A method for forging a plate
By installing auxiliary baffles on existing rolling equipment and adopting symmetrical drawing and thinning technology, the forging of 5000mm*5000mm*20mm thick aluminum alloy plates was achieved, which solved the problem of difficulty in forming wide-width plates in the existing technology and ensured The precise forming and performance of the board meet the requirements.
Patent Information
- Application Number
- CN202410939844.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The existing technology is difficult to form 5000mm*5000mm*20mm thick aluminum alloy plates. Especially in the forging method, when the width is greater than 4000mm and the thickness is less than 70mm, it is difficult to achieve redirection shaping and forming of the required shape and size.
Using the existing rolling equipment combined with the forging method of symmetrical drawing and thinning, by installing an auxiliary baffle on the periphery of the forging tooling, the plate is stretched toward the edge at half the width, and the thickness of the plate is gradually reduced to the required thickness. Existing equipment enables precise forming of ultra-wide sheets.
There is no need to develop ultra-wide rolling equipment, and only simple auxiliary baffles are needed to achieve precise forming of ultra-wide thin plates, solving the problem of difficulty in forming plates of this specification with the existing forging process, and ensuring the size and performance of the plates. Meet the needs.
Smart Images

Figure CN118455434B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy plate forging, and in particular to a plate forging method. Background Art
[0002] As aerospace equipment represented by rockets develops towards large-scale, integrated and high-performance directions, there is an urgent need for super-large components. Taking the existing Φ3350mm-class rocket tank as an example, there are three main methods for preparing the tank top cover (diameter 3350mm, thickness 20mm), a key structural component: Method 1 is to use 2219 and 2195 plates to first form an arc-shaped melon slice, and then weld it into a top cover; Method 2 is to use 4000mm wide plates and spin them into a top cover as a whole; Method 3 is to use 2500mm wide plates, weld them into 5000mm wide plates, and then flush them into a top cover. Method 1 adopts a welded structure, which requires overall thickening and reinforcement, limiting the further lightweighting of the rocket body; Option 2 adopts an overall forming method, but for large thin-walled parts, this method is prone to wrinkles and instability, and the process control is difficult and the process flow is complicated; Option 3 adopts a liquid filling forming method, which is currently the best solution for preparing large top covers, but it is necessary to solve the problem of overall preparation of 5000mm*5000mm*20mm thick aluminum alloy plates.
[0003] At present, the main methods for preparing plates are rolling and forging. The best manufacturing method for wide plates is rolling, but the current widest rolling mill in China has a width of 4500mm, which cannot form plates with a width greater than 4500mm. For conventional forging methods, when the plate width is greater than 4000mm and the thickness is less than 70mm, it is difficult to achieve redirection and shaping, and the required shape and size cannot be formed. Therefore, it is urgent to develop a forming method for aluminum alloy plates with a size of not less than 5000mm*5000mm*20mm based on existing equipment. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a forging method for a plate, which can utilize existing rolling equipment to achieve precise forming of ultra-wide thin plates.
[0005] The technical solution provided by the present invention is as follows:
[0006] A forging method for a plate comprises the following steps:
[0007] S1. Ingot heating: heating and keeping the ingot warm;
[0008] S2, blanking: using the existing conventional upsetting and drawing process to blank;
[0009] S3, return to the furnace for heating: return the slab to the heating furnace for heating and heat preservation;
[0010] S4. Install the auxiliary baffle: install the auxiliary baffle on the periphery of the lower flat anvil of the existing forging tooling;
[0011] S5, symmetrical thinning: along the half of the width of the plate ± 200mm, stretch to the edge, and then along the half of the adjacent side ± 200mm, stretch to the edge, until the plate is pressed down by 15-25% in one quarter of the quadrant; repeat the above steps in the other three quadrants until the overall thickness of the plate is pressed down by 15-25%;
[0012] S6. Repeat step S5 to forge the plate to a desired thickness.
[0013] Preferably, the size of the slab obtained after blanking in step S2 is 2500-3200*2500-3200 mm.
[0014] Preferably, in step S4, the height of the auxiliary baffle does not exceed 100 mm from the upper end surface of the lower anvil.
[0015] Preferably, in step S1, the ingot is heated to 420° C. to 510° C. and kept warm for 10 to 30 hours.
[0016] Preferably, the ingot in step S1 is an aluminum alloy ingot.
[0017] Preferably, in step S3, the slab is heated to 420° C. to 510° C. and kept warm for 5 to 15 hours.
[0018] Preferably, in step S5, a drawing anvil with a width of 200 to 400 mm and a length of not less than 1500 mm is used for the drawing operation, and each anvil is pressed down by 15 to 25% in the width direction until it reaches the edge of the plate.
[0019] Preferably, the width of the plate obtained after forging in step S6 is not less than 5000 mm.
[0020] The present invention has the following advantages over the prior art:
[0021] 1) Compared with the existing rolling process, the forging method of the plate of the present invention does not require the development of ultra-wide rolling equipment and can be carried out using existing equipment;
[0022] 2) Compared with the existing conventional forging process, the forging method of the plate of the present invention only needs to add a simple auxiliary baffle, combined with a symmetrical drawing and thinning solution, to achieve the precise forming of ultra-wide thin plates, solving the problem that the existing conventional process is difficult to achieve redirection shaping on plates of this specification and cannot form the required shape and size. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 It is a schematic diagram of the structure of the forging tool and the slab in the embodiment of the present invention;
[0025] Figure 2 It is a schematic diagram of the structure of the first drawing and thinning of the 1 / 4 quadrant of the plate in an embodiment of the present invention;
[0026] Figure 3 It is a schematic diagram of the structure of the first drawing and thinning of the entire plate in an embodiment of the present invention;
[0027] Figure 4 It is a schematic diagram of the structure of the final drawing and thinning of the 1 / 4 quadrant of the plate in an embodiment of the present invention;
[0028] Figure 5 Schematic diagram of the structure of the finished plate product in an embodiment of the present invention.
[0029] Reference numerals:
[0030] 1. Auxiliary baffle; 2. Lower flat anvil; 3. Slab. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0032] like Figure 1-5 As shown, an embodiment of the present invention provides a forging method for a plate, comprising the following steps:
[0033] S1. Ingot heating: heat the aluminum alloy ingot to 420°C to 510°C and keep it warm for 10 to 30 hours;
[0034] S2. Blanking: The conventional upsetting and drawing process is used for blanking. The size of the blank obtained after blanking is 2500-3200*2500-3200mm;
[0035] S3, return to the furnace for heating: return the slab 3 to the heating furnace and heat it to 420°C to 510°C, and keep it warm for 5 to 15 hours;
[0036] S4. Install the auxiliary baffle: install the auxiliary baffle 1 on the periphery of the lower flat anvil 2 of the existing forging tooling, and the height of the auxiliary baffle shall not exceed 100 mm from the upper end surface of the lower flat anvil;
[0037] S5, symmetrical thinning: along the half of the width of the plate ± 200mm, stretch to the edge, and then along the half of the adjacent side ± 200mm, stretch to the edge, until the plate is pressed down by 15-25% in one quarter of the quadrant; repeat the above steps in the other three quadrants until the overall thickness of the plate is pressed down by 15-25%;
[0038] S6. Repeat step S5 to forge the plate to a desired thickness. The width of the plate obtained after forging is not less than 5000 mm.
[0039] In this embodiment, in step S5, a flat anvil with a width of 200 to 400 mm and a length of not less than 1500 mm is used for the stretching operation. The flat anvil is used to press down 15 to 25% in the width direction of each anvil until it reaches the edge of the plate.
[0040] In this embodiment, the auxiliary baffle 1 can be split and installed on four sides. It is connected to the lower anvil 2 by bolts to ensure that there are more than three equidistant connection points on each side. Because the auxiliary baffle 1 is different from the traditional mold, it only serves to block the plate from being forged and is formed to the edge first to prevent irregular shapes. The force it bears is relatively small. Therefore, there is no problem of solid plate entering the gap.
[0041] Example 1
[0042] A forging method for a plate comprises the following steps:
[0043] S1. Use 2219 aluminum alloy, the ingot specification is Φ800*1800mm, heat the ingot to 470℃ and keep it warm for 16h;
[0044] S2. The conventional upsetting and drawing process is used to open the blank, and the size of the forging slab is 3000*3000*100mm;
[0045] S3, heating the slab to 470°C and keeping it warm for 8h;
[0046] S4. Install an auxiliary baffle on the lower anvil, the height of which is 80 mm higher than the upper end surface of the lower anvil;
[0047] S5. Pull the plate toward the edge at half of the plate width, and then pull it toward the edge at half of the adjacent edge until one quarter of the plate is pressed down by 20%; repeat the above steps in the other three quadrants until the overall thickness of the plate is pressed down by 20%;
[0048] S6. Repeat the above steps to forge the plate to 5000*5000*20mm.
[0049] Example 2
[0050] A forging method for a plate comprises the following steps:
[0051] S1. Use 2219 aluminum alloy, the ingot specification is Φ1360*1250mm, heat the ingot to 470℃ and keep it warm for 28h;
[0052] S2. The conventional upsetting and drawing process is used to open the blank, and the size of the forging slab is 3000*3000*210mm;
[0053] S3, heating the slab to 470°C and keeping it warm for 12 hours;
[0054] S4. Install an auxiliary baffle on the lower anvil, the height of which is 80 mm higher than the upper end surface of the lower anvil;
[0055] S5. Pull the plate toward the edge at half of the plate width, and then pull it toward the edge at half of the adjacent edge until one quarter of the plate is pressed down by 20%; repeat the above steps in the other three quadrants until the overall thickness of the plate is pressed down by 20%;
[0056] S6. Repeat the above steps to forge the plate to 5000*5000*50mm.
[0057] The finished products were observed to have no cracks in the plates obtained by forging in the above Examples 1 and 2, and the plate sizes met the requirements. The corresponding properties met the requirements after subsequent liquid filling forming and heat treatment, thereby achieving the preparation of ultra-wide aluminum alloy sheets.
[0058] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A forging method for a plate, characterized in that: The steps are as follows: S1. Ingot heating: heating and keeping the ingot warm; S2, blanking: using the existing conventional upsetting and drawing process to blank; S3, return to the furnace for heating: return the slab to the heating furnace for heating and heat preservation; S4. Install the auxiliary baffle: install the auxiliary baffle on the periphery of the lower flat anvil of the existing forging tooling; S5, symmetrical thinning: along the half of the width of the plate ± 200mm, stretch to the edge, and then along the half of the adjacent side ± 200mm, stretch to the edge, until the plate is pressed down by 15-25% in one quarter of the quadrant; repeat the above steps in the other three quadrants until the overall thickness of the plate is pressed down by 15-25%; S6. Repeat step S5 to forge the plate to a desired thickness. After forging, the width of the plate obtained is not less than 5000 mm and the thickness is less than 70 mm.
2. The forging method of a plate material according to claim 1, characterized in that: The size of the slab obtained after the blanking in the step S2 is 2500-3200*2500-3200mm.
3. The forging method of a plate material according to claim 1, characterized in that: In step S4, the height of the auxiliary baffle does not exceed 100 mm from the upper end surface of the lower flat anvil.
4. The forging method of a plate material according to claim 1, 2 or 3, characterized in that: In the step S1, the ingot is heated to 420° C. to 510° C. and kept warm for 10 to 30 hours.
5. The forging method of a plate material according to claim 1, 2 or 3, characterized in that: The ingot in step S1 is an aluminum alloy ingot.
6. The forging method of a plate material according to claim 1, 2 or 3, characterized in that: In step S3, the slab is heated to 420° C. to 510° C. and kept warm for 5 to 15 hours.
7. The forging method of a plate material according to claim 1, 2 or 3, characterized in that: In step S5, a flat anvil with a width of 200 to 400 mm and a length of not less than 1500 mm is used for the stretching operation. The flat anvil is used to press down 15 to 25% in the width direction of each anvil until it reaches the edge of the plate.