A ZIF-based high-entropy alloy catalyst, its preparation method and application
By preparing ZIF-based high-entropy alloy catalysts, the problems of expensive noble metal catalysts and poor performance of non-noble metal catalysts were solved, and a highly efficient catalytic effect was achieved for the complete conversion of furfural to furfuryl alcohol at low temperatures.
Patent Information
- Application Number
- CN202410548021.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-30
AI Technical Summary
Existing processes for the hydrogenation of furfural to sugar alcohols often employ expensive precious metal catalysts or non-precious metal catalysts that fail to achieve the desired catalytic effect. Catalyst preparation is often accompanied by complex modification processes.
The preparation method of ZIF-based high-entropy alloy catalyst involves calcining a mixture of metal salt solution and benzimidazole solution to form a carbon support that encapsulates the high-entropy alloy structure, promoting metal dispersion, reducing particle size, and utilizing reducing gas to form a stable catalyst.
Achieving complete conversion and high selectivity of furfural at lower temperatures, with a conversion rate of up to 100% and a selectivity of 95.4% for furfural to furfuryl alcohol, avoids the use of precious metals and complex modification processes.
Smart Images

Figure CN118437336B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of biotransformation technology. More specifically, it relates to a ZIF-based high-entropy alloy catalyst, its preparation method, and its application. Background Technology
[0002] Furfural is a bio-based molecule. As a reactive molecule, its aldehyde group is attached to a furan ring and it is produced by the dehydration of xylan's repeating unit, xylan acid. Furfural can be further upgraded to furfuryl alcohol, 2-methylfuran, 2-methyltetrahydrofuran, tetrahydrofuran, furan, 1,5-pentanediol, 1-pentanol, and butanol. Catalytic processes include ring hydrogenation and ring-opening hydrogenation, hydrogenolysis, decarbonization, and hydrodeoxygenation. Approximately 62% of global furfural production is used for hydrogenation to furfuryl alcohol. Furfural alcohol is an intermediate in the production of lysine, ascorbic acid, and lubricants. Simultaneously, furfuryl alcohol is widely used in the foundry industry due to its flexibility as a binder base and in pharmaceutical synthesis.
[0003] To establish favorable catalytic sites and promote high catalyst dispersion in the support, thermal reduction catalysts derived from metal-organic frameworks (MOFs) are widely used in catalytic transfer hydrogenation (CTH) processes. These catalysts consist of organic linkages and metal ions or clusters. These organic links and ordered arrangement of metal ions and clusters result in a large surface area and a loose, porous structure. They are used as templates or precursors for preparing metal nanoparticles, porous carbon composites, and other nanostructures. Despite significant efforts in CTH reactions, some unresolved issues remain regarding the rational design and accurate synthesis of heterogeneous catalysts to achieve lower-energy and more economical processes. For example, noble metal catalysts such as Pd, Ru, Au, and Pt have been frequently used in past reports; however, their high cost limits their widespread use, and noble metals are prone to over-hydrogenation, leading to byproducts. Conventional non-noble metal catalysts often fail to achieve the desired catalytic performance, and catalyst preparation often involves complex modification processes. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing process for preparing sugar alcohols by hydrogenation of furfural, which often uses expensive precious metal catalysts or non-precious metal catalysts that fail to achieve the required catalytic effect, and the preparation of catalysts is often accompanied by complex modification processes. The present invention provides a method for preparing ZIF-based high-entropy alloy catalysts.
[0005] The purpose of this invention is to provide a ZIF-based high-entropy alloy catalyst prepared by the aforementioned method.
[0006] Another object of the present invention is to provide the application of the ZIF-based high-entropy alloy catalyst.
[0007] The above-mentioned objective of this invention is achieved through the following technical solution:
[0008] This invention protects a method for preparing a ZIF-based high-entropy alloy catalyst, comprising the following steps:
[0009] S1. Prepare metal salt solution and benzimidazole solution separately, and mix them to react and obtain catalyst precursor;
[0010] S2. The catalyst precursor obtained in step S1 is first calcined at 700-800℃ for 0.5-1.5h under a protective gas atmosphere, and then calcined again under a reducing gas atmosphere until complete, thus obtaining the ZIF-based high-entropy alloy catalyst. Calcination under a protective gas atmosphere is mainly to carbonize the MOF, and calcination under a reducing gas atmosphere is to reduce the metal.
[0011] The metal salt solution contains nickel, cobalt, copper, and iron ions;
[0012] The benzimidazole solution contains zinc ions;
[0013] The molar ratio of nickel, cobalt, copper, and iron ions in the metal salt solution to zinc ions in the benzimidazole solution is 1:(0.9–1.1):(0.9–1.1):(0.9–1.1):(9.5–10.5). Zinc, as the main metal in the metal-organic framework (ZIF), needs to maintain the highest possible content. After forming the ZIF precursor, a small amount of other metals is added to replace zinc, facilitating the incorporation of other metals into the ZIF framework without affecting the overall structure of the ZIF.
[0014] The preparation method of a catalyst directly affects the dispersion, actual loading, and particle size distribution of the active components, thus influencing the catalyst's activity. To address the shortcomings of existing technologies, the inventors' team synthesized a novel high-entropy alloy catalyst with a carbon support integrally encapsulating a high-entropy alloy structure. Specifically, benzimidazole was selected as a ligand, which promotes metal dispersion in the precursor liquid, reduces metal particle size, and prevents metal agglomeration or precipitation. Simultaneously, the carbon support formed after reduction and calcination acts as an effective metal protectant to inhibit metal leaching, providing a stable ZIF-based high-entropy catalyst. The resulting catalyst was used for the catalytic hydrogenation of furfural to furfuryl alcohol, achieving complete conversion of furfural (up to 100% conversion) to furfuryl alcohol (selectivity up to 95.4%) at relatively low temperatures (<150℃).
[0015] Furthermore, the nickel, cobalt, copper, iron, and zinc ions are respectively Ni 2+ Co 2+ Cu 2+ Fe 3+ Zn 2+ .
[0016] Furthermore, the nickel ions are derived from soluble nickel salts selected from nickel acetate, nickel nitrate, nickel chloride, or hydrates of any of the above nickel salts.
[0017] More preferably, the soluble nickel salt is any one of nickel acetate tetrahydrate, nickel nitrate hexahydrate, and nickel chloride hexahydrate. Anhydrous cobalt salts are expensive; therefore, considering cost, this application selects the relatively inexpensive anhydrous cobalt salt. The principles for using the other four metal ions are the same as above.
[0018] Furthermore, the cobalt ions are derived from soluble cobalt salts selected from cobalt acetate, cobalt nitrate, cobalt chloride, or hydrates of any of the above cobalt salts.
[0019] Furthermore, the copper ions are derived from soluble copper salts, which are selected from copper acetate, copper nitrate, copper chloride, or hydrates of any of the above copper salts.
[0020] Furthermore, the iron ions are derived from soluble iron salts, which are selected from ferric nitrate, ferric acetate, ferric chloride, or hydrates of any of the above iron salts.
[0021] Furthermore, the zinc ions are derived from a soluble zinc salt, which is selected from zinc acetate, zinc nitrate, zinc chloride, or a hydrate of any of the above zinc salts.
[0022] Preferably, the molar ratio of benzimidazole to zinc ions in the benzimidazole solution is 1:(0.6-0.8).
[0023] Preferably, the polar organic solvent is selected from methanol, ethanol, or isopropanol.
[0024] Preferably, the molar ratio of benzimidazole to the polar organic solvent is 1:(14-16).
[0025] Furthermore, the preparation of the benzimidazole solution includes the following steps: dissolving benzimidazole in a polar organic solvent, adding ammonium hydroxide and zinc salt to it, and mixing thoroughly to obtain the solution.
[0026] Furthermore, the preparation of the metal salt solution includes the following steps: adding four metal salts, namely nickel salt, cobalt salt, copper salt and iron salt, into a polar organic solvent in no particular order and mixing them thoroughly to obtain the metal salt solution;
[0027] Preferably, the reducing gas is selected from hydrogen and carbon monoxide.
[0028] Furthermore, the protective gas is selected from nitrogen, argon, helium, or neon.
[0029] Preferably, the calcination time under a protective gas atmosphere is 0.8 to 1.2 hours, more preferably 1 hour.
[0030] Preferably, the calcination time is 2-3 hours, more preferably 2 hours.
[0031] Furthermore, the calcination heating rate is 2 to 10 °C / min, more preferably 5 °C / min.
[0032] Furthermore, in step S1, the mixing reaction is followed by post-processing, which includes centrifugation, washing, and drying.
[0033] More specifically, the post-treatment involves centrifuging the fully reacted mixture, washing the precipitate with methanol, centrifuging again, repeating this step 3 to 5 times, and then placing the washed precipitate in a forced-air drying oven at 90 to 120°C (preferably 105°C) for drying for 8 to 24 hours (preferably 24 hours) to obtain the catalyst precursor.
[0034] This invention also protects the ZIF-based high-entropy alloy catalyst prepared by the aforementioned method.
[0035] Furthermore, with the total molar content of metal elements as 100%, the relative molar content ratio of nickel, cobalt, copper, iron and zinc in the ZIF-based high-entropy alloy catalyst is 1%~3.5%: 10~15%: 12%~26%: 6.5%~21%: 35%~70%.
[0036] This invention also protects the application of the ZIF-based high-entropy alloy catalyst in furfural hydrogenation.
[0037] Furthermore, the furfural hydrogenation is carried out in a hydrogen atmosphere using isopropanol as a solvent, where furfural is hydrogenated to produce sugar alcohol under the action of a ZIF-based high-entropy alloy catalyst.
[0038] Preferably, the catalytic temperature of the ZIF-based high-entropy alloy catalyst in the hydrogenation of furfural is 110–140 °C.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] This invention utilizes a novel preparation method to synthesize a novel ZIF-based high-entropy alloy catalyst with a carbon support integrally encapsulating a high-entropy alloy structure. Specifically, benzimidazole is selected as a ligand, which can promote metal dispersion in the precursor liquid, reduce metal particle size, and prevent metal agglomeration or precipitation. At the same time, the carbon support formed after reduction and calcination acts as an effective metal protectant to inhibit metal leaching, providing a stable high-entropy catalyst. The obtained catalyst is used for the catalytic hydrogenation of furfural to prepare furfuryl alcohol, achieving complete conversion of furfural (up to 100% conversion rate) to furfuryl alcohol (selectivity up to 95.4%) at a relatively low temperature (<150℃). Attached Figure Description
[0041] Figure 1 The image shows the SEM image of the ZIF-based high-entropy alloy catalyst obtained in Example 1.
[0042] Figure 2 The EDS spectrum is used to characterize the dispersion characteristics and core-shell structure of the ZIF-based high-entropy alloy catalyst obtained in Example 1.
[0043] Figure 3 The images show TEM images (a, b) of the ZIF-based high-entropy alloy catalyst obtained in Example 1 and the particle size distribution of the high-entropy alloy nanoparticles in the catalyst (c).
[0044] Figure 4 The images show TEM images (a, b) of the ZIF-based high-entropy alloy catalyst obtained in Example 3 and the particle size distribution of the high-entropy alloy nanoparticles in the catalyst (c).
[0045] Figure 5 The above are statistical diagrams of X-ray diffraction data of ZIF-based high-entropy alloy catalysts obtained in Examples 1-3.
[0046] Figure 6 The image shows a statistical graph of the X-ray diffraction data of the catalyst obtained in Comparative Example 1.
[0047] Figure 7 The chart shows the statistical data of H2 adsorption content analysis of the ZIF-based high-entropy alloy catalysts obtained in Examples 1-3. Detailed Implementation
[0048] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.
[0049] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.
[0050] Example 1: Preparation of ZIF-based high-entropy alloy catalyst
[0051] 0.5 mmol nickel acetate tetrahydrate (0.124 g), cobalt acetate tetrahydrate (0.125 g), copper acetate monohydrate (0.1 g), and ferric nitrate nonahydrate (0.202 g) were dissolved in 20 mL of methanol to obtain mixture A. 10 mmol benzimidazole (1.2 g) was dissolved in 150 mmol methanol (48 g). 10 mmol ammonium hydroxide (0.6 g) and 5 mmol zinc acetate dihydrate (1.100 g) were added while stirring at room temperature. The mixture was stirred at 300 rpm for 10 min at room temperature to obtain suspension B. Mixture A was poured into suspension B, and the mixture was stirred at 300 rpm for 3 h at room temperature to obtain suspension C. The suspension was centrifuged at 3000 r / min for 8 min, the centrifuged liquid was discarded, 20 mL of methanol was added and centrifuged again. This step was repeated three times to collect solid D, which was dried in a 105℃ forced-air drying oven for 24 h to obtain solid E. Solid E was placed in an atmosphere furnace and heated to 800℃ at a rate of 5℃ / min under a nitrogen atmosphere and held for 1 h. Then the atmosphere was changed to a hydrogen atmosphere and calcined for another 2 h to obtain the ZIF-based high-entropy alloy catalyst.
[0052] Example 2: Preparation of ZIF-based high-entropy alloy catalyst
[0053] The difference from Example 1 is that the calcination temperature of Example 2 is 750°C. Specifically, solid E is placed in an atmosphere furnace and heated to 750°C at a rate of 5°C / min under a nitrogen atmosphere and held for 1 hour. Then, the atmosphere is changed to a hydrogen atmosphere and calcination is continued for 2 hours to obtain the ZIF-based high-entropy alloy catalyst.
[0054] The other steps and parameters are the same as in Example 1.
[0055] Example 3: Preparation of ZIF-based high-entropy alloy catalyst
[0056] The difference from Example 1 is that the calcination temperature of Example 3 is 700°C. Specifically, solid E is placed in an atmosphere furnace and heated to 700°C at a rate of 5°C / min under a nitrogen atmosphere and held for 1 hour. Then, the atmosphere is changed to a hydrogen atmosphere and calcination is continued for 2 hours to obtain the ZIF-based high-entropy alloy catalyst.
[0057] The other steps and parameters are the same as in Example 1.
[0058] Example 4: Preparation of ZIF-based high-entropy alloy catalyst
[0059] In Example 4, the molar ratio of nickel acetate tetrahydrate, cobalt acetate tetrahydrate, copper acetate monohydrate, ferric nitrate nonahydrate, and zinc acetate dihydrate was 1:0.9:0.9:0.9:10, specifically 0.5 mmol nickel acetate tetrahydrate (0.124 g), 0.45 mmol cobalt acetate tetrahydrate (0.112 g), copper acetate monohydrate (0.898 g), ferric nitrate nonahydrate (0.182 g), and 5 mmol zinc acetate dihydrate (1.100 g).
[0060] The other steps and parameters are the same as in Example 1.
[0061] Example 5: Preparation of ZIF-based high-entropy alloy catalyst
[0062] In Example 5, the molar ratio of nickel acetate tetrahydrate, cobalt acetate tetrahydrate, copper acetate monohydrate, ferric nitrate nonahydrate, and zinc acetate dihydrate was 1:1.1:1.1:1.1:10, specifically 0.5 mmol nickel acetate tetrahydrate (0.124 g), 0.55 mmol cobalt acetate tetrahydrate (0.137 g), copper acetate monohydrate (0.110 g), ferric nitrate nonahydrate (0.222 g), and 5 mmol zinc acetate dihydrate (1.100 g).
[0063] The other steps and parameters are the same as in Example 1.
[0064] Comparative Example 1: Preparation of a non-high-entropy alloy furfural hydrogenation catalyst
[0065] The difference from Example 1 is that the calcination temperature of Comparative Example 1 was 600°C, at which point the metal was not completely reduced and remained in a non-high-entropy alloy state. Figure 6 .
[0066] The other steps and parameters are the same as in Example 1.
[0067] Comparative Example 2: Preparation of Non-High Entropy Alloy Furfural Hydrogenation Catalyst
[0068] The difference from Example 1 is that the molar ratio of nickel acetate tetrahydrate, cobalt acetate tetrahydrate, copper acetate monohydrate, ferric nitrate nonahydrate, and zinc acetate dihydrate in Comparative Example 2 is 1:1:1:1:1, specifically 0.5 mmol nickel acetate tetrahydrate (0.124 g), cobalt acetate tetrahydrate (0.125 g), copper acetate monohydrate (0.1 g), ferric nitrate nonahydrate (0.202 g), and 0.5 mmol zinc acetate dihydrate (0.110 g).
[0069] At this point, the zinc salt content, which forms the main framework of the MOF, is similar to that of other metals. As the other four metals are added to the MOF precursor, most of the zinc salt is replaced, affecting the formation of the MOF. The MOF loses its coordination anchoring of the five metals, and metal precipitation is likely to occur during the subsequent reduction process, making it impossible to form a pure phase high-entropy alloy.
[0070] The other steps and parameters are the same as in Example 1.
[0071] Experimental Performance Testing
[0072] (1) Determination of furfural conversion rate
[0073] 1. Experimental Method:
[0074] 0.05 g of the ZIF-based high-entropy alloy catalyst prepared in Examples 1-3 was loaded into a polytetrafluoroethylene liner of a magnetically stirred reactor, along with 0.05 g of furfural and 20 mL of isopropanol. A stir bar was placed in the reactor, the liner was placed inside, and the reactor was sealed. Hydrogen gas was purged 2-3 times. The reaction was carried out at 400 rpm under a hydrogen pressure of 2 MPa, starting from the time the target temperature was reached, for 9 hours. After the reaction was complete, the mixture was allowed to cool naturally to room temperature. The liquid product was collected, filtered through an organic filter membrane (13 mm × 0.22 μm), diluted, and tested using an Agilent 8860 microscope. The furfural conversion rate and furfuryl alcohol selectivity in the liquid were used as indicators; higher furfural conversion rate and higher furfuryl alcohol selectivity indicated better catalytic performance.
[0075] 2. Experimental Results
[0076] Table 1 Furfural Conversion Rate
[0077]
[0078] The experimental results are shown in Table 1. The furfural hydrogenation catalysts obtained in Examples 1 to 3 have good low-temperature catalytic activity. The furfural conversion rate reaches 100% at a catalytic temperature of 140℃. In particular, the selectivity of furfural obtained in Example 1 can reach 87.7% at a catalytic temperature of 120℃.
[0079] In addition, the catalysts obtained in Examples 4 and 5 have essentially the same catalytic effect as those in Example 1, and will not be described again here.
[0080] (2) Morphology and particle size distribution determination
[0081] The furfural hydrogenation catalyst obtained in Example 1 was analyzed using scanning electron microscopy (SEM), and the results are as follows: Figure 1 As shown, most of the high-entropy alloys have uniform morphology and size, and are dispersed on the carbon support.
[0082] The furfural hydrogenation catalyst obtained in Example 1 was analyzed using TEM field transmission electron microscopy combined with energy dispersive spectroscopy. The results are as follows: Figure 2 As shown, the catalyst obtained in Example 1 contains five elements: Fe, Co, Ni, Cu, and Zn. The high-entropy alloy is distributed in the catalyst in particulate form, and the C element encapsulates the other five elements, exhibiting a structure in which the carbon support completely encapsulates the high-entropy alloy. The catalysts obtained in Examples 2-5 have essentially the same structural characteristics as those in Example 1, and will not be described again here.
[0083] The ZIF-based high-entropy alloy catalysts obtained in Examples 1 and 3 were subjected to TEM morphology and particle size determination. The results are as follows: Figures 3-4 As shown, by Figure 3 It can be seen that the catalyst obtained in Example 1 is well dispersed, with high-entropy alloy particles (black particles) uniformly distributed on the carbon support. The particle size distribution of HEA nanoparticles in catalysts calcined at different temperatures varies; the smaller the particle size, the better the catalytic activity. Example 1 has the smallest particle size and the best catalytic activity, achieving 100% furfural conversion and 95.4% furfuryl alcohol selectivity at 140℃.
[0084] (3) X-ray diffraction
[0085] X-ray diffraction analysis was performed on the ZIF-based high-entropy alloy catalysts obtained in Examples 1-3, and the results are as follows: Figure 5 As shown in the figure, the catalyst obtained by calcination in the example contains high entropy alloy (HEA) and FeCoNi ternary alloy.
[0086] In addition, the catalysts obtained in Examples 4 and 5 have similar X-ray diffraction characteristics to those in Example 1, and all contain high-entropy alloy (HEA) and FeCoNi ternary alloy, which will not be described in detail here.
[0087] The X-ray diffraction measurement results of Comparative Example 1 are as follows: Figure 6 As shown, the ligands have not yet been carbonized and still exhibit the special peak shape of the corresponding metal-organic framework. The metal is still in the elemental state and oxidation state and has not yet formed a high-entropy alloy.
[0088] (4) H2-TPD analysis
[0089] The ZIF-based high-entropy alloy catalysts obtained in Examples 1-3 were subjected to H2-TPD analysis, and the results are as follows: Figure 7As shown, the H2 desorption curve of the catalyst can be divided into two regions: the first region is around 500–600℃, and the second region is 600–700℃. Example 1 shows two desorption peaks in the second region, corresponding to the two active sites in the catalyst, HEA and the FeCoNi ternary alloy, but the peak intensity of the ternary alloy is very weak. The hydrogen desorption peak of Example 2 is in the same temperature range as that of Example 1, indicating that the hydrogen binding ability of the catalyst in Example 2 is the same as that in Example 1, only with slightly fewer hydrogen capture sites, reflected in a smaller peak area than that in Example 1. The hydrogen desorption peak area and desorption temperature of Example 3 are both weaker than those of Example 1, indicating a weaker hydrogen binding ability and fewer hydrogen capture sites. To a certain extent, stronger hydrogen adsorption by the catalyst manifests as a stronger hydrogen supply capacity in the furfural hydrogenation reaction.
[0090] In addition, the catalysts obtained in Examples 4 and 5 have similar H2-TPD analysis to those in Example 1, which will not be repeated here.
[0091] (5) ICP-OES analysis
[0092] Table 2. Relative molar metal content of furfural hydrogenation catalysts at different reduction temperatures, analyzed by ICP-OES.
[0093]
[0094]
[0095] Note: The total molar amount of metal in the catalyst is taken as 100%.
[0096] ICP-OES analysis was performed using the catalysts obtained in Examples 1 and 3 as representatives. The results are shown in Table 2. As the reduction temperature increased, the zinc content gradually decreased, which was due to the evaporation of zinc. Correspondingly, the molar proportion of other metal elements gradually increased. The multiple active sites of the high-entropy alloy were more likely to play a role. It is quite obvious that compared with Comparative Example 1, Examples 1 and 3 both showed better catalytic performance for furfural.
[0097] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. Application of a ZIF-based high-entropy alloy catalyst in the preparation of furfuryl alcohol by hydrogenation of furfural, characterized in that, The ZIF-based high-entropy alloy catalyst is prepared by the following steps: S1. Prepare metal salt solution and benzimidazole solution separately, and mix them to react and obtain catalyst precursor; S2. The catalyst precursor obtained in step S1 is first calcined at 800 °C for 0.5~1.5 h in a protective gas atmosphere, and then calcined again in a reducing gas atmosphere until complete, thus obtaining the ZIF-based high-entropy alloy catalyst. The metal salt solution contains nickel, cobalt, copper, and iron ions; The benzimidazole solution contains zinc ions; The molar ratio of nickel, cobalt, copper, and iron ions in the metal salt solution to zinc ions in the benzimidazole solution is 1:(0.9~1.1):(0.9~1.1):(0.9~1.1):(9.5~10.5). The preparation of the benzimidazole solution includes the following steps: dissolving benzimidazole in a polar organic solvent, adding ammonium hydroxide and zinc salt to it, and mixing thoroughly to obtain the solution; Based on the total molar content of metal elements as 100%, the relative molar contents of nickel, cobalt, copper, iron and zinc in the ZIF-based high-entropy alloy catalyst are 1%~3.5%: 10~15%: 12%~26%: 6.5%~21%: 35%~70%, respectively.
2. Use according to claim 1, characterized in that, The molar ratio of benzimidazole to zinc ions in the benzimidazole solution is 1:(0.6~0.8).
3. The application according to claim 1, characterized in that, The preparation of the metal salt solution includes the following steps: adding four metal salts, namely nickel salt, cobalt salt, copper salt and iron salt, into a polar organic solvent in no particular order and mixing them thoroughly to obtain the metal salt solution.
4. The application according to claim 1 or 3, characterized in that, The polar organic solvent is selected from methanol, ethanol or isopropanol.
5. The application according to claim 1, characterized in that, The nickel ions are derived from soluble nickel salts selected from nickel acetate, nickel nitrate, nickel chloride, or hydrates of any of the above nickel salts.
6. The application according to claim 1, characterized in that, The cobalt ions are derived from soluble cobalt salts selected from cobalt acetate, cobalt nitrate, cobalt chloride, or hydrates of any of the above cobalt salts.
7. The application according to claim 1, characterized in that, The iron ions are derived from soluble iron salts selected from ferric nitrate, ferric chloride, or hydrates of any of the above iron salts.
8. In the application according to claim 1, the copper ions are derived from a soluble copper salt selected from copper acetate, copper nitrate, copper chloride, or a hydrate of any of the above copper salts.
9. The application according to claim 1, characterized in that, The zinc ions are derived from soluble zinc salts selected from zinc acetate, zinc nitrate, zinc chloride, or hydrates of any of the above zinc salts.
10. The application according to claim 1, characterized in that, The ZIF-based high-entropy alloy catalyst has a catalytic temperature of 120~140 °C in furfural hydrogenation.
11. The application according to claim 1, characterized in that, The furfural hydrogenation is carried out in a hydrogen atmosphere using isopropanol as a solvent, where furfural is hydrogenated to furfuryl alcohol under the action of a ZIF-based high-entropy alloy catalyst.
Citation Information
Patent Citations
Monatomic catalyst and application thereof
CN112156802A
Carbon-based multi-metal-site super-lean high-entropy alloy catalyst as well as preparation method and application thereof
CN114588951A