor and a reduction box. The first main shaft 21 and the second main shaft 31 are fixed to the differential by a coupling or a key connection, so that power is input into the cylinder 10 through the first main shaft 21 and the second main shaft 31. It can be understood that the first main shaft 21 and the second main shaft 31 both penetrate into the cylinder 10 and are sealed and connected to the cylinder 10.
[0057] The cage agitator 40 includes: at least two cage frames 41 arranged in sequence along the axial direction of the cylinder 10, and a transmission 42 arranged between adjacent cage frames 41 for reducing the rotation speed of each cage frame 41 in sequence according to a predetermined ratio. The front and rear sides of the cage agitator 40 are respectively provided with a first viscosity sensor 43 and a second viscosity sensor 44.
[0058] Among them, Figure 1 and Figure 2As shown, the cage frame 41 includes: a frame portion 411, and mounting plates 412 fixed on both sides of the frame portion 411. The frame portion 411 can adopt an existing cage frame structure. The cross-section of the frame portion 411 can be set to be circular or polygonal. A transmission shaft 413 is provided on the mounting plate 412. The transmission shaft 413 can be integrally formed with the mounting plate 412, or can be fixed to the mounting plate 412 by welding, or can be detachably connected to the mounting plate 412 by bolt connection or key connection. The transmission shaft 413 can be connected to the power input end / power output end of the transmission 42. Whether the transmission shaft 413 is connected to the power output end or the output end of the transmission 42 depends on the position of the transmission shaft 413. The cage frame 41 is connected and fixed to the first main shaft 21 and the transmission 42 through the mounting plate 412, and the frame portion 411 is hollow as a whole, which can effectively avoid high-viscosity melt from sticking to the shaft, prevent the melt from being heated for a long time and coking, and improve the melt quality.
[0059] Furthermore, reinforcing ribs 414 are provided in the frame portion 411. The reinforcing ribs 414 may be a plurality of annular structures spaced apart and vertically arranged in the frame portion 411, or may be a plurality of ribs arranged horizontally and fixed at both ends to the mounting plate 412. The reinforcing ribs 414 may be fixed to the frame portion 411 by welding. A plurality of cage spokes 415 having a trapezoidal cross section are provided around the periphery of the frame portion 411. A plurality of cage bodies 41 are evenly arranged around the periphery of the frame portion 411. For example, if the cross section of the frame portion 411 is a regular polygon, the cage spokes 415 may be welded and fixed at each corner of the regular polygon. Preferably, the highest point of the cage spokes 415 is located on one side of the rotation direction of the cage body 41. The cage spokes 415 may also play a role in strengthening the structural strength of the cage body 41. The minimum gap between the highest point of the cage spokes 415 and the inner wall of the cylinder 10 is 5 to 20 mm.
[0060] The reinforcement ribs 414 can be provided to increase the structural strength of the frame 411, ensuring that the frame 411 does not deform during rotation. The cage spokes 415 can help the cage agitator 40 to scrape off the melt attached to the inner wall of the cylinder 10 during rotation, preventing the melt from coking due to long-term heating after hanging on the wall. The frame 411 can perform parallel film drawing on the melt, and the reinforcement ribs 414 and the cage spokes 415 can perform vertical film formation on the melt, thereby improving the film forming effect and the devolatilization efficiency.
[0061] like Figure 1 and Figure 3As shown, the transmission 42 includes: a housing 421, a driving gear 422 and a driven gear 423 that are rotatably connected to the housing 421 and coaxially arranged, and a transmission gear set 424 that is arranged between the driving gear 422 and the driven gear 423 for speed conversion. The driving gear 422, the driven gear 423 and the transmission gear set 424 have different transmission ratios. The transmission gear set 424 is mainly used to transmit the power of the driving gear 422 to the driven gear 423; preferably, the transmission gear set 424 includes a first gear meshed with the driving gear 422 and a second gear meshed with the driven gear 423, and the first gear meshed with the driven gear 423. The wheel and the second gear are coaxially arranged and fixed to each other. The driving gear 422 and the driven gear 423 are respectively connected to the transmission shaft 413 of the adjacent cage frame 41. Usually, the driving gear 422 and the driven gear 423 are fixed with a connecting shaft extending from the box body 421 and forming a mechanical seal. The connecting shaft and the transmission shaft 413 can be fixed by connecting parts such as sleeves. In actual applications, the lengths of the transmission shaft 413 and the connecting shaft and the overall thickness of the transmission 42 need to be set as small as possible so that the cage agitator 40 has sufficient film-forming area. The transmission 42 is fixed to the cylinder 10 through supporting feet fixed to the outer wall of the box body 421.
[0062] The power transmission between adjacent cage frames 41 is realized by the driving gear 422, the driven gear 423 and the transmission gear set 424. By setting a reasonable transmission ratio among the driving gear 422, the transmission gear set 424 and the driven gear 423, the rotation speed of each cage frame 41 can be reduced in sequence. In this embodiment, three groups of cage frames 41 are arranged, and the rotation speed ratios of the three groups of cage frames 41 are 1: (0.75-0.9): (0.5-0.7) in sequence.
[0063] The first viscosity sensor 43 and the second viscosity sensor 44 can both be existing sensors. The first viscosity sensor 43 and the second viscosity sensor 44 are both fixed to the cylinder 10 and their test heads extend into the cylinder 10. The first viscosity sensor 43 and the second viscosity sensor 44 are respectively located at the front and rear sides of the cage agitator 40 and do not interfere with the cage agitator 40. The first viscosity sensor 43 and the second viscosity sensor 44 are both connected to an external controller and send the collected viscosity values to the external control. The external controller can adopt an existing controller structure such as a PLC controller, and the external controller is connected to the first power system 20 and the second power system 30 to control the output speed of the first power system 20 and the second power system 30.
[0064] like Figure 1 , Figure 4 and Figure 5As shown, the transfer agitator 50 includes: an inner fixed ring 51, an outer support ring 52, and a plurality of reaction disks 53 fixed between the inner fixed ring 51 and the outer support ring 52. The inner wall of the cylinder 10 is rotatably connected with a plurality of support rollers 54 that abut against and support the outer support ring 52. The plurality of reaction disks 53 are evenly spaced along the axial direction of the inner fixed ring 51. The inner side of the reaction disk 53 is fixed to the inner fixed ring 51, and the outer side is fixed to the outer support ring 52. The reaction disk 53 is provided with a plurality of reaction grooves 531 and / or reaction holes 532. The support rollers 54 are arranged near the middle of the cylinder 10, and at least two groups are symmetrically arranged. In some embodiments, the reaction disk 53 can also be tilted on the inner fixed ring 51 to facilitate a certain feeding effect on the melt. By arranging reaction grooves 531 and / or reaction holes 532 on the reaction disk 53 to facilitate the passage of the melt and film formation, the height of the melt in the cylinder 10 usually does not exceed half the height of the cylinder 10. Therefore, arranging the support plate close to the middle of the cylinder 10 can avoid immersing the support roller 54 in the melt and affecting its rotation.
[0065] In some exemplary embodiments, a stepped mounting section 511 is provided at one end of the inner fixed ring 51 close to the annular agitator 60, and the stepped mounting section 511 is used for rotationally connecting with the annular agitator 60. Usually, a bearing is embedded in the stepped mounting section 511 to facilitate rotational connection with the annular agitator 60. At the same time, in some embodiments, a plurality of through grooves may be provided on the outer support ring 52 between adjacent reaction disks 53 to facilitate film formation of the melt and reduce adhesion of the melt to the surface of the outer support ring 52.
[0066] In the combined polymerization reactor of the prior art, the cage agitator 40 and the disc agitator are usually arranged separately, and a supporting structure such as a support frame is arranged in the middle of the cylinder 10 to support the main shafts of the cage agitator 40 and the disc agitator. Since the supporting structure needs to occupy a certain space, the distance between the cage agitator 40 and the disc agitator is large, which will reduce the space utilization rate in the cylinder 10. The embodiment of the present application replaces the supporting structure with a transfer agitator 50. While supporting the rotating free ends of the cage agitator 40 and the ring agitator 60, the melt can be further stirred to form a film, thereby improving the space utilization rate in the cylinder 10 and further improving the stripping efficiency.
[0067] like Figure 1As shown, the annular agitator 60 includes: two oppositely arranged face plates 61, a plurality of annular spokes 62 arranged between the two face plates 61, and a plurality of annular agitators 63 fixed to the annular spokes 62 and arranged along the axial direction of the cylinder 10, wherein one face plate 61 is fixed to the second main shaft 31, and the other face plate 61 is fixed with a linkage shaft 64 rotatably connected to the step mounting section 511, and the linkage shaft 64 is rotatably connected to the step mounting section 511 by an interference fit with the inner ring of the bearing. The flower disk 61 is used to realize the installation connection with the second main shaft 31 and the transfer stirrer 50, and the connection and fixation of each ring stirrer 60 are realized by the ring spokes 62. The melt is pulled into a film in parallel by the ring stirring member 63 and the melt is pulled into a film vertically by the ring spokes 62, thereby improving the film forming effect and the devolatilization efficiency. The ring stirrer 60 is hollow as a whole, which can effectively avoid the high viscosity melt from sticking to the shaft, prevent the melt from being heated for a long time and produce coking, and improve the quality of the melt. In this embodiment, the circular shape formed by the ring spokes 62 as a whole occupies 0.25~0.5 of the diameter of the cylinder 10.
[0068] Specifically, Figure 6 and Figure 7 As shown, the faceplate 61 can be a disc structure, or it can be a circular base plate with a plurality of radial protrusions, the annular spokes 62 are welded and fixed to the ends of the protrusions, and the annular stirring member 63 includes: a plurality of connecting ribs 631 fixed to each annular spoke 62, an outer ring body 632 fixed to the ends of the connecting ribs 631, and a plurality of inner ring bodies 633 fixed to the connecting ribs 631, the minimum gap between the outer ring body 632 and the inner wall of the cylinder 10 is 2 to 10 mm, and the diameter of the annular stirring member 63 accounts for The diameter of the annular stirring piece 63 is 0.05-0.5 of the diameter of the cylinder 10, where the diameter of the annular stirring piece 63 can specifically be the length of the connecting rib 631; the connecting rib 631, the outer ring body 632 and the inner ring body 633 cooperate with each other, so that the melt can effectively form a film on the annular stirring piece 63, and by controlling the appropriate gap between the outer ring body 632 and the inside of the cylinder 10, it is helpful for the annular stirring piece 63 to scrape off the melt attached to the inner wall of the cylinder 10 during rotation, so as to avoid coking caused by long-term heating after the melt adheres to the wall.
[0069] Furthermore, in some embodiments, Figure 8 As shown, a plurality of porous discs 65 are fixed inside the connecting rib 631, the middle of the porous disc 65 is hollow, the number ratio of the porous disc 65 to the annular stirring member 63 is 1:(1-10), and the area of the porous disc 65 accounts for 0.05-0.25 of the cross-sectional area of the cylinder 10, and the porous disc 65 can be arranged corresponding to the annular stirring member 63, and can also be arranged offset from the annular stirring member 63; by arranging the porous disc 65, it is possible to further assist in parallel film drawing of the melt, further increase the film forming area, and further improve the devolatilization efficiency.
[0070] In this embodiment, the ratio of the total length of the cage agitator 40 to the total length of the ring agitator 60 is 1: (0.2~5), and the ratio of the total length of the ring agitator 60 to the total length of the transfer agitator 50 is 1: (0.1~0.3). The main function of the transfer agitator 50 is to replace the existing supporting structure to support the cage agitator 40 and the ring agitator 60, and at the same time add a stirring method to improve the film forming area and the devolatilization efficiency. Therefore, the overall length of the transfer agitator 50 should not be too long, and is usually equivalent to the overall length of the existing supporting structure.
[0071] In some embodiments, a bubble level gauge is provided at the front and middle sections of the cylinder 10 to detect the liquid level, and a radioactive source level gauge is provided at the discharge port 12 of the rear section of the cylinder 10 to detect the liquid level. At the same time, a scraper is provided at the rear end of the cylinder 10, and the scraper is fitted with the linkage shaft 64 to scrape off excess melt adhering to the linkage shaft 64.
[0072] The method for preparing high-viscosity bottle polyester in the final polycondensation reactor specifically includes: continuously feeding a bottle polyester melt material having an IPA content of 0.25% to 3.0% and an intrinsic viscosity of 0.15 dL / g to 0.40 dL / g into the final polycondensation reactor, adjusting the output speed of the first power system 20 according to the viscosity value detected by the first viscosity sensor 43 and / or the second viscosity sensor 44, reacting for 50 minutes to 150 minutes under the conditions of a temperature of 265°C to 290°C and an absolute pressure of 0Pa to 2000Pa, and preparing a high-viscosity bottle polyester melt with an intrinsic viscosity of 0.70 dL / g to 1.0 dL / g.
[0073] Wherein, adjusting the output speed of the first power system 20 according to the viscosity value detected by the first viscosity sensor 43 and / or the second viscosity sensor 44 specifically includes:
[0074] If the viscosity value measured by the first viscosity sensor 43 is 0.15 dL / g to 0.25 dL / g, the output speed of the first power system 20 is controlled to be 6 rpm to 10 rpm;
[0075] If the viscosity value measured by the first viscosity sensor 43 is 0.25 dL / g to 0.35 dL / g, the output speed of the first power system 20 is controlled to be 4.5 rpm to 6 rpm;
[0076] If the viscosity value measured by the first viscosity sensor 43 is 0.35 dL / g to 0.40 dL / g, the output speed of the first power system 20 is controlled to be 3 rpm to 4.5 rpm; or,
[0077] If the viscosity value measured by the second viscosity sensor 44 is 0.55 dL / g to 0.70 dL / g, the output speed of the first power system 20 is controlled to be 5 rpm to 6.5 rpm.
[0078] When the viscosity value increases, if the rotation speed is too fast, it will be difficult to form a film in time or the thickness of the liquid film will be too large. Therefore, when the melt viscosity increases, the rotation speed needs to be appropriately reduced. According to the above strategy, the output speed of the first power system 20 is adjusted according to the viscosity value detected by the first viscosity sensor 43 and / or the second viscosity sensor 44, so that reasonable speed control can be performed corresponding to different viscosity gradients.
[0079] In actual application, the strategy of adjusting the rotational speed of the first power system 20 according to the viscosity value measured by the first viscosity sensor 43 is used as the first strategy, and the strategy of adjusting the rotational speed of the first power system 20 according to the viscosity value measured by the second viscosity sensor 44 is used as the second strategy. The first strategy is implemented in the initial stage of the operation of the reactor. After the reaction has been running for a sufficient time, the viscosity value at the end of the cage reactor increases. Since the ultimate goal of the polycondensation reaction is to obtain a high-viscosity melt, when the viscosity of the melt is high enough, the second strategy is implemented at this time, so that the cage reactor stirs the high-viscosity melt at an appropriate rotational speed. Of course, when the viscosity value measured by the second viscosity sensor 44 is greater than 0.70dL / g, the second strategy can also be implemented.
[0080] Since the melt in the annular agitator 60 is in a high viscosity state, the second power system 30 is usually controlled to rotate at a predetermined low speed. In this embodiment, the output speed of the second power system 30 is controlled at 0.5 rpm to 4 rpm.
[0081] During the polycondensation reaction, the pre-polycondensation melt is fed into the barrel 10 from the feed port 11, and the cage stirrer 40 is driven to rotate by the first power system 20 through the first main shaft 21. The cage stirrer 40 synchronously drives the transfer stirrer 50 to rotate during the rotation process, and the second power system 30 drives the ring stirrer 60 to rotate through the second main shaft 31. Since the ring stirrer 60 is rotatably connected to the transfer stirrer 50, the two can rotate at different speeds respectively, thereby meeting the differential stirring requirements of the front and rear melts in different viscosity states;
[0082] In the initial state, the first power system 20 is controlled to rotate at a predetermined speed to provide power according to the pre-detected viscosity value of the pre-condensation melt. During the rotation of the cage stirrer 40, the melt viscosity at the front and rear sides of the cage stirrer 40 is detected by the first viscosity sensor 43 and the second viscosity sensor 44, respectively, and the output speed of the first power system 20 is adjusted according to the real-time measured viscosity value, so that the cage stirrer 40 can be adjusted to rotate at a more reasonable speed according to the viscosity state of the melt, so that the melt can be efficiently devolatilized by film formation. The melt located in the annular stirrer 60 is in a high viscosity state, and the second power system 30 is usually controlled to rotate at a predetermined low speed.
[0083] Meanwhile, the cage stirrer 40 is composed of a plurality of cage frames 41, and the adjacent cage frames 41 are connected by a transmission 42 in a differential rotation with decreasing rotation speeds in sequence, so that the film-forming states of the front section and the rear section of the cage stirrer 40 are similar, and the mass transfer and devolatilization efficiencies of the front section and the rear section are kept similar, which is beneficial to improving the overall mass transfer and devolatilization efficiency; and the transfer stirrer 50 arranged between the cage stirrer 40 and the annular stirrer 60, on the one hand, can replace the supporting structure in the existing technology to provide support for the rotating free ends of the cage stirrer 40 and the annular stirrer 60, and on the other hand, can also stir the melt to form a film through the reaction disk 53, and can further improve the utilization rate of the internal space of the cylinder 10, so as to further improve the devolatilization efficiency;
[0084] The temperature in the cylinder 10 is controlled to be 265°C to 290°C and the absolute pressure is 0Pa to 2000Pa. The cylinder 10 is in a high vacuum state by evacuating the gas phase outlet 13 by a vacuum system. When the pre-condensation melt is supplied into the cylinder 10, the melt is lifted up by the cage frame 41 during the rotation of the cage frame stirrer 40. During the rising and falling process, the melt is formed into a film by the action of gravity and undergoes a polycondensation reaction. Low molecular weight substances and alcohol reaction products are extracted from the gas phase outlet 13, the molecular chains of the polymer increase, the degree of polymerization increases, and the ethylene glycol in the melt and the ethylene glycol content produced by the polycondensation are reduced. The melt viscosity increases rapidly under the action of vacuum, and the melt in the front and rear sections of the cage frame agitator 40 can be effectively filmed after differential rotation of different cage frames 41, and then filmed after the transfer agitator 50 and the annular agitator 60 in turn, so that the characteristic viscosity of the melt finally reaching the discharge port 12 is 0.70dL / g to 1.0dL / g, and the preparation of high-viscosity polyester melt for bottles can be completed; the final polycondensation reactor and preparation method of the present invention have high film-forming efficiency, can effectively improve the mass transfer and devolatilization efficiency, reduce the polycondensation reaction time, and improve the melt quality. Example 1
[0085] A method for preparing high-viscosity bottle polyester in a final polycondensation reactor. In this embodiment, PET bottle-grade polyester is prepared from terephthalic acid, isophthalic acid, ethylene glycol, and phosphoric acid as raw materials, wherein isophthalic acid accounts for 0.25% of the total weight of the synthetic polyester, terephthalic acid accounts for 70.65% of the total weight of the synthetic polyester, ethylene glycol accounts for 29% of the total weight of the synthetic polyester, and phosphoric acid accounts for (10-50) ppm of the total weight of the polyester. After beating, esterification, and pre-polycondensation, terephthalic acid, isophthalic acid, ethylene glycol, and phosphoric acid form a pre-polycondensation melt, and the intrinsic viscosity of the pre-polycondensation melt is controlled at 0.15 dL / g.
[0086] The pre-condensation melt is fed into the barrel 10 from the feed port 11, and the reaction temperature is controlled to be 265°C and the absolute pressure is 10Pa. The reaction is carried out for 90 minutes. In this embodiment, the length ratio of the cage stirrer to the length of the annular stirrer 60 is 1:0.2, and the length ratio of the annular stirrer 60 to the length of the transfer stirrer 50 is 1:0.3. The low-viscosity pre-condensation melt is firstly efficiently film-formed under the action of the cage stirrer 40. At this time, the content of ethylene glycol in the melt and the ethylene glycol produced by polycondensation are both high. The viscosity of the melt increases rapidly under the action of vacuum. In order to avoid the melt hanging on the wall of the reactor, the pre-condensation melt is heated for a long time. Heat will produce coking, and the cage spokes 415 are designed to be trapezoidal, with the minimum gap between the top and the reactor wall controlled at 5mm. The trapezoidal structure of the cage spokes 415 helps the cage agitator 40 to scrape off the melt attached to the inner wall of the cylinder 10 during rotation; since the viscosity of the polyester melt located in the cage agitator 40 is relatively low, the liquid film forming effect is unstable, and the stirring speed of the cage agitator 40 is increased to compensate for the poor film forming effect of the liquid film. In this embodiment, the output speed of the first power system 20 is controlled to 6rpm, and the speed ratios of the three groups of cage frames 41 are 1:0.8:0.6 respectively.
[0087] After the polyester melt passes through the cage frame agitator 40 for efficient film forming and devolatilization, the intrinsic viscosity can increase to about 0.6dL / g. As the dynamic viscosity of the melt increases, if the cage frame agitator 40 located in the rear section is still rotated at a relatively high speed, the film forming effect of the melt in the rear section of the cage frame agitator 40 will be weakened, the liquid film thickness will increase, the small molecules such as ethylene glycol generated by polycondensation cannot be effectively volatilized, the driving force of the polycondensation reaction decreases, and the increase rate of the polyester melt viscosity slows down. In the embodiment of the present invention, the cage frame 41 is decelerated in stages by the transmission 42 for differential rotation, so that the melt located in the rear section of the cage frame agitator 40 can also form a film more effectively, thereby improving the film forming effect and the devolatilization efficiency.
[0088] Subsequently, the polyester melt begins to enter the transfer stirrer 50 and the annular stirrer 60 for disc and annular film devolatilization. The multiple groups of annular stirring members 63 arranged on the annular stirrer 60 are hollow annular structures. The minimum gap between the annular stirring members 63 and the inner wall of the cylinder 10 is controlled at 2 mm. The diameter of the annular spokes 62 accounts for 0.25 of the diameter of the cylinder 10. A porous disc 65 is arranged inside the annular spokes 62. The number ratio of the porous disc 65 to the annular stirring member 63 is 1:1. The surface of the porous disc 65 is The area of the outer ring body 632 accounts for 0.05 of the cross-sectional area of the cylinder 10, and the diameter of the outer ring body 632 accounts for 0.05 of the diameter of the cylinder 10. When the high-viscosity melt passes between the inner ring body 633, the outer ring body 632 and the connecting ribs 631, due to the high viscosity of the melt, the melt will have a slower flow speed on the annular stirring member 63, and can form an effective film on the inner ring body 633, the outer ring body 632 and between the two, and the film forming area is large and the time is long, thereby effectively increasing the devolatilization area and achieving a viscosity-increasing effect. The presence of the porous disk 65, on the one hand, enhances the support of the annular stirrer 60, and on the other hand, performs disk surface film formation on the high-viscosity melt, and the high-viscosity melt is further filmed and devolatilized at the disk surface and circular holes to increase the viscosity.
[0089] In addition, in addition to the parallel film formation of the melt by the annular stirring element 63 and the porous disc 65, the annular spokes 62 will also vertically film the high-viscosity melt as the annular stirrer 60 rotates. On the one hand, it disturbs the high-viscosity melt to make it evenly mixed, and on the other hand, it vertically pulls the film to assist the high-viscosity melt in devolatilization. The transfer stirrer 50 arranged between the cage stirrer 40 and the annular stirrer 60 can not only provide rotation support for both, but also further perform parallel film formation through the reaction disc 53, which can further improve the devolatilization efficiency. The hollow design of the cage stirrer 40 and the annular stirrer 60 can effectively reduce the high-viscosity melt from hanging on the disc and sticking to the shaft, and a set of scrapers, such as an annular scraper, is added at the rear end of the disc section, which can easily scrape the high-viscosity melt from the wall of the cylinder 10 and transport it to the discharge port 12. Since the melt viscosity at the annular agitator 60 is relatively high, a too high rotation speed will result in the liquid film not forming, which is not conducive to the removal of small molecules. In addition, a high rotation speed will have an adverse effect on the radius and shape of the annular agitator 60, especially on the basis of precise fit with the inner wall of the cylinder 10, which is easy to scratch. At this time, the output speed of the second power system 30 is usually controlled at 2rpm.
[0090] By using the final polycondensation reactor and preparation method, the low-viscosity bottle polyester melt can be liquid-phase viscosity-increased to 0.7 dL / g, the polyester melt has a terminal carboxyl group of 40 mol / t, a melting point of 255°C, an L value of 84, and a b value of -3. Example 2
[0091] The difference between this embodiment and embodiment 1 is that isophthalic acid accounts for 1.8% of the total weight of the synthetic polyester, and other process parameters and reactor design parameters are consistent. By using the final polycondensation reactor and preparation method, the low-viscosity bottle polyester melt is liquid-phase thickened to 0.7 dL / g, the polyester melt has a terminal carboxyl group of 40 mol / t, a melting point of 244°C, an L value of 84, and a b value of -3. Example 3
[0092] The difference between this embodiment and embodiment 1 is that isophthalic acid accounts for 3.0% of the total weight of the synthetic polyester, and other process parameters and reactor design parameters are consistent. The final polycondensation reactor and preparation method are used to increase the viscosity of the low-viscosity bottle polyester melt to 0.7 dL / g in liquid phase, the polyester melt has a terminal carboxyl group of 40 mol / t, a melting point of 240°C, an L value of 85.8, and a b value of -3. Example 4
[0093] In this embodiment, PET bottle-grade polyester is prepared from terephthalic acid, isophthalic acid, ethylene glycol, and phosphoric acid as raw materials, wherein isophthalic acid accounts for 1.8% of the total weight of the synthetic polyester, terephthalic acid accounts for 69.2% of the total weight of the synthetic polyester, ethylene glycol accounts for 29% of the total weight of the synthetic polyester, and phosphoric acid accounts for (10-50) ppm of the total weight of the polyester. After beating, esterification, and pre-condensation, terephthalic acid, isophthalic acid, ethylene glycol, and phosphoric acid form a pre-condensation melt, and the intrinsic viscosity of the pre-condensation melt is controlled at 0.20 dL / g.
[0094] The pre-condensation melt is fed into the barrel 10 from the feed port 11, and the reaction is carried out for 120 minutes under the conditions of the reaction temperature being 275°C and the absolute pressure being 100 Pa. In this embodiment, the ratio of the length of the cage frame agitator to the length of the ring agitator 60 is 1:0.5, the ratio of the length of the ring agitator 60 to the length of the transfer agitator 50 is 1:0.2, the minimum gap between the top of the cage frame spoke 415 and the inside of the cylinder 10 is controlled at 10 mm, the minimum gap between the ring agitator 63 and the inner wall of the cylinder 10 is controlled at 5 mm, the diameter of the ring spoke 62 accounts for 0.3 of the diameter of the cylinder 10, and a porous disc 65 is provided inside the ring spoke 62, the number ratio of the porous disc 65 to the ring agitator 63 is 1:3, the area of the porous disc 65 accounts for 0.1 of the cross-sectional area of the cylinder 10, the diameter of the outer ring body 632 accounts for 0.1 of the diameter of the cylinder 10, the output speed of the first power system 20 is 4 rpm, the speed ratios of the three groups of cage frame bodies 41 are 1:0.9:0.7 respectively, and the output speed of the second power system 30 is 0.5 rpm.
[0095] By using the final polycondensation reactor and preparation method, the low-viscosity bottle polyester melt liquid phase viscosity is increased to 0.78 dL / g, the polyester melt terminal carboxyl group is 35 mol / t, the melting point is 244°C, the L value is 85.1, and the b value is -2.8. Example 5
[0096] The difference between this embodiment and embodiment 4 is that the intrinsic viscosity of the pre-condensation melt is controlled at 0.30 dL / g. The pre-condensation melt is fed into the barrel 10 from the feed port 11, and the reaction is controlled at a reaction temperature of 280°C and an absolute pressure of 250 Pa for 135 minutes. In this embodiment, the ratio of the length of the cage frame agitator to the length of the ring agitator 60 is 1:2.5, the ratio of the length of the ring agitator 60 to the length of the transfer agitator 50 is 1:0.15, the minimum gap between the top of the cage frame spoke 415 and the inside of the cylinder 10 is controlled at 15 mm, the minimum gap between the ring agitator 63 and the inner wall of the cylinder 10 is controlled at 8 mm, the diameter of the ring spoke 62 accounts for 0.4 of the diameter of the cylinder 10, and a porous disc 65 is provided inside the ring spoke 62, the number ratio of the porous disc 65 to the ring agitator 63 is 1:5, the area of the porous disc 65 accounts for 0.2 of the cross-sectional area of the cylinder 10, the diameter of the outer ring body 632 accounts for 0.25 of the diameter of the cylinder 10, the output speed of the first power system 20 is 6 rpm, the speed ratios of the three groups of cage frame bodies 41 are 1:0.8:0.65 respectively, and the output speed of the second power system 30 is 1.5 rpm.
[0097] By using the final polycondensation reactor and preparation method, the low-viscosity bottle polyester melt liquid phase viscosity is increased to 0.84dL / g, the polyester melt terminal carboxyl group is 32mol / t, the melting point is 244°C, the L value is 84.2, and the b value is -2.5. Example 6
[0098] The difference between this embodiment and embodiment 4 is that the intrinsic viscosity of the pre-condensation melt is controlled at 0.35 dL / g. The pre-condensation melt is fed into the barrel 10 from the feed port 11, and the reaction temperature is controlled to be 285°C and the absolute pressure is 500 Pa for 150 minutes. In this embodiment, the ratio of the length of the cage frame agitator to the length of the ring agitator 60 is 1:4, the ratio of the length of the ring agitator 60 to the length of the transfer agitator 50 is 1:0.1, the minimum gap between the top of the cage frame spoke 415 and the inside of the cylinder 10 is controlled at 18 mm, the minimum gap between the ring agitator 63 and the inner wall of the cylinder 10 is controlled at 9 mm, the diameter of the ring spoke 62 accounts for 0.45 of the diameter of the cylinder 10, and a porous disc 65 is provided inside the ring spoke 62, the number ratio of the porous disc 65 to the ring agitator 63 is 1:8, the area of the porous disc 65 accounts for 0.25 of the cross-sectional area of the cylinder 10, the diameter of the outer ring body 632 accounts for 0.4 of the diameter of the cylinder 10, the output speed of the first power system 20 is 8 rpm, the speed ratios of the three groups of cage frame bodies 41 are 1:0.75:0.6 respectively, and the output speed of the second power system 30 is 2.5 rpm.
[0099] By using the final polycondensation reactor and preparation method, the low-viscosity bottle polyester melt liquid phase viscosity is increased to 0.91dL / g, the polyester melt terminal carboxyl group is 30mol / t, the melting point is 244°C, the L value is 84.0, and the b value is -2.2. Example 7
[0100] The difference between this embodiment and embodiment 4 is that the intrinsic viscosity of the pre-condensation melt is controlled at 0.40 dL / g. The pre-condensation melt is fed into the cylinder 10 from the feed port 11, and the reaction temperature is controlled to be 290°C and the absolute pressure is 2000 Pa for 150 minutes. In this embodiment, the ratio of the length of the cage frame agitator to the length of the ring agitator 60 is 1:5, the ratio of the length of the ring agitator 60 to the length of the transfer agitator 50 is 1:0.1, the minimum gap between the top of the cage frame spoke 415 and the inside of the cylinder 10 is controlled at 20 mm, the minimum gap between the ring agitator 63 and the inner wall of the cylinder 10 is controlled at 10 mm, the diameter of the ring spoke 62 accounts for 0.5 of the diameter of the cylinder 10, and a porous disc 65 is provided inside the ring spoke 62, the number ratio of the porous disc 65 to the ring agitator 63 is 1:10, the area of the porous disc 65 accounts for 0.25 of the cross-sectional area of the cylinder 10, the diameter of the outer ring body 632 accounts for 0.5 of the diameter of the cylinder 10, the output speed of the first power system 20 is 10 rpm, the speed ratios of the three groups of cage frame bodies 41 are 1:0.75:0.5 respectively, and the output speed of the second power system 30 is 4 rpm.
[0101] By using the final polycondensation reactor and preparation method, the low-viscosity bottle polyester melt liquid phase viscosity is increased to 1.0 dL / g, the polyester melt terminal carboxyl group is 5 mol / t, the melting point is 244°C, the L value is 82.0, and the b value is -1.8.
[0102] Comparative Example 1
[0103] PET bottle-grade polyester is made from terephthalic acid, isophthalic acid, ethylene glycol and phosphoric acid, wherein isophthalic acid accounts for 1.8% of the total weight of the synthetic polyester, terephthalic acid accounts for 69.2% of the total weight of the synthetic polyester, ethylene glycol accounts for 29% of the total weight of the synthetic polyester, and phosphoric acid accounts for (10-50) ppm of the total weight of the polyester. After beating, esterification and pre-condensation, terephthalic acid, isophthalic acid, ethylene glycol and phosphoric acid form a pre-condensation melt, and the intrinsic viscosity of the pre-condensation melt is controlled at 0.25 dL / g.
[0104] The precondensation melt enters a conventional disc reactor and reacts for 100 minutes under the conditions of a reaction temperature of 285°C and an absolute pressure of 100 Pa. The obtained bottle polyester melt has a viscosity of 0.65 dL / g, a terminal carboxyl group of 24 mol / t, a melting point of 244°C, an L value of 86.0, and a b value of -3.2.
[0105] In order to more clearly show the comparison of various embodiments, the influence of the structural parameters of the reactor on the performance of bottle polyester is shown in the following table:
[0106]
[0107] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which are equivalent modifications and improvements made to the above embodiments based on the essential technology of the present invention, and all of them belong to the protection scope of the present invention.
Claims
1. A method for preparing high-viscosity bottle polyester using a final polycondensation reactor, It is characterized in that The method is implemented based on a final polycondensation reactor, which comprises: A cylinder, wherein the front end of the cylinder is provided with a feed inlet, the rear end is provided with a discharge outlet, and the middle part and the top of the rear end of the cylinder are both provided with gas phase outlets connected to the vacuum system; A first power system and a second power system are respectively arranged at the front and rear sides of the cylinder, the first power system is connected to a first main shaft, and the second power system is connected to a second main shaft; A cage stirrer connected to the first main shaft, the cage stirrer comprising: at least two cage frames arranged in sequence along the axial direction of the cylinder, and a transmission arranged between adjacent cage frames for reducing the rotation speed of each cage frame in sequence according to a predetermined ratio, and a first viscosity sensor and a second viscosity sensor are respectively arranged on the front side and the rear side of the cage stirrer; A transfer stirrer fixed at the end of the cage stirrer, the transfer stirrer comprising: an inner fixed ring, an outer support ring, and a plurality of reaction disks fixed between the inner fixed ring and the outer support ring, the inner wall of the cylinder being rotatably connected to a plurality of support rollers that abut and support the outer support ring; and a circular agitator connected to the second main shaft and rotatably connected to the intermediate agitator; The cage frame includes: a frame portion, and mounting plates fixed to both sides of the frame portion, wherein a transmission shaft is provided on the mounting plate, and the transmission shaft can be connected to a power input end / power output end of the transmission; The frame body is provided with reinforcing ribs, and the outer periphery of the frame body is provided with a plurality of cage spokes with trapezoidal cross sections, and the minimum gap between the highest point of the cage spokes and the inner wall of the cylinder is 5 to 20 mm; The transmission comprises: a housing, a driving gear and a driven gear rotatably connected to the housing and coaxially arranged, and a transmission gear set arranged between the driving gear and the driven gear for speed conversion, the driving gear and the driven gear are respectively connected to the transmission shaft of the adjacent cage frame, and the transmission is fixed to the cylinder through supporting feet; The cage frames are provided in three groups, and the speed ratios of the three groups of cage frames are 1: (0.75-0.9): (0.5-0.7) respectively. Adjusting the output speed of the first power system according to the viscosity value detected by the first viscosity sensor and / or the second viscosity sensor specifically includes: If the viscosity value measured by the first viscosity sensor is 0.15 dL / g to 0.25 dL / g, the output speed of the first power system is controlled to be 6 rpm to 10 rpm; If the viscosity value measured by the first viscosity sensor is 0.25 dL / g to 0.35 dL / g, the output speed of the first power system is controlled to be 4.5 rpm to 6 rpm; If the viscosity value measured by the first viscosity sensor is 0.35 dL / g to 0.40 dL / g, the output speed of the first power system is controlled to be 3 rpm to 4.5 rpm; or, If the viscosity value measured by the second viscosity sensor is 0.55 dL / g to 0.70 dL / g, the output speed of the first power system is controlled to be 5 rpm to 6.5 rpm; The method comprises: continuously feeding a polyester melt material for bottles having an isophthalic acid content of 0.25% to 3.0% and an intrinsic viscosity of 0.15 dL / g to 0.40 dL / g into the final polycondensation reactor, adjusting the output speed of the first power system according to the viscosity value detected by the first viscosity sensor and / or the second viscosity sensor, reacting for 50 minutes to 150 minutes under the conditions of a temperature of 265° C. to 290° C. and an absolute pressure of 0 Pa to 2000 Pa, and preparing a high-viscosity polyester melt for bottles having an intrinsic viscosity of 0.70 dL / g to 1.0 dL / g.
2. The method for preparing high-viscosity bottle polyester by using a final polycondensation reactor according to claim 1, It is characterized in that The inner side of the reaction disk is fixed to the inner fixed ring, and the outer side is fixed to the outer support ring. The reaction disk is provided with a plurality of reaction grooves and / or reaction holes. The support rollers are arranged near the middle of the cylinder, and at least two groups are symmetrically arranged.
3. The method for preparing high-viscosity bottle polyester by using a final polycondensation reactor according to claim 2, It is characterized in that A stepped mounting section is provided at one end of the inner fixed ring close to the annular agitator, and the stepped mounting section is used for being rotatably connected to the annular agitator.
4. The method for preparing high-viscosity bottle polyester by using a final polycondensation reactor according to claim 3, It is characterized in that The annular agitator comprises: two faceplates arranged opposite to each other, a plurality of annular spokes arranged between the two faceplates, and a plurality of annular agitators fixed to the annular spokes and arranged along the axis direction of the cylinder body, wherein one of the faceplates is fixed to the second main shaft, and the other faceplate is fixed with a linkage shaft rotatably connected to the stepped mounting section.
5. The method for preparing high-viscosity bottle polyester by using a final polycondensation reactor according to claim 4, It is characterized in that The annular stirring element comprises: a plurality of connecting ribs fixed to the annular spokes, an outer ring body fixed to the ends of the connecting ribs, and a plurality of inner ring bodies fixed to the connecting ribs. The minimum gap between the outer ring body and the inner wall of the cylinder is 2 to 10 mm.
6. The method for preparing high-viscosity bottle polyester by using a final polycondensation reactor according to claim 5, It is characterized in that A plurality of porous discs are also fixed inside the connecting ribs, and the ratio of the number of the porous discs to the number of the annular stirring elements is 1:(1-10).