An antibacterial material containing modified polyurethane thermoplastic elastomer and preparation method thereof
By using a combination of modified polyurethane, chemical cross-linked structure of polyurethane and epoxy nano-silica and cardanol in antibacterial materials, the problem of insufficient antibacterial performance and tensile properties of existing antibacterial materials is solved, and efficient antibacterial properties are achieved. effect and good mechanical properties.
Patent Information
- Application Number
- CN202410677636.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-05-29
AI Technical Summary
Existing antibacterial materials have deficiencies in antibacterial performance and tensile properties, making it difficult to meet the needs of efficient antibacterial and good mechanical properties at the same time.
An antibacterial material containing modified polyurethane thermoplastic elastomer is used. By reacting modified polyurethane, polyurethane and epoxy nano-silica under specific proportions and conditions, a stable chemical cross-linked structure is formed, and cardanol is added to enhance the antibacterial performance. .
It achieves good antibacterial effect and high tensile properties of the material. The diameter of the antibacterial zone reaches 15.8-16.8mm, and the tensile property reaches 41.6-42.8MPa, which significantly improves the mechanical properties of the material.
Smart Images

Figure CN118440491B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of antibacterial technology, in particular to an antibacterial material containing a modified polyurethane thermoplastic elastomer and a preparation method thereof. Background Art
[0002] Polyurethane (PU) is a thermoplastic elastomer, also known as thermoplastic polyurethane rubber (TPU). It is a (AB)n type block linear polymer, usually connected by diphenylmethane diisocyanate (MDI). Polyurethane thermoplastic elastomers are cross-linked by intermolecular hydrogen bonds or light cross-linking between macromolecular chains. These two cross-linking structures are reversible as the temperature rises or falls.
[0003] Cardanol is a natural phenolic compound extracted from cashew shell and cashew peel. It has multiple biological activities such as antioxidant and antibacterial. The present invention applies cardanol to antibacterial materials to further improve their antibacterial properties. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies of the prior art, the present invention provides an antibacterial material containing a modified polyurethane thermoplastic elastomer and a preparation method thereof, which has good antibacterial properties and tensile properties.
[0006] (II) Technical solution
[0007] To achieve the above object, the present invention provides the following technical solution: an antibacterial material containing modified polyurethane thermoplastic elastomer, comprising the following weight components: 20-30 parts by weight of modified polyurethane, 80-100 parts by weight of polyurethane, and 3-5 parts by weight of epoxy nano-silica.
[0008] Preferably, the preparation method of the polyurethane comprises the following steps: removing water from the polyether diol and mixing it evenly with hexamethylene diisocyanate, introducing nitrogen, then dropping a dibutyltin dilaurate catalyst, reacting at 50-80°C for 2-4h, performing prepolymerization, then adding a triazine-based chain extender, stirring to continue the chain extension reaction, and after the reaction is completed, cooling and discharging to obtain the polyurethane.
[0009] Preferably, the mass ratio of the polyether diol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and triazine-based chain extender is 1.2-2:1:0.01-0.02:0.4-0.8.
[0010] Preferably, the preparation method of the triazine-based chain extender is:
[0011] (1) adding ethylenediamine and 1,3-propane sultone to an acetone solvent for dissolution, then dropping a sodium hydroxide solution with a concentration of 2-6%, reacting at 60-90° C. for 6-12 hours, concentrating under reduced pressure after the reaction to remove the solvent, and recrystallizing the crude product in ethanol to obtain sodium sulfonate modified ethylenediamine;
[0012] (2) Adding sodium sulfonate modified ethylenediamine to a 3-6% sodium hydroxide aqueous solution, stirring to dissolve, then adding dropwise an acetone solution containing diethanolamine-dichlorotriazine at 2-5° C., stirring for 40-50 minutes, and then stirring and reacting at 25-50° C. for 2-4 hours, finally heating to 70-90° C., stirring and reflux for 10-14 hours, distilling under reduced pressure after the reaction, adding the precipitated product to ethanol for recrystallization, and obtaining a triazine-based chain extender.
[0013] Preferably, the mass ratio of ethylenediamine to 1,3-propane sultone in (1) is 1:1.2-1.6.
[0014] Preferably, the mass ratio of sodium sulfonate-modified ethylenediamine to diethanolamine-dichlorotriazine in (2) is 2-3.4:1.
[0015] Preferably, the preparation method of the modified polyurethane is:
[0016] S1. Add purified polyurethane particles to dimethylformamide solvent, stir and dissolve at 90-100°C for 4-7h, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, pass nitrogen for protection, then add triethylamine, and oil bath at 45-60°C for 8-12h. After the reaction, wash with acetonitrile and dry to obtain olefinated polyurethane;
[0017] S2. Add olefinated polyurethane, cardanol, and 1,1′-bis(dimethylsilyl)ferrocene into the reactor, stir evenly, continue to add chloroplatinic acid catalyst, react at 50-70°C for 2-4h, filter after reaction, wash and dry to obtain modified polyurethane.
[0018] Preferably, the mass ratio of the polyurethane particles, methacrylate isothiocyanate, polyurethane film and triethylamine in S1 is 1.5-1.7:2.1-2.4:1:0.02-0.03.
[0019] Preferably, the mass ratio of olefinated polyurethane, cardanol, 1,1′-bis(dimethylsilyl)ferrocene and chloroplatinic acid catalyst in S2 is 1:0.8-1.2:0.4-0.9:0.02-0.04.
[0020] Preferably, the method comprises the following steps: adding modified polyurethane, polyurethane and epoxy nano-silica into a reaction kettle according to a ratio, pumping carbon dioxide into the reaction kettle with a booster pump, controlling the pressure at 0.8-1.2Mpa, controlling the temperature at 130-150°C, maintaining the pressure for 3-5h, and then rapidly releasing the pressure at a rate of 3-6Mpa / min, and after reducing the pressure to normal pressure, rapidly transferring the raw materials to a foaming device, heating for foaming, and cooling for finalizing to obtain an antibacterial material containing a modified polyurethane thermoplastic elastomer.
[0021] (III) Beneficial technical effects
[0022] The invention adds modified polyurethane, polyurethane and epoxy nano-silica into a reaction kettle, pumps carbon dioxide into the reaction kettle with a booster pump, controls the pressure and temperature, maintains the pressure, then quickly releases the pressure, and after the pressure is reduced to normal pressure, quickly transfers the raw materials to a foaming device, heats and foams, and cools and shapes, to obtain an antibacterial material containing a modified polyurethane thermoplastic elastomer.
[0023] During the heating process of the reactor, the terminal hydroxyl groups of the modified polyurethane and polyurethane will undergo a ring-opening reaction with the epoxy groups of the epoxy nano-silica, and the three will form a stable chemical cross-link, increase the interfacial compatibility between each other, and improve their mechanical properties.
[0024] The sodium sulfonate groups in polyurethane and the cardanol and ferrocene groups in modified polyurethane all have antibacterial effects, synergistically antibacterial, and constitute an antibacterial system; the long chain of cardanol will be entangled with polyurethane to form an interpenetrating network, which improves its mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the reaction scheme of triazine-based chain extender. DETAILED DESCRIPTION
[0026] Example 1
[0027] (1) adding ethylenediamine and 1,3-propane sultone to an acetone solvent for dissolution, wherein the mass ratio of ethylenediamine to 1,3-propane sultone is 1:1.2, then dropping 6 ml of a 2% sodium hydroxide solution, reacting at 60° C. for 6 h, concentrating under reduced pressure to remove the solvent after the reaction, and recrystallizing the crude product in ethanol to obtain sodium sulfonate modified ethylenediamine;
[0028] (2) adding sodium sulfonate-modified ethylenediamine to 5 ml of 3% sodium hydroxide aqueous solution, stirring to dissolve, and then dropping an acetone solution containing diethanolamine-dichloro-s-triazine at 2° C., wherein the mass ratio of sodium sulfonate-modified ethylenediamine to diethanolamine-dichloro-s-triazine is 2:1, stirring for 40 minutes, and then stirring and reacting at 25° C. for 2 hours, and finally heating to 70° C., stirring and reflux for 10 hours, and distilling under reduced pressure after the reaction, adding the precipitated product to ethanol for recrystallization to obtain a triazine-based chain extender;
[0029] (3) removing water from the polyether diol and mixing it evenly with hexamethylene diisocyanate, introducing nitrogen, then dropping a dibutyltin dilaurate catalyst, reacting at 50° C. for 2 hours to perform prepolymerization, and then adding a triazine-based chain extender, wherein the mass ratio of the polyether diol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and triazine-based chain extender is 1.2:1:0.01:0.4, stirring to continue the chain extension reaction, and after the reaction is completed, cooling and discharging to obtain a polyurethane;
[0030] (4) adding purified polyurethane particles to a dimethylformamide solvent, stirring and dissolving at 90° C. for 4 hours, and then drying to obtain a polyurethane film; adding methyl methacrylate isothiocyanate to the polyurethane film, introducing nitrogen for protection, and then adding triethylamine, wherein the mass ratio of the polyurethane particles, methyl methacrylate isothiocyanate, the polyurethane film, and the triethylamine is 1.5:2.1:1:0.02, and the reaction is carried out at 45° C. in an oil bath for 8 hours. After the reaction, washing with acetonitrile and drying are carried out to obtain an olefinic polyurethane;
[0031] (5) Adding olefinated polyurethane, cardanol, and 1,1′-bis(dimethylsilyl)ferrocene to a reactor, wherein the mass ratio of olefinated polyurethane, cardanol, 1,1′-bis(dimethylsilyl)ferrocene, and chloroplatinic acid catalyst is 1:0.8:0.4:0.02, stirring evenly, continuing to add chloroplatinic acid catalyst, reacting at 50° C. for 2 h, filtering after completion, washing and drying to obtain modified polyurethane;
[0032] (6) 20 parts by weight of modified polyurethane, 80 parts by weight of polyurethane, and 3 parts by weight of epoxy nano-silica are added to a reactor, and carbon dioxide is pumped into the reactor using a booster pump to control the pressure at 0.8 MPa and the temperature at 130°C. The pressure is maintained for 3 hours, and then the pressure is quickly released at a rate of 3 MPa / min. After the pressure is reduced to normal pressure, the raw materials are quickly transferred to a foaming equipment, heated for foaming, and cooled for setting to obtain an antibacterial material containing a modified polyurethane thermoplastic elastomer.
[0033] Example 2
[0034] (1) adding ethylenediamine and 1,3-propane sultone to an acetone solvent for dissolution, wherein the mass ratio of ethylenediamine to 1,3-propane sultone is 1:1.6, then dropping 12 ml of a 6% sodium hydroxide solution, reacting at 90° C. for 12 h, concentrating under reduced pressure to remove the solvent after the reaction, and recrystallizing the crude product in ethanol to obtain sodium sulfonate modified ethylenediamine;
[0035] (2) adding sodium sulfonate-modified ethylenediamine to 10 ml of 6% sodium hydroxide aqueous solution, stirring to dissolve, and then dropping an acetone solution containing diethanolamine-dichloro-s-triazine at 5° C., wherein the mass ratio of sodium sulfonate-modified ethylenediamine to diethanolamine-dichloro-s-triazine is 3.4:1, stirring for 50 minutes, and then stirring at 50° C. for 4 hours, and finally heating to 90° C., stirring and reflux for 14 hours, and distilling under reduced pressure after the reaction, adding the precipitated product to ethanol for recrystallization to obtain a triazine-based chain extender;
[0036] (3) removing water from the polyether diol and mixing it evenly with hexamethylene diisocyanate, introducing nitrogen, then dropping a dibutyltin dilaurate catalyst, reacting at 80° C. for 4 hours for prepolymerization, and then adding a triazine-based chain extender, wherein the mass ratio of the polyether diol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and triazine-based chain extender is 2:1:0.02:0.8, stirring to continue the chain extension reaction, and after the reaction is completed, cooling and discharging to obtain a polyurethane;
[0037] (4) adding purified polyurethane particles to a dimethylformamide solvent, stirring and dissolving at 100° C. for 7 hours, and then drying to obtain a polyurethane film; adding methyl methacrylate isothiocyanate to the polyurethane film, introducing nitrogen for protection, and then adding triethylamine, wherein the mass ratio of the polyurethane particles, methyl methacrylate isothiocyanate, the polyurethane film, and the triethylamine is 1.7:2.4:1:0.03, and the reaction is carried out at 60° C. in an oil bath for 12 hours. After the reaction, washing with acetonitrile and drying are carried out to obtain an olefinic polyurethane;
[0038] (5) Adding olefinated polyurethane, cardanol, and 1,1′-bis(dimethylsilyl)ferrocene to a reactor, wherein the mass ratio of olefinated polyurethane, cardanol, 1,1′-bis(dimethylsilyl)ferrocene, and chloroplatinic acid catalyst is 1:1.2:0.9:0.04, stirring evenly, continuing to add chloroplatinic acid catalyst, reacting at 70° C. for 4 hours, filtering after completion, washing and drying to obtain modified polyurethane;
[0039] (6) 30 parts by weight of modified polyurethane, 100 parts by weight of polyurethane, and 5 parts by weight of epoxy nano-silica are added to a reactor, and carbon dioxide is pumped into the reactor using a booster pump to control the pressure at 1.2 MPa and the temperature at 150°C. The pressure is maintained for 5 hours, and then the pressure is quickly released at a rate of 6 MPa / min. After the pressure is reduced to normal pressure, the raw materials are quickly transferred to a foaming equipment, heated for foaming, and cooled for setting to obtain an antibacterial material containing a modified polyurethane thermoplastic elastomer.
[0040] Example 3
[0041] (1) adding ethylenediamine and 1,3-propane sultone to an acetone solvent for dissolution, wherein the mass ratio of ethylenediamine to 1,3-propane sultone is 1:1.4, then dropping 9 ml of a 4% sodium hydroxide solution, reacting at 75° C. for 9 h, and concentrating under reduced pressure to remove the solvent after the reaction, and recrystallizing the crude product in ethanol to obtain sodium sulfonate modified ethylenediamine;
[0042] (2) adding sodium sulfonate-modified ethylenediamine to 7.5 ml of 4.5% sodium hydroxide aqueous solution, stirring to dissolve, and then dropping an acetone solution containing diethanolamine-dichloro-s-triazine at 3.5° C., wherein the mass ratio of sodium sulfonate-modified ethylenediamine to diethanolamine-dichloro-s-triazine is 2.7:1, stirring for 45 minutes, and then stirring and reacting at 37.5° C. for 3 hours, and finally heating to 80° C., stirring and reflux for 12 hours, and distilling under reduced pressure after the reaction, adding the precipitated product to ethanol for recrystallization to obtain a triazine-based chain extender;
[0043] (3) removing water from the polyether diol and mixing it with hexamethylene diisocyanate, introducing nitrogen, then dropping a dibutyltin dilaurate catalyst, reacting at 65° C. for 3 hours to perform prepolymerization, and then adding a triazine-based chain extender, wherein the mass ratio of the polyether diol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and triazine-based chain extender is 1.6:1:0.05:0.6, stirring to continue the chain extension reaction, and after the reaction is completed, cooling and discharging to obtain a polyurethane;
[0044] (4) Add purified polyurethane particles to dimethylformamide solvent, stir and dissolve at 95° C. for 5.5 hours, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, introduce nitrogen for protection, and then add triethylamine, wherein the mass ratio of polyurethane particles, methyl methacrylate isothiocyanate, polyurethane film, and triethylamine is 1.6:2.25:1:0.025, and place in an oil bath at 52.5° C. for 10 hours. After the reaction, wash with acetonitrile and dry to obtain an olefinated polyurethane;
[0045] (5) Adding olefinated polyurethane, cardanol, and 1,1′-bis(dimethylsilyl)ferrocene to a reactor, wherein the mass ratio of olefinated polyurethane, cardanol, 1,1′-bis(dimethylsilyl)ferrocene, and chloroplatinic acid catalyst is 1:1.0:0.65:0.03, stirring evenly, continuing to add chloroplatinic acid catalyst, reacting at 60° C. for 3 h, filtering after completion, washing and drying to obtain modified polyurethane;
[0046] (6) 25 parts by weight of modified polyurethane, 90 parts by weight of polyurethane, and 4 parts by weight of epoxy nano-silica are added to a reactor, and carbon dioxide is pumped into the reactor using a booster pump to control the pressure at 1.0 MPa and the temperature at 140°C. The pressure is maintained for 4 hours, and then the pressure is quickly released at a rate of 4.5 MPa / min. After the pressure is reduced to normal pressure, the raw materials are quickly transferred to a foaming equipment, heated for foaming, and cooled for setting to obtain an antibacterial material containing a modified polyurethane thermoplastic elastomer.
[0047] Comparative Example 1
[0048] Compared with Example 3, no modified polyurethane was added, and the other component raw materials were the same.
[0049] Comparative Example 2
[0050] Compared with Example 3, no polyurethane was added, and the raw materials of other components were the same.
[0051] Comparative Example 3
[0052] Compared with Example 3, no modified polyurethane and polyurethane were added, and the other component raw materials were the same.
[0053] A Staphylococcus aureus liquid with a concentration of 2×108 CFU / mL was added as a test strain to a sterilized culture dish, and then a solid agar medium was added and dissolved, cooled to 45°C, and then poured into a culture dish, 20 mL was poured into each plate with an inner diameter of 10 cm, and then the antibacterial materials of the embodiments of the present invention and the comparative example (with a diameter of 3 cm and a thickness of 1 mm) were placed on the culture plate, and cultured in a constant temperature incubator for 12 hours at a temperature of 37°C. After culture, the diameter of the inhibition zone was measured. The test results are shown in Table 1.
[0054] Table 1: Antimicrobial testing.
[0055]
[0056]
[0057] It can be seen from Table 1 that the diameter of the antibacterial zone of the antibacterial material containing the modified polyurethane thermoplastic elastomer of the present invention reaches 15.8-16.8 mm, indicating that it has a good antibacterial effect.
[0058] The tensile properties of the material were tested using an electronic universal testing machine. The test results are shown in Table 2.
[0059] Table 2: Tensile properties tested.
[0060] project Tensile properties (MPa) Example 1 41.6 Example 2 42.8 Example 3 41.9 Comparative Example 1 21.3 Comparative Example 2 20.4 Comparative Example 3 16.5
[0061] As can be seen from Table 2, the tensile properties of the antibacterial material containing the modified polyurethane thermoplastic elastomer of the present invention reach 41.6-42.8 MP, indicating that it has good tensile properties and therefore good mechanical properties.
[0062] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An antibacterial material containing a modified polyurethane thermoplastic elastomer, characterized in that: The invention comprises the following components by weight: 20-30 parts by weight of modified polyurethane, 80-100 parts by weight of polyurethane, and 3-5 parts by weight of epoxy nano-silicon dioxide; The preparation method of polyurethane comprises the following steps: removing water from polyether diol and mixing it evenly with hexamethylene diisocyanate, introducing nitrogen, then dropping dibutyltin dilaurate as a catalyst, reacting at 50-80° C. for 2-4 hours, performing prepolymerization, then adding a triazine chain extender, stirring to continue the chain extension reaction, and after the reaction is completed, cooling and discharging to obtain polyurethane; The preparation method of the triazine-based chain extender is: (1) Add ethylenediamine and 1,3-propane sultone to an acetone solvent to dissolve them, then dropwise add a 2-6% sodium hydroxide solution, react at 60-90° C. for 6-12 hours, and after the reaction, concentrate under reduced pressure to remove the solvent, and recrystallize the crude product in ethanol to obtain sodium sulfonate modified ethylenediamine; (2) adding sodium sulfonate modified ethylenediamine to a 3-6% sodium hydroxide aqueous solution, stirring to dissolve, then dropping an acetone solution containing diethanolamine-dichlorotriazine at 2-5°C, stirring for 40-50 minutes, then stirring at 25-50°C for 2-4 hours, finally heating to 70-90°C, stirring and reflux for 10-14 hours, distilling under reduced pressure after the reaction, adding the precipitated product to ethanol for recrystallization, and obtaining a triazine-based chain extender; The preparation method of the modified polyurethane is: S1. Add purified polyurethane particles to dimethylformamide solvent, stir and dissolve at 90-100°C for 4-7h, and then dry to obtain a polyurethane film; add methyl methacrylate isothiocyanate to the polyurethane film, pass nitrogen for protection, then add triethylamine, and oil bath at 45-60°C for 8-12h. After the reaction, wash with acetonitrile and dry to obtain olefinated polyurethane; S2. Add olefinated polyurethane, cardanol, and 1,1′-bis(dimethylsilyl)ferrocene into the reactor, stir evenly, continue to add chloroplatinic acid catalyst, react at 50-70°C for 2-4h, filter after reaction, wash and dry to obtain modified polyurethane.
2. The antibacterial material containing modified polyurethane thermoplastic elastomer according to claim 1, characterized in that: The mass ratio of the polyether diol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst and triazine chain extender is 1.2-2:1:0.01-0.02:0.4-0.
8.
3. The antibacterial material containing modified polyurethane thermoplastic elastomer according to claim 1, characterized in that: The mass ratio of ethylenediamine to 1,3-propane sultone in (1) is 1:1.2-1.
6.
4. The antibacterial material containing modified polyurethane thermoplastic elastomer according to claim 1, characterized in that: The mass ratio of sodium sulfonate-modified ethylenediamine to diethanolamine-dichlorotriazine in (2) is 2-3.4:
1.
5. The antibacterial material containing modified polyurethane thermoplastic elastomer according to claim 1, characterized in that: The mass ratio of the polyurethane particles, methacrylate isothiocyanate, polyurethane film and triethylamine in S1 is 1.5-1.7:2.1-2.4:1:0.02-0.
03.
6. The antibacterial material containing modified polyurethane thermoplastic elastomer according to claim 1, characterized in that: The mass ratio of olefinated polyurethane, cardanol, 1,1′-bis(dimethylsilyl)ferrocene and chloroplatinic acid catalyst in S2 is 1:0.8-1.2:0.4-0.9:0.02-0.
04.
7. A method for preparing an antibacterial material containing a modified polyurethane thermoplastic elastomer according to any one of claims 1 to 6, characterized in that: The following steps are involved: Modified polyurethane, polyurethane and epoxy nano-silica are added to a reactor according to the ratio, and carbon dioxide is pumped into the reactor with a booster pump to control the pressure at 0.8-1.2Mpa and the temperature at 130-150°C. The pressure is maintained for 3-5 hours, and then the pressure is quickly released at a rate of 3-6Mpa / min. After the pressure is reduced to normal pressure, the raw materials are quickly transferred to a foaming equipment, heated for foaming, and cooled for shaping to obtain an antibacterial material containing a modified polyurethane thermoplastic elastomer.