A micro-array cavity device and its protection method

By using a combination of two deposition rates in the microarray cavity device to form the seed layer and the surface film layer, the problems of low preparation efficiency and poor uniformity of the parylene protective film layer in the existing technology are solved, and a more efficient Water vapor isolation and improved stability.

CN118441240BActive Publication Date: 2024-10-25上海派拉纶新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410903619.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-25
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

In the process of miniaturization of micro-array cavity devices, the production of water vapor in semiconductor devices affects the performance. The preparation efficiency of the existing parylene protective film layer is low and the uniformity is difficult to ensure.

Method used

Two different deposition rates are used to deposit the first film layer and the second film layer in sequence. A seed layer with a lower deposition rate is formed first, and then the surface film layer is formed. The uniformity of the film layer is improved by controlling the thickness ratio, and the masking glue is removed. layer to achieve deposition of the parylene protective layer.

Benefits of technology

It effectively ensures the uniformity of film formation at different locations within the microarray cavity device, improves the deposition efficiency of the film layer, and reduces the cost of process preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118441240B_ABST
    Figure CN118441240B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of plating process technology, and in particular to a micro-array intracavity device and a protection method thereof. The protection method is beneficial to improving the safety and plating uniformity of the multi-channel semiconductor device by placing a multi-channel semiconductor device in a plating tool for positioning and distribution. At the same time, two different deposition rates are used to sequentially deposit a first film layer and a second film layer, that is, a lower deposition rate is first used to form a seed layer, which is beneficial to improving the uniformity of film formation in the gap between grains in the micro-array intracavity device, and can improve the deposition efficiency of the film layer, while reducing the cost of process preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plating technology, and in particular to a micro-array inner cavity device and a protection method thereof. Background Art

[0002] Parylene is a new type of thermoplastic used to make extremely thin films or deposited coatings. Parylene has good gas and water vapor barrier properties, physical and mechanical properties, electrical insulation and corrosion resistance. It is the most effective moisture-proof, mildew-proof, anti-corrosion and salt spray-proof coating material.

[0003] For micro-array intracavity devices, there are many channel structures inside after the semiconductor structure is formed. The heat absorption or heat release of these semiconductor devices will produce water vapor, thereby affecting the performance of the semiconductor device. The preparation of a parylene protective film layer for isolating water vapor is an effective solution. However, with the miniaturization of the size of micro-array intracavity devices, the density of semiconductor grains is getting larger and larger, and the gap between grains is getting smaller and smaller, resulting in low preparation efficiency of the protective film layer, and the uniformity of the protective film layer is difficult to ensure. Therefore, how to achieve uniform preparation of the protective film layer of micro-array intracavity devices is an urgent problem to be solved. Summary of the invention

[0004] The object of the present invention is to provide a micro-array intracavity device and a protection method thereof, so as to solve the problem of water vapor existing in the channel of the existing micro-array intracavity device.

[0005] In a first aspect, an embodiment of the present invention provides a method for protecting a micro-array intracavity device, comprising the following steps:

[0006] S100, forming a shielding adhesive layer in the area of ​​the micro-array inner cavity device where the parylene protective layer is not required;

[0007] S200, placing the micro-array inner cavity device prepared with the masking adhesive layer on a plating tool in a deposition chamber of a parylene plating device;

[0008] S300, depositing a first film layer in the internal channel of the micro-array intracavity device at a first deposition rate; the first deposition rate is 0.1 μm / h to 0.5 μm / h, and the thickness of the first film layer is 2 μm to 5 μm;

[0009] S400, continuously depositing a second film layer on the surface of the first film layer at a second deposition rate; the second deposition rate is 0.6 μm / h to 1.5 μm / h, the thickness of the second film layer is 10 μm to 20 μm, and the thickness ratio of the first film layer to the second film layer is 1:3 to 1:10;

[0010] S500, removing the masking adhesive layer, thereby obtaining the micro-array intracavity device with a parylene protective layer; wherein the parylene protective layer is composed of a first film layer and a second film layer.

[0011] Optionally, in step S300, depositing a first film layer in an internal channel of the microarray intracavity device using a first deposition rate includes:

[0012] The temperature of the evaporation chamber is 120℃~140℃, and the gas pressure of the deposition chamber is 10mTorr~15mTorr.

[0013] Optionally, in step S400, the step of continuously depositing the second film layer on the surface of the first film layer at a second deposition rate includes:

[0014] The temperature of the evaporation chamber is 130°C~160°C, and the gas pressure of the deposition chamber is 15mTorr~20mTorr.

[0015] Optionally, between step S200 and step S300, the following steps are further included:

[0016] S201, placing a C-type p-xylene raw material in a parylene coating device, sealing and evacuating the device;

[0017] S202, when the vacuum degree of the deposition chamber reaches 6mTorr~12mTorr, the raw material is heated and gasified to form paraxylene vapor;

[0018] S203, the p-xylene vapor is cracked to form monomer toluene vapor, and is transported into the deposition chamber through a pipeline to achieve a parylene protective layer deposition process.

[0019] Optionally, in step S100, a shielding adhesive layer is formed in a region of the micro-array cavity device where a parylene protective layer is not required, including:

[0020] S110, forming a rectangular glue frame by connecting the ends in a staggered manner, and making the outer edge of the rectangular glue frame just flush with the outer edge of the micro-array inner cavity device;

[0021] S120, using the same glue in the rectangular glue frame to fill it in a bow shape to form the masking glue layer.

[0022] Optionally, in step S200, placing the micro-array cavity device prepared with the shielding adhesive layer on a plating tool in a deposition chamber of a parylene plating device comprises:

[0023] S210, placing a plurality of the micro-array inner cavity devices prepared with a masking adhesive layer on the positioning marks preset on the plating tool in sequence;

[0024] S220, placing the entire plating tool at a position close to the edge of the turntable of the deposition chamber.

[0025] Optionally, before step S210, the method further includes:

[0026] A plating tool is provided; the plating tool is provided with a plurality of positioning marks which are evenly arranged.

[0027] Optionally, in step S500, the masking glue layer is removed to obtain the micro-array cavity device with the parylene protective layer, including:

[0028] S510, after the deposition process of the parylene protective layer is completed, a laser is used to disconnect the area where the shielding adhesive layer is connected to the micro-array intracavity device; wherein the laser pulse width is 10 ps to 100 ps, ​​and the wavelength is 355 nm.

[0029] Optionally, in step S510, the step of using a laser to disconnect the region where the shielding adhesive layer is connected to the micro-array intracavity device comprises:

[0030] S511, placing the micro-array cavity device after the parylene protective layer deposition process into a jig sideways so that the side to be cut is exposed;

[0031] S512, cutting along the boundary of the masking adhesive layer using preset laser parameters;

[0032] S513, removing the masking adhesive layer.

[0033] In a second aspect, the present invention further provides a micro-array intracavity device obtained by using the protection method described in the first aspect.

[0034] The embodiments of the present invention have at least the following technical effects:

[0035] The protection method for a micro-array intracavity device provided in an embodiment of the present invention uses two different deposition rates to sequentially deposit a first film layer and a second film layer, that is, a seed layer is first formed at a lower deposition rate to form a non-differentiated base layer on the surface of the internal channel of the micro-array intracavity device, which can avoid particle aggregation caused by an excessively fast initial growth rate, and then a surface film layer is formed on the seed layer to improve the uniformity of the film layer. By controlling the thickness value and thickness ratio of the seed layer and the subsequent surface film layer, the uniformity of film formation at different positions in the multi-channel semiconductor device can be effectively guaranteed, and at the same time, the deposition efficiency of the film layer can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 A schematic diagram of the overall structure of a parylene plating device provided in an embodiment of the present invention;

[0038] Figure 2 A flow chart of a protection method for a micro-array intracavity device provided by an embodiment of the present invention;

[0039] Figure 3 A schematic diagram of a first deposition rate and a second deposition rate provided in an embodiment of the present invention;

[0040] Figure 4 The embodiment of the present invention provides Figure 2 Schematic diagram of the process between step S200 and step S300;

[0041] Figure 5 The embodiment of the present invention provides Figure 2 Specific flow diagram of step S100;

[0042] Figure 6 The embodiment of the present invention provides Figure 2 Specific flow diagram of step S200;

[0043] Figure 7 The embodiment of the present invention provides Figure 2 Specific flow diagram of step S500;

[0044] Figure 8 The embodiment of the present invention provides Figure 7 Specific flow diagram of step S510;

[0045] Fig. 9 A schematic diagram of the specific structure of a micro-array intracavity device provided by an embodiment of the present invention;

[0046] Fig.10 A schematic diagram of the specific structure of a parylene protective film layer inside a micro-array cavity device provided by an embodiment of the present invention.

[0047] Icons: 100-evaporation chamber; 200-cracking chamber; 300-deposition chamber; 310-turntable; 320-plating tooling; 400-semiconductor refrigeration chip; 410-cold substrate; 420-hot substrate; 430-conductive layer; 440-grain gap; 450-parylene protective film layer; 451-first film layer; 452-second film layer. DETAILED DESCRIPTION

[0048] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Those skilled in the art will understand that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art in the field to which the present invention belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as here.

[0050] Those skilled in the art will appreciate that, unless otherwise stated, the singular forms "a", "an", "said" and "the" used herein may also include plural forms. It should be further understood that the term "comprising" used in the specification of the present invention refers to the presence of the features, integers, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof. The term "and / or" used herein includes all or any unit and all combinations of one or more associated listed items.

[0051] Combination Figures 1 to 3 As shown, an embodiment of the present invention provides a method for protecting a micro-array intracavity device, comprising the following steps:

[0052] S100, forming a shielding adhesive layer in an area of ​​the micro-array inner cavity device where a parylene protective layer does not need to be prepared.

[0053] Specifically, the area of ​​the micro-array cavity device that does not need to be prepared with a protective layer (such as a pad or substrate) is coated with a layer of UV light-curing glue on the substrate or pad using a high-precision glue coating device. The glue coating is a zero-tolerance coating, that is, by selecting a suitable UV glue, a nozzle with a smaller diameter and an optimized path for spraying the UV glue, and then achieving it through a two-step method.

[0054] S200, placing the micro-array inner cavity device prepared with the masking adhesive layer on a plating tool in a deposition chamber of a parylene plating device.

[0055] Specifically, the plating tool 320 is used to carry the micro-array intracavity devices. The semiconductor device with masking glue has weak adhesion with the carrying component, which can prevent the smaller micro-array intracavity devices from slipping and uneven position distribution when the turntable 310 of the deposition chamber 300 rotates.

[0056] It can be understood that the parylene plating device generally includes: a silo, an evaporation chamber 100, a cracking chamber 200 and a deposition chamber 300 arranged in sequence. The silo stores powdered paraxylene raw materials, and the silo includes a silo door. By opening the silo door, the paraxylene raw materials can be added to the silo, and closing the silo door can seal the silo. The inlet of the evaporation chamber 100 is connected to the silo, and the evaporation chamber 100 is heated at about 150°C and sublimated into a gaseous dimer molecule state. The outlet of the evaporation chamber 100 is connected to the inlet of the cracking chamber 200, and the pyrolysis is heated in the cracking chamber 200 to crack into a gaseous single molecule free radical state. The heating pyrolysis temperature is generally maintained at 500°C~850°C, preferably 650°C. The outlet of the pyrolysis chamber 200 is connected to the inlet of the deposition chamber 300, and the pyrolysis p-xylene vapor enters the deposition chamber 300. The deposition temperature of the deposition chamber 300 is generally maintained at 20°C~35°C, preferably 30°C.

[0057] In some embodiments, see Figure 4 , the following steps are also included between step S200 and step S300:

[0058] S201, placing C-type p-xylene raw material in the parylene coating device, sealing and evacuating the device.

[0059] Specifically, the C-type paraxylene raw material is fed into the feed port of the parylene coating device, and the entire device is sealed and vacuumed.

[0060] S202, when the vacuum degree of the deposition chamber reaches 6-12 mTorr, the C-type paraxylene raw material is heated and gasified to form paraxylene vapor.

[0061] S203, the p-xylene vapor is cracked to form monomer toluene vapor, and is transported into the deposition chamber through a pipeline to achieve a parylene protective layer deposition process.

[0062] Next, the specific deposition process of the parylene protective layer is described through step S300 and step S400.

[0063] S300, depositing a first film layer in the internal channel of the micro-array intracavity device using a first deposition rate; the first deposition rate is 0.1 μm / h-0.5 μm / h, and the thickness of the first film layer is 2 μm-5 μm.

[0064] Specifically, the first film layer is a seed layer. A relatively low deposition rate corresponds to a relatively low gas pressure. The free path of the monomer molecules is relatively large, and they have a larger free diffusion distance. They will diffuse through the narrow gaps between the grains to the interior to be deposited into a film. The film formation is relatively uniform, and this thinner first film layer will become the seed layer for the later deposition of the second film layer, which is beneficial to the deposition of subsequent film layers.

[0065] S400, continuously depositing a second film layer on the surface of the first film layer at a second deposition rate; the second deposition rate is 0.6 μm / h to 1.5 μm / h, the thickness of the second film layer is 10 μm to 20 μm, and the thickness ratio of the first film layer to the second film layer is 1:3 to 1:10.

[0066] Specifically, due to the presence of the seed layer, a non-differentiated substrate is formed on the surface of the internal channel of the microarray cavity device, so that the second film layer grown subsequently will be more uniform. This step increases the deposition rate in order to take into account both deposition efficiency and process cost. The specific principle of improving uniformity by growing two film layers at different rates is as follows: Since the microarray cavity device itself is produced by a composite of multiple materials, the thermal conductivity of different materials is different, and the deposited protective film layer is easier to grow on materials with high thermal conductivity. In addition, there will be some randomly distributed protrusions on the surface of the substrate inside the device. These protrusions will provide a core for the growth of the film, so that the film will grow preferentially on the protrusions. In this case, when the deposition rate is fast, these preferential growth situations will become more serious, and the film will lose its chain growth and aggregate into particles. Therefore, the embodiment of the present invention can make the substrate consistent by growing a thin first film layer at a low rate in advance, so that when the second film layer is grown at a high rate, the possibility of preferential growth in a certain area is reduced, which is beneficial to improving the uniformity of the film layer. Among them, the first deposition rate T1 and the second deposition rate T2 are as follows Figure 3 As shown, the first deposition rate T1 and the second deposition rate T2 can be adjusted by controlling the gas pressure of the deposition chamber 300 , and the thickness of the first film layer and the second film layer can be measured and monitored by an online thickness tester.

[0067] S500, removing the masking adhesive layer, thereby obtaining a micro-array cavity device with a parylene protective layer; wherein the parylene protective layer is composed of a first film layer and a second film layer.

[0068] Specifically, after the deposition of the parylene protective layer is completed, the masking glue layer needs to be removed to obtain a micro-array intracavity device with the parylene protective layer.

[0069] The protection method of the micro-array intracavity device provided in the present embodiment is beneficial to improving the safety and plating uniformity of the multi-channel semiconductor device by placing the multi-channel semiconductor device in the plating tool 320 for positioning and distribution, and at the same time, two different deposition rates are used to deposit the first film layer and the second film layer in sequence, that is, a lower deposition rate is first used to form a seed layer, which is beneficial to improving the uniformity of film formation in the grain gaps in the micro-array intracavity device, and can improve the deposition efficiency of the film layer, while reducing the cost of process preparation.

[0070] Optionally, in step S300, a first film layer is deposited in an internal channel of the micro-array intracavity device using a first deposition rate, comprising:

[0071] The temperature of the evaporation chamber of the parylene coating device is 120℃~140℃, and the gas pressure of the deposition chamber is 10 mTorr~15mTorr.

[0072] Specifically, by adjusting the temperature of the gasification, the deposition pressure is adjusted, and the deposition rate is controlled. It is understandable that the main factor in the plating process is the gas pressure, which can reflect the concentration of the p-xylene vapor, that is, the greater the gas pressure, the higher the concentration of the p-xylene vapor, and the lower the gas pressure, the lower the concentration of the p-xylene vapor. The polymerization reaction presents more chain reactions, and the deposition rate is low at this time, and the thickness of the film layer is more uniform.

[0073] Optionally, in step S400, the second film layer is continuously deposited on the surface of the first film layer using a second deposition rate, including:

[0074] The temperature of the evaporation chamber of the parylene coating device is 130℃~160℃, and the gas pressure of the deposition chamber is 15 mTorr~20mTorr.

[0075] Specifically, when depositing at a larger gas pressure, the higher the concentration of toluene vapor, the more branched chains will grow. At this time, the deposition rate is high, and the thickness uniformity will be affected to a certain extent. However, since the first film layer forms a seed layer, a non-differentiated base is formed on the surface to be deposited, which improves the uniformity of the second film layer. Therefore, even if the deposition rate of the second film layer increases, it will not reduce the uniformity of the entire parylene protective layer. In addition, the increase in the deposition rate is conducive to improving the overall deposition efficiency of the parylene protective layer, further reducing the process cost.

[0076] In some embodiments, see Figure 5 In step S100, a shielding adhesive layer is formed in an area of ​​the micro-array cavity device where a parylene protective layer is not required, including:

[0077] S110, forming a rectangular glue frame by connecting the ends in a staggered manner, and making the outer edge of the rectangular glue frame just flush with the outer edge of the micro-array inner cavity device;

[0078] S120, use the same glue in the rectangular glue frame and fill it in a bow shape to form a masking glue layer.

[0079] The glue in this embodiment is UV light curing glue, i.e. UV glue of acrylic resin system, the main components of which are acrylic resin and a small amount of acrylic resin modified substance, and some photoinitiators, stabilizers, etc. In addition to protecting the micro semiconductor device, the masking glue layer can also fix the micro array cavity device substrate by utilizing the viscosity of the masking glue.

[0080] In some embodiments, see Figure 6 In step S200, the micro-array cavity device prepared with the shielding adhesive layer is placed on a plating tool in a deposition chamber of a parylene plating device, including:

[0081] S210, placing a plurality of micro-array cavity devices prepared with masking adhesive layers on the positioning marks preset on the plating tool in sequence.

[0082] Specifically, since the size of the micro-array cavity device is small, in order to improve the plating efficiency of the parylene protective layer, the protective layer can be plated on multiple micro-array cavity devices at one time. Therefore, the embodiment of the present invention designs a plating tool, and pre-sets multiple positioning marks on the plating tool, and a micro-array cavity device prepared with a shielding adhesive layer is placed on each positioning mark.

[0083] S220, placing the entire plating tool near the edge of the turntable of the deposition chamber.

[0084] Specifically, after all the micro-array intracavity devices are placed on the plating tool 320, the entire plating tool 320 is fixed to the turntable 310 of the deposition chamber 300. In the case of the same rotation, the plating tool 320 located at the edge of the turntable 310 travels a longer path in one rotation, thereby ensuring that the micro-array intracavity devices are in more complete contact with the reaction gas, which is beneficial to improving the uniformity of the plating film layer.

[0085] Optionally, before step S210, the method further includes:

[0086] A plating tool 320 is provided; a plurality of evenly arranged positioning marks are set on the plating tool 320.

[0087] Specifically, the positioning marks on the plating device are evenly distributed, for example, arranged in concentric circular arrays, the diameters of the multiple circular arrays gradually increase, and the spacing between adjacent positioning marks in the same circular array is equal.

[0088] Optionally, see Figure 7In step S500, the masking glue layer is removed to obtain a micro-array cavity device with a parylene protective layer, including:

[0089] S510, after the deposition process of the parylene protective layer is completed, a laser is used to disconnect the area where the shielding adhesive layer is connected to the micro-array inner cavity device; wherein the laser pulse width is 10-100ps and the wavelength is 355nm.

[0090] Optionally, see Figure 8 In step S510, the area where the shielding glue layer is connected to the micro-array cavity device is disconnected by laser, including:

[0091] S511, placing the micro-array cavity device that has completed the parylene protective layer deposition process sideways into the jig so that the side that needs to be cut is exposed;

[0092] S512, cutting along the boundary of the masking adhesive layer using preset laser parameters;

[0093] S513, removing the masking adhesive layer.

[0094] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0095] Example 1

[0096] In order to better understand the present invention, the micro-array cavity device in the embodiment of the present invention is specifically described by taking a semiconductor cooling sheet as an example. Fig. 9 and Fig.10 As shown, the semiconductor cooling sheet 400 generally has a three-layer structure, the cold substrate 410 (heat absorbing surface) is used to contact the object to be cooled, the hot substrate 420 (heat releasing surface) is used to release heat, and a semiconductor grain array is embedded between the cold substrate 410 and the hot substrate 420, half of the grains are P-type semiconductors, and half of the grains are N-type semiconductors. A pair of grains form a PN junction, and the PN junction is electrically connected through the conductive layer 430. According to the Peltier effect, when current passes through the PN junction, heat absorption or heat release will occur, thereby forming condensed water. Therefore, through the protection method of the parylene protective layer provided by the embodiment of the present invention, the semiconductor cooling sheet is placed on the positioning mark corresponding to the plating tooling to ensure the spacing between each semiconductor cooling sheet, and two different deposition rates are used to deposit the parylene protective film layer 450 in the grain gap 440, which takes into account the problems of film uniformity and deposition efficiency, which is conducive to improving the stability of the micro-array intracavity device. The specific protection method of the semiconductor cooling sheet 400 includes the following steps:

[0097] S100, the shielding film layer is coated on the cold substrate, hot substrate and pads of the conductive layer (extension of the hot substrate, used to connect the wires) of the semiconductor cooling plate to prevent the Parylene film layer from being deposited in these areas and affecting the heat exchange performance of the semiconductor cooling plate.

[0098] S200, placing the semiconductor cooling sheet with the shielding adhesive layer on the plating tool 320 in the deposition chamber 300 of the parylene plating device.

[0099] S300, depositing a first film layer 451 in the internal channel of the semiconductor refrigeration plate using a first deposition rate; the first deposition rate is 0.2 μm / h; the temperature of the evaporation chamber 100 of the parylene plating device is 127° C., and the gas pressure of the deposition chamber 300 is 12 mTorr.

[0100] S400, the second film layer 452 is continuously deposited on the surface of the first film layer using a second deposition rate; the second deposition rate is 1 μm / h; the thickness of the first film layer 451 is 4 μm, the thickness of the second film layer 452 is 16 μm, and the thickness ratio of the first film layer 451 to the second film layer 452 is 1:4; the temperature of the evaporation chamber 100 of the parylene plating device is 145°C, and the gas pressure of the deposition chamber 300 is 16.5 mTorr.

[0101] S500 , removing the masking adhesive layer, thereby obtaining a semiconductor refrigeration sheet with a parylene protective layer; wherein the parylene protective film layer 450 is composed of a first film layer 451 and a second film layer 452 .

[0102] Example 2

[0103] The method of Example 1 is followed, except that the gas pressure in the deposition chamber 300 is adjusted by adjusting the temperature of the evaporation chamber 100, so that the first deposition rate in step S300 is 0.1 μm / h, the temperature of the evaporation chamber 100 of the parylene plating apparatus is 121° C., and the gas pressure in the deposition chamber 300 is 10.5 mTorr.

[0104] Example 3

[0105] The method of Example 1 is followed, except that the gas pressure in the deposition chamber 300 is adjusted by adjusting the temperature of the evaporation chamber 100, so that the first deposition rate in step S300 is 0.4 μm / h, the temperature of the evaporation chamber of the parylene plating device is 138°C, and the gas pressure in the deposition chamber 300 is 14 mTorr.

[0106] Example 4

[0107] The method of Example 1 is followed, except that the gas pressure in the deposition chamber 300 is adjusted by adjusting the temperature of the evaporation chamber 100, so that the second deposition rate in step S400 is 0.6 μm / h, the temperature of the evaporation chamber 100 of the parylene plating device in step S400 is 141°C, and the gas pressure in the deposition chamber 300 is 15.4 mTorr.

[0108] Example 5

[0109] The method of Example 1 is followed, except that the gas pressure in the deposition chamber 300 is adjusted by adjusting the temperature of the evaporation chamber, so that the second deposition rate in step S400 is 1.4 μm / h, the temperature of the evaporation chamber 100 of the parylene plating apparatus is 155° C., and the gas pressure in the deposition chamber 300 is 19 mTorr.

[0110] Example 6

[0111] The method of Example 1 is referred to, except that the deposition time of the deposition chamber 300 is adjusted so that the thickness of the first film layer is 5 μm, and the thickness ratio of the first film layer to the second film layer is 1:3.

[0112] Example 7

[0113] The method of Example 1 is referred to, except that the deposition time of the deposition chamber 300 is adjusted so that the thickness of the first film layer is 2 μm, and the thickness ratio of the first film layer to the second film layer is 1:9.

[0114] Example 8

[0115] The method of Example 1 is referred to, except that the deposition time of the deposition chamber 300 is adjusted so that the thickness of the second film layer is 17 μm, and the thickness ratio of the first film layer to the second film layer is 1:6.

[0116] Comparative Example 1

[0117] The method of Example 1 is referred to, except that in step S300, the first deposition rate is 0.7 μm / h.

[0118] Comparative Example 2

[0119] The method of Example 1 is referred to, except that in step S400, the second deposition rate is 0.4 μm / h.

[0120] Comparative Example 3

[0121] The method of Example 1 is referred to, except that the thickness of the first film layer is 8 μm, and the thickness ratio of the first film layer to the second film layer is 1:1.5.

[0122] Comparative Example 4

[0123] The method of Example 1 is referred to, except that the thickness of the second film layer is 8 μm, and the thickness ratio of the first film layer to the second film layer is 1:0.6.

[0124] Test Case

[0125] The parylene protective layers obtained in the above examples and comparative examples were sliced ​​and tested, and the variance results of the slice thickness are shown in Table 1.

[0126] Table 1 Average and variance of the thickness of the parylene film layer in different embodiments

[0127]

[0128] It can be seen from the above results that, compared with the comparative example, the solution of the embodiment of the present invention can better improve the uniformity of the parylene protective layer, which is beneficial to protect the grains in the micro-array cavity device. Further, according to Example 1 and Examples 2-8, it can be seen that the solution of the preferred embodiment 1 of the present invention is beneficial to improve the thickness uniformity of the parylene protective layer, and is more conducive to isolating and protecting water vapor, thereby improving the stability of the micro-array cavity device. It should be noted that in comparative example 2, the second deposition rate in step S400 is only 0.4 μm / h. To achieve the same film thickness, the deposition time is greatly increased. If the deposition time is too long, the deposition material will change and the uniformity of the deposited film will be reduced (such as: for xylene containing Cl (C-type parylene) or F (F-type parylene), the corresponding functional groups will be released during the reaction in the vacuum chamber, C-type will release HCl, and F-type will release HF. Moreover, the longer the deposition time, the more this reaction will occur, and the more HCl (hydrochloric acid) or HF (hydrofluoric acid) will be released. The benzene rings after dehydrogenation and dechlorination are mixed with the benzene rings without defunctionalization. When the film is deposited, the chemical reaction will be uneven, thereby reducing the uniformity of the deposited film); in addition, if the second deposition rate is too low and the process time is long, the process conditions such as pressure and temperature are also prone to fluctuations over a long period of time, and the accumulation of fluctuations will also reduce the uniformity of the deposited film. For Example 2, the first deposition rate of step S300 is 0.1 μm / h, so it also takes 40 hours to reach the first film layer thickness of 4 μm. However, when depositing the first film layer, the overall thickness of the film layer is thinner, and the overall uniformity will be better. In addition, in the initial stage of deposition, the deposited material releases less HCl (hydrochloric acid) or HF (hydrofluoric acid), which has less effect on the uniformity of the film layer. Therefore, the film uniformity of the thinner first film layer deposited in the same deposition time will be better than the film uniformity of the thicker second film layer.

[0129] In the description of the present invention, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0130] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0131] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific conditions. In the description of this specification, specific features, structures, materials or characteristics can be combined in a suitable manner in any one or more embodiments or examples.

[0132] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for protecting a microarray cavity device, It is characterized in that The following steps are involved: S100, forming a shielding adhesive layer in the area of ​​the micro-array inner cavity device where the parylene protective layer is not required; S200, placing the micro-array inner cavity device prepared with the masking adhesive layer on a plating tool in a deposition chamber of a parylene plating device; S300, depositing a first film layer in the internal channel of the micro-array intracavity device at a first deposition rate; the first deposition rate is 0.1 μm / h to 0.5 μm / h, and the thickness of the first film layer is 2 μm to 5 μm; S400, continuously depositing a second film layer on the surface of the first film layer at a second deposition rate; the second deposition rate is 0.6 μm / h to 1.5 μm / h, the thickness of the second film layer is 10 μm to 20 μm, and the thickness ratio of the first film layer to the second film layer is 1:3 to 1:10; S500, removing the masking adhesive layer, thereby obtaining the micro-array intracavity device with a parylene protective layer; wherein the parylene protective layer is composed of a first film layer and a second film layer.

2. The protection method for the microarray cavity device according to claim 1, It is characterized in that In step S300, the step of depositing a first film layer in the internal channel of the microarray cavity device using a first deposition rate includes: The temperature of the evaporation chamber of the parylene plating device is 120° C. to 140° C., and the gas pressure of the deposition chamber is 10 mTorr to 15 mTorr.

3. The protection method for the microarray cavity device according to claim 1, It is characterized in that In step S400, the step of continuously depositing a second film layer on the surface of the first film layer at a second deposition rate includes: The temperature of the evaporation chamber of the parylene plating device is 130° C. to 160° C., and the gas pressure of the deposition chamber is 15 mTorr to 20 mTorr.

4. The protection method for the microarray cavity device according to claim 1, It is characterized in that Also included between step S200 and step S300: S201, placing a C-type p-xylene raw material in a parylene coating device, sealing and evacuating the device; S202, when the vacuum degree of the deposition chamber reaches 6mTorr~12mTorr, the raw material is heated and gasified to form paraxylene vapor; S203, the p-xylene vapor is cracked to form monomer toluene vapor, and is transported into the deposition chamber through a pipeline to achieve a parylene protective layer deposition process.

5. The protection method for the microarray intracavity device according to claim 1, It is characterized in that In step S100, a shielding adhesive layer is formed in an area of ​​the micro-array cavity device where a parylene protective layer is not required, including: S110, forming a rectangular glue frame by connecting the ends in a staggered manner, and making the outer edge of the rectangular glue frame just flush with the outer edge of the micro-array inner cavity device; S120, using the same glue in the rectangular glue frame to fill it in a bow shape to form the masking glue layer.

6. The method for protecting a microarray cavity device according to claim 1, It is characterized in that In step S200, the micro-array cavity device prepared with the shielding adhesive layer is placed on a plating tool in a deposition chamber of a parylene plating device, including: S210, placing a plurality of the micro-array inner cavity devices prepared with a masking adhesive layer on the positioning marks preset on the plating tool in sequence; S220, placing the entire plating tool at a position close to the edge of the turntable of the deposition chamber.

7. The protection method for the microarray cavity device according to claim 6, It is characterized in that Before step S210, the method further includes: A plating tool is provided; the plating tool is provided with a plurality of positioning marks which are evenly arranged.

8. The method for protecting a microarray cavity device according to claim 1, It is characterized in that In step S500, the masking glue layer is removed to obtain the micro-array cavity device with the parylene protective layer, including: S510, after the deposition process of the parylene protective layer is completed, a laser is used to disconnect the area where the shielding adhesive layer is connected to the micro-array intracavity device; wherein the laser pulse width is 10 ps to 100 ps, ​​and the wavelength is 355 nm.

9. The protection method for the microarray cavity device according to claim 8, It is characterized in that In step S510, the step of using a laser to disconnect the region where the shielding adhesive layer is connected to the micro-array intracavity device includes: S511, placing the micro-array cavity device after the parylene protective layer deposition process into a jig sideways so that the side to be cut is exposed; S512, cutting along the boundary of the masking adhesive layer using preset laser parameters; S513, removing the masking adhesive layer.

10. A micro-array cavity device with a parylene protective layer, It is characterized in that Obtained by the protection method according to any one of claims 1 to 9.