A method for preparing a multi-element catalyst and its application

By preparing a multi-element catalyst, the problem of mercury loss in mercuric chloride catalyst during calcium carbide PVC production was solved, the catalyst activity and selectivity were improved, high-efficiency catalysis under low concentration conditions was achieved, the industry's mercury consumption requirements were met, and PVC production efficiency and product quality were improved.

CN118454741BActive Publication Date: 2026-11-17GUIZHOU UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410506232.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2026-11-17
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

In existing calcium carbide-based PVC production, the use of mercuric chloride catalysts leads to severe mercury loss and serious environmental pollution, and it is difficult to meet the industry requirements for mercury consumption per unit of product. The catalyst also has poor catalytic effect under low concentration conditions.

Method used

A multi-component catalyst preparation method was adopted, in which activated carbon was treated by impregnation with Co(NO3)2, Ni(NO3)2 and 2-methylimidazole to form a dimethylimidazole nickel cobalt metal organic film. Combined with a solution of mercuric chloride, zinc, manganese, copper and cadmium, a multi-component catalyst with high adsorption selectivity and catalytic activity was prepared, which is suitable for background converters.

Benefits of technology

It improves the activity and selectivity of the catalyst, reduces the mercury content, extends the service life, increases the yield and purity of PVC, meets the catalytic requirements under low-concentration raw material conditions, and reduces the mercury consumption per ton of PVC to 35g/T-PVC.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a method for preparing a multi-component catalyst and its application, comprising the following steps: S1, weighing one part each of Co(NO3)2, Ni(NO3)2, and 2-methylimidazole, dissolving and mixing them separately in methanol solution to obtain a mixed solution; S2, soaking activated carbon in the mixed solution at 60-90℃, and then naturally drying to obtain metal-modified activated carbon; S3, dissolving mercuric chloride, zinc chloride, manganese chloride, copper chloride, and cadmium chloride in water to prepare an adjusting solution; S4, soaking the metal-modified activated carbon in the adjusting solution obtained in step S3, and then drying to obtain the multi-component catalyst. This multi-component catalyst is suitable for use in a background converter for the synthesis of vinyl chloride. The multi-component catalyst prepared using this invention exhibits good catalytic conversion effect, strong adsorption selectivity, and long service life, overcoming the shortcomings of existing products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a multi-element catalyst and its application, belonging to the field of chemical engineering. Background Technology

[0002] The calcium carbide-based PVC production industry generates tens of thousands of tons of mercury-containing waste annually, including waste mercury catalysts, placing immense pressure on the environment. Mercury emission reduction and pollution control in the PVC industry have become pressing issues hindering the development of the calcium carbide-based PVC industry.

[0003] The synthesis of vinyl chloride via the calcium carbide process is an exothermic reaction using mercuric chloride as a catalyst, employing a series reaction process with a front-end converter and a back-end converter. In the front-end converter, a mixed gas containing 50.5% hydrogen chloride and 49.5% acetylene is introduced for reaction; the high reactant concentrations result in a vigorous catalytic synthesis reaction at a high temperature. In the back-end converter, the reactants are the mixed gas from the front-end reaction, where the concentrations of both hydrogen chloride and acetylene are lower than 25%, while the concentration of the product vinyl chloride is higher. This results in a relatively mild catalytic synthesis reaction at a lower temperature.

[0004] Mercuric chloride, also known as "mercuric chloride," sublimates and leaks at high temperatures, leading to catalyst deactivation. Current processes use mercuric chloride catalysts containing 4-6.5% mercuric chloride, resulting in significant mercury loss and mercury consumption as high as 70-90 g / T of PVC. The mercuric chloride content of existing catalysts is 4-6.5%, which is too high and causes serious environmental pollution. Furthermore, the "Assessment Rules for the Completion of the Target of Halving Mercury Content in Calcium Carbide Method Polyvinyl Chloride (Trial)" requires that by the end of 2020, the mercury consumption per ton of PVC produced using the calcium carbide method should be set at 49.14 grams. The current mercuric chloride catalysts consume a large amount of mercury per ton. Meanwhile, the concentrations of acetylene and hydrogen chloride in the downstream converter are low, resulting in mercury consumption of 70-90 grams per ton of PVC using existing mercuric chloride catalysts, which does not meet industry requirements.

[0005] Different catalysts are developed for different converters. By strengthening the skeleton structure of the activated carbon support for the catalyst, the adsorption performance of the activated carbon support for mercuric chloride and other catalytic aids is improved. This is beneficial to improve the stability of mercury in the catalyst, improve the catalytic performance and service life of the catalyst, reduce the mercury content of the catalyst, reduce the amount of mercury consumed in the PVC production reaction, and reduce mercury pollution. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing a multi-element catalyst and its application, which is suitable for a background converter for the synthesis of vinyl chloride.

[0007] The technical solution of this invention:

[0008] The first objective of this invention is to provide a method for preparing a multi-element catalyst, comprising the following steps:

[0009] S1. Weigh out one part each of Co(NO3)2, Ni(NO3)2 and 2-methylimidazole, dissolve and mix them separately with methanol solution to obtain a mixed solution;

[0010] S2. At 60-90℃, take the mixed solution to soak activated carbon, and then dry it naturally to obtain metal-modified activated carbon;

[0011] S3. Dissolve mercuric chloride, zinc chloride, manganese chloride, copper chloride, and cadmium chloride in water to prepare an adjusting solution;

[0012] S4. Take the adjustment solution obtained in step S3, soak the metal-modified activated carbon, and dry it to obtain a multi-element catalyst.

[0013] In step S1, the ratio of Co(NO3)2∶Ni(NO3)2∶2-methylimidazole in the mixture is 1:1:1 by weight.

[0014] In step S2, the metal-modified activated carbon contains 0.5% nickel and 0.5% cobalt by mass fraction, with the remainder being activated carbon.

[0015] In step S3, the mercury:zinc:manganese:copper:cadmium ratio in the adjustment solution is (0.5-1):(2-6):(2-6):(1-5):(1-5) by weight.

[0016] A second objective of this invention is to provide the application of the multi-element catalyst prepared by the above-described preparation method in the catalytic synthesis of PVC.

[0017] Specifically, the application of the multi-element catalyst prepared by the above preparation method in the background converter of calcium carbide PVC synthesis.

[0018] More specifically, the application of the multi-element catalyst prepared by the above method in the synthesis of PVC from low-concentration raw materials. The low-concentration raw materials are hydrogen chloride and acetylene, both with a volume concentration ≤25%.

[0019] Beneficial effects:

[0020] The method of this invention is simple and easy to implement, requires few control conditions, and the resulting multi-element catalyst has the characteristics of good catalytic conversion effect, strong adsorption selectivity and long service life. It is suitable for the background converter of calcium carbide PVC synthesis and can improve PVC yield and purity under low concentration raw material conditions.

[0021] This invention involves impregnating an activated carbon support with Co(NO3)2 and Ni(NO3)2 and 2-methylimidazole, which forms a dimethylimidazole nickel-cobalt metal-organic film on the pore surface of the activated carbon support. The nickel-cobalt complex has a periodically arranged metal-nitrogen coordination structure, offering advantages such as high specific surface area and tunable porosity, thus improving the catalytic performance and adsorption selectivity of the activated carbon. Because this activated carbon support exhibits high adsorption selectivity and large adsorption capacity for mercury and multi-metal catalytic promoters, it significantly enhances the strength of the activated carbon's pore framework. Furthermore, the dimethylimidazole cobalt-nickel film possesses a certain catalytic effect, which can significantly reduce the mercuric chloride content in the catalyst; that is, the catalyst of this invention has a low mercury content.

[0022] The catalyst of this invention is suitable for use in a back-end converter. Because the gas concentration in the back-end converter is relatively low, i.e. the converter temperature is low, the catalytic conversion rate of the mixed gas will be low. However, the catalyst of this invention has excellent catalytic effect and can improve the yield and purity of the product. For example, the reaction between acetylene and hydrogen chloride in the front-end converter is an exothermic reaction, which will lead to a decrease in the selectivity of the catalyst, thereby resulting in a large amount of by-products.

[0023] During the applicant's research, it was discovered that single impregnation can lead to an excessive amount of loading on the support due to intermolecular forces, meaning that the catalytically active components are dispersed on the support in the form of clusters. However, by using a conditioning solution for secondary impregnation, the prepared catalyst has the technical advantages of small particle size, high dispersion, and high catalytic conversion rate of the catalytically active components.

[0024] To further demonstrate the catalytic effect of the catalyst prepared in this invention, the inventors prepared a batch of 15 tons of multi-element catalyst and tested it on the No. 2 converter (backstage) of Hubei Yihua Chemical Co., Ltd. After sampling and gas chromatography analysis, the inlet acetylene concentration was 22%, the hydrogen chloride concentration was 24%, and the outlet hydrogen chloride volume fraction was 14% and the acetylene volume fraction was 12% (Table 1, Example 1); tests were conducted on the No. 4 converter (backstage) (Table 1, Example 2); and tests were conducted on the No. 8 converter (backstage) (Table 1, Example 3). The results show that when the multi-element catalyst prepared by this invention synthesizes vinyl chloride, the reaction temperature is 115-140℃, the yield is 95-98%, the vinyl chloride purity is 96.7-97.2%, and the selectivity for vinyl chloride reaches 96-100%. The purity of the crude vinyl chloride product after distillation reaches 99.99% (V / %), which meets the production requirements of vinyl chloride. The service life is greater than 13,000 hours. The mercury consumption per ton of PVC is 35g / T-PVC.

[0025] Table 1. Detection results of vinyl chloride synthesis test

[0026]

[0027] The inventors used the catalyst of this invention in a front-end converter at a reaction temperature of approximately 200°C. The inlet hydrogen chloride volume fraction was 50.5%, the acetylene volume fraction was 49.5%, and the byproduct dichloroethane accounted for 10% of the product, leading to a higher than normal temperature. Since the catalyst exhibits selectivity for the chemical reaction, a large amount of pale yellow liquid dichloroethane flowed out from the lower end of the front-end converter, affecting the entire catalytic reaction system. Therefore, the catalyst of this invention is not suitable for front-end converters. Detailed Implementation

[0028] The present invention will be further described below with reference to embodiments, but these should not be construed as limiting the invention. Structures or processes not specifically described are conventional prior art in the field.

[0029] A method for preparing a multi-element catalyst includes the following steps:

[0030] S1. Weigh out one part each of Co(NO3)2, Ni(NO3)2 and 2-methylimidazole, dissolve and mix them separately with methanol solution to obtain a mixed solution;

[0031] S2. At 60-90℃, take the mixed solution to soak activated carbon, and then dry it naturally to obtain metal-modified activated carbon;

[0032] S3. Dissolve mercuric chloride, zinc chloride, manganese chloride, copper chloride, and cadmium chloride in water to prepare an adjusting solution;

[0033] S4. Take the adjustment solution obtained in step S3, soak the metal-modified activated carbon, and dry it to obtain a multi-element catalyst.

[0034] In step S1, the ratio of Co(NO3)2∶Ni(NO3)2∶2-methylimidazole in the mixture is 1:1:1 by weight.

[0035] Immersing activated carbon supports in a solution containing Co(NO3)2 and Ni(NO3)2 can form a dimethylimidazolium nickel cobalt metal-organic film on the pore surface of the support, thereby improving the catalytic performance, adsorption selectivity and strength of the activated carbon.

[0036] In step S2, the metal-modified activated carbon contains 0.5% nickel and 0.5% cobalt by mass fraction, with the remainder being activated carbon.

[0037] In step S3, the mercury:zinc:manganese:copper:cadmium ratio in the adjustment solution is (0.5-1):(2-6):(2-6):(1-5):(1-5) by weight.

[0038] Activated carbon with a dimethylimidazolium nickel cobalt metal organic film on its surface is immersed in a solution containing mercury, zinc, manganese, copper and cadmium, which has the effect of anchoring catalytic active components and the advantage of mercury fixation.

[0039] This invention strictly controls the mass content of cobalt and nickel. If the cobalt and nickel content is too low, the synergistic catalytic effect cannot be fully exerted, resulting in a low catalytic conversion rate. If the cobalt and nickel content is too high, the dimethylimidazolium nickel cobalt metal-organic film will occupy a large amount of the pore structure of the activated carbon support, resulting in low dispersion of mercury, zinc, manganese, copper, and cadmium. Through long-term research by the applicant, it has been found that the synergistic effect is maximized when the content of mercury, zinc, manganese, copper, and cadmium is (0.5-1):(2-6):(2-6):(1-5):(1-5).

[0040] The following examples are provided in conjunction with specific circumstances.

[0041] Example 1

[0042] A method for preparing a multi-element catalyst includes the following steps:

[0043] S1. Weigh out one part each of Co(NO3)2, Ni(NO3)2 and 2-methylimidazole, dissolve them separately in methanol solution, and mix them to obtain a mixture; the mixture contains Co(NO3)2, Ni(NO3)2 and 2-methylimidazole in equal weight ratio;

[0044] S2. At 60℃, take the mixed solution to soak activated carbon, and after natural drying, obtain metal-modified activated carbon;

[0045] S3. According to the weight ratio of mercury:zinc:manganese:copper:cadmium = 1∶2∶2∶5∶5, mix mercuric chloride, zinc chloride, manganese chloride, copper chloride and cadmium chloride to prepare an adjusting solution;

[0046] S4. Take the adjustment solution from step S3, soak the metal-modified activated carbon, and dry it to obtain a multi-element catalyst. The mass contents of mercury, zinc, manganese, copper, cadmium, nickel and cobalt in the multi-element catalyst are 1%, 2%, 2%, 5%, 5%, 0.5% and 0.5% respectively, with the remainder being activated carbon.

[0047] Example 2

[0048] A method for preparing a multi-element catalyst includes the following steps:

[0049] S1. Weigh out one part each of Co(NO3)2, Ni(NO3)2 and 2-methylimidazole, dissolve them separately in methanol solution, and mix them to obtain a mixture; the mixture contains Co(NO3)2, Ni(NO3)2 and 2-methylimidazole in equal weight ratio;

[0050] S2. At 60℃, take the mixed solution to soak activated carbon, and after natural drying, obtain metal-modified activated carbon;

[0051] S3. According to the weight ratio of mercury:zinc:manganese:copper:cadmium = 1∶6∶6∶1∶1, mix mercuric chloride, zinc chloride, manganese chloride, copper chloride and cadmium chloride to prepare an adjusting solution;

[0052] S4. Take the adjustment solution from step S3, soak the metal-modified activated carbon, and dry it to obtain a multi-element catalyst. The mass contents of mercury, zinc, manganese, copper, cadmium, nickel and cobalt in the multi-element catalyst are 1%, 6%, 6%, 1%, 1%, 0.5% and 0.5% respectively, with the remainder being activated carbon.

[0053] Example 3

[0054] A method for preparing a multi-element catalyst includes the following steps:

[0055] S1. Weigh out one part each of Co(NO3)2, Ni(NO3)2 and 2-methylimidazole, dissolve them separately in methanol solution, and mix them to obtain a mixture; the mixture contains Co(NO3)2, Ni(NO3)2 and 2-methylimidazole in equal weight ratio;

[0056] S2. At 60℃, take the mixed solution to soak activated carbon, and after natural drying, obtain metal-modified activated carbon;

[0057] S3. According to the weight ratio of mercury:zinc:manganese:copper:cadmium = 1∶3∶3∶3∶3, mix mercuric chloride, zinc chloride, manganese chloride, copper chloride, and cadmium chloride to prepare an adjusting solution;

[0058] S4. Take the adjustment solution from step S3, soak the metal-modified activated carbon, and dry it to obtain a multi-element catalyst. The mass contents of mercury, zinc, manganese, copper, cadmium, nickel and cobalt in the multi-element catalyst are 1%, 3%, 3%, 3%, 3%, 0.5% and 0.5% respectively, with the remainder being activated carbon.

Claims

1. A method for preparing a multi-element catalyst, characterized in that, Includes the following steps: S1. Weigh out one part each of Co(NO3)2, Ni(NO3)2 and 2-methylimidazole, dissolve and mix them separately with methanol solution to obtain a mixed solution; S2. At 60-90℃, take the mixed solution to soak activated carbon, and then dry it naturally to obtain metal-modified activated carbon; S3. Dissolve mercuric chloride, zinc chloride, manganese chloride, copper chloride, and cadmium chloride in water to prepare an adjusting solution; S4. Take the adjustment solution obtained in step S3, soak the metal-modified activated carbon, and dry it to obtain a multi-element catalyst. In step S1, the ratio of Co(NO3)2∶Ni(NO3)2∶2-methylimidazole in the mixture is 1:1:1 by weight. In step S2, the metal-modified activated carbon contains 0.5% nickel and 0.5% cobalt by mass fraction, with the remainder being activated carbon. In step S3, the mercury:zinc:manganese:copper:cadmium content in the conditioning solution is (0.5-1):(2-6):(2-6):(1-5):(1-5) by weight.

2. The application of the multi-element catalyst prepared by the method described in claim 1 in the catalytic synthesis of PVC.

3. The application of the multi-element catalyst prepared by the method described in claim 1 in the background converter of calcium carbide PVC synthesis.

4. The application of the multi-element catalyst prepared by the method described in claim 1 in the synthesis of PVC from low-concentration raw materials.

5. The application as described in claim 4, characterized in that, The low-concentration raw materials are hydrogen chloride and acetylene, both with a volume concentration ≤25%.

Citation Information

Patent Citations

  • High-stability composite mercury catalyst for hydrochlorination of acetylene

    CN102085485A

  • Catalyst of vinyl chloride prepared through acetylene hydrochlorination and preparation method therefor

    CN105268478A

  • Copper-based mercury-free catalyst for producing vinyl chloride by calcium carbide method and preparation and use method thereof