Epoxy resin / graphitized carbon fiber felt composite material and preparation method thereof
By using a three-dimensional layered structure of carbon fiber felt and graphitization process, the problem of low thermal conductivity of polymer-based thermal management materials is solved, high thermal conductivity at low filler content is achieved, and it is suitable for the field of electronic packaging.
Patent Information
- Application Number
- CN202410932514.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The thermal conductivity of existing polymer-based thermal management materials is low, which limits their application in the field of electronic packaging. Especially in high-power density electronic devices, how to improve thermal conductivity at low filler content is a key issue.
Carbon fiber felt with a three-dimensional layered structure is used as a thermally conductive filler. Epoxy resin/graphitized carbon fiber felt composite materials are prepared through graphitization, stacking, vacuum impregnation and hot pressing molding processes to build a layered structure and an in-plane orientation structure to improve thermal conductivity. .
At a loading of 8.5wt%, the in-plane thermal conductivity of the epoxy resin/graphitized carbon fiber felt composite reaches 1.88W/mK, which significantly improves the thermal conductivity and builds a continuous three-dimensional thermal conductivity network at low content.
Smart Images

Figure CN118459938B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal conductive composite materials, and particularly relates to an epoxy resin / graphitized carbon fiber felt composite material and a preparation method thereof. Background Art
[0002] Appropriate temperature is the key to ensure the normal operation of electronic equipment and devices. The heat accumulation caused by the high power density of electronic components poses a threat to their stability and accuracy. Thermal management materials have been widely used to control and adjust the heat dissipation of various heat-generating components. Polymers are often used as the matrix of thermal management materials due to their light weight, corrosion resistance, easy processing, and good chemical stability. However, due to the low thermal conductivity of the polymer itself, usually <0.5W / mK, its application in the field of electronic packaging is limited. Therefore, improving the thermal conductivity of polymer-based thermal management materials is urgently needed to alleviate the heat dissipation problem.
[0003] The blending method is the most commonly used method due to its simple process. Fillers with high thermal conductivity are added to the polymer matrix. As the amount of filler added increases, the filler content reaches the percolation value, and the thermal conductivity of the polymer-based composite material is improved through the percolation effect of the filler. Commonly used fillers generally include metal fillers, ceramic fillers, carbon materials, etc. A high filler content will form an effective thermal conductivity path, but a high content of metal or ceramic fillers will damage the processing performance and mechanical properties of the composite material.
[0004] Orientation is also an effective method. Freeze-drying, magnetic orientation, electroplating, etc. make the filler form a fixed orientation in a certain direction, thereby obtaining a high thermal conductivity in a single direction.
[0005] As the research deepened, researchers found that constructing a three-dimensional thermal conductive network in the matrix can significantly improve the thermal conductivity of composite materials. Various three-dimensional network methods reduce the thermal resistance during phonon propagation by constructing a three-dimensional thermal conductive path in the matrix, including foam method (metal foam, carbon foam, ceramic foam, polymer foam), self-assembly method, spinning method, etc. These three-dimensional network methods can greatly improve the thermal conductivity of polymer-based composites. However, interfacial thermal resistance and filler dispersion problems are important factors that hinder the improvement of thermal conductivity of filled composites. Therefore, how to obtain high thermal conductivity at low content is a key issue. Summary of the invention
[0006] The object of the present invention is to provide an epoxy resin / graphitized carbon fiber felt composite material with low load and high in-plane conductivity and a preparation method thereof.
[0007] To achieve the above purpose, the technical solution used in the present invention is:
[0008] An epoxy resin / graphitized carbon fiber felt composite material uses a three-dimensional layered carbon fiber felt as a thermal conductive filler and an epoxy resin as a matrix, and is prepared through graphitization, stacking, vacuum impregnation and hot pressing processes to obtain a carbon fiber / epoxy composite material; wherein the three-dimensional layered carbon fiber felt has a layered structure and an in-plane oriented structure.
[0009] The surface density of the carbon fiber felt with three-dimensional layered structure is 10-50 g / m 2 .
[0010] In-plane thermal conductivity of the epoxy resin / graphitized carbon fiber felt composite material The in-plane thermal conductivity of the composite material reaches 1.88 W / mK at a loading of 8.5 wt %.
[0011] The preparation method of the epoxy resin / graphitized carbon fiber felt composite material comprises the following steps:
[0012] S1. Carbon fiber surface treatment:
[0013] The carbon fiber is soaked in anhydrous ethanol to dissolve the sizing agent and other surface treatment additives on the surface of the carbon fiber;
[0014] S2, dispersed carbon fiber:
[0015] The surface treated carbon fiber is mixed with a dispersant, stirred at high speed to fully disperse the fiber, and then subjected to ultrasonic treatment;
[0016] S3, preparing a formed carbon fiber sheet:
[0017] Mix carbon fiber, polyvinyl alcohol and anhydrous ethanol solution, then add the mixed solution into a sheet making machine, add a filter screen at the bottom of the sheet making machine, turn on the pneumatic homogenization to make sheets, and after the sheet making is completed, use filter paper to transfer the formed carbon fiber sheet;
[0018] S4, drying, hot pressing:
[0019] Vacuum drying; hot pressing;
[0020] S5. Graphitization and stacking treatment:
[0021] After graphitization, the carbon fiber is cut into certain specifications and stacked into different layers, ranging from 10 to 30 layers, to obtain a carbon fiber felt with a three-dimensional layered structure;
[0022] S6. Vacuum impregnation:
[0023] The three-dimensional layered carbon fiber felt is naturally impregnated in an epoxy resin solution and then vacuum impregnated;
[0024] S7, cooling and demoulding after hot pressing and curing:
[0025] An epoxy resin / graphitized carbon fiber felt composite material was prepared.
[0026] In step S3, during the vacuum impregnation process, the carbon fiber felt accounts for 3wt%-9wt% of the impregnation solution.
[0027] In step S2, the stirring speed is 2000-3000 r / min, the time is 60-150 minutes, and the ultrasonic treatment time is 10-40 minutes.
[0028] In step S5, the graphitization temperature is 1700° C. to 2000° C., and the time is 24 to 48 hours.
[0029] In step S6, the natural impregnation time is 30-90 minutes, and the vacuum impregnation time is 10-25 minutes.
[0030] In step S7, the hot pressing temperature is 100-120° C. and the time is 0.5-2 hours.
[0031] Based on the above technical solution, the present invention has the following beneficial effects:
[0032] ① Construct a three-dimensional layered carbon fiber felt with a layered structure and an in-plane oriented structure.
[0033] ② After carbonization, an epoxy resin / graphitized carbon fiber felt composite material with excellent thermal conductivity was prepared.
[0034] ③ When the filler loading is 8.5wt%, the in-plane thermal conductivity of the epoxy resin / graphitized carbon fiber felt composite material-25L can reach up to 1.88W / mK.
[0035] ④ Use carbon fiber to construct a continuous three-dimensional thermal conductive network to achieve the goal of obtaining high thermal conductivity at a low content. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is a microscopic morphology diagram of the carbon fiber felt in the present invention;
[0037] Figure 2 is a microscopic morphology of carbon fibers after carbonization in the present invention;
[0038] Figure 3 The scanning electron microscope images of the epoxy / graphitized carbon fiber felt composite material of the present invention in different directions;
[0039] Figure 4 This is a graph showing the diameter change of the fiber after graphitization of the present invention;
[0040] Figure 5 XRD and Raman spectra of the carbon fiber felt and graphitized carbon fiber felt in the present invention;
[0041] Figure 6 is a thermal conductivity diagram of the epoxy resin / graphitized carbon fiber felt composite material of the present invention;
[0042] Figure 7 Temperature distribution images and surface temperature curves at different times. DETAILED DESCRIPTION
[0043] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0044] Example 1 Epoxy resin / graphitized carbon fiber felt (Epoxy / G-CFF)-10L
[0045] S1. Soak the carbon fiber in 80% anhydrous ethanol to dissolve the sizing agent and other surface treatment additives on the fiber surface.
[0046] S2. Place the surface treated fiber and dispersant (in a mass ratio of 1:0.1) in a high-speed mixer and stir at 2250 r / min for 60 minutes to fully disperse the fiber, and then subject it to ultrasonic treatment for 10 minutes.
[0047] S3. Pour the fiber, polyvinyl alcohol, and anhydrous ethanol solution (in a mass ratio of 1:8:100) into a beaker, place the beaker in a magnetic stirring device to mix them evenly (1000r, 1h), then add the mixed solution to the sheet maker, add a filter screen to the bottom of the sheet maker, turn on the pneumatic homogenizer to make sheets. After the sheet is made, use filter paper to transfer the formed carbon fiber sheet.
[0048] S4. The carbon fiber sheet obtained above is placed in a vacuum drying oven and heated at 80° C. for 9 hours. After the excess anhydrous ethanol is volatilized, the heating is stopped.
[0049] S5. Place the dried carbon fiber sheet in a hot press at 100° C. for pressing to prepare a formed carbon fiber felt (CFF, the same below).
[0050] S6. Place the CFF in a graphitization furnace for graphitization treatment (1650° C.), thereby forming graphitized carbon fiber felt (G-CFF, the same below). Cut the graphitized carbon fiber felt into certain specifications and stack them into 10 layers.
[0051] S7. Mix the epoxy resin and curing agent in a mass ratio of 2:1, stir for 4 minutes, and prepare the epoxy resin. The content ratio of the epoxy resin to the molded carbon fiber felt is 3wt%.
[0052] S8. After naturally impregnating the graphitized carbon fiber felt in the epoxy resin for 30 minutes, vacuum impregnation was performed for 10 minutes.
[0053] S9, after hot pressing and curing at 90°C for 0.5h, cooling and demolding were performed to prepare an epoxy resin / carbon fiber felt composite material with excellent thermal conductivity.
[0054] Example 2 Epoxy resin / graphitized carbon fiber felt (Epoxy / G-CFF)-15L
[0055] S1. Soak the carbon fiber in 85% anhydrous ethanol to dissolve the sizing agent and other surface treatment additives on the fiber surface.
[0056] S2. Place the surface treated fibers and dispersant (in a mass ratio of 1:0.2) in a high-speed mixer and stir at 2500 r / min for 90 minutes to fully disperse the fibers, and then subject them to ultrasonic treatment for 20 minutes.
[0057] S3. Pour the fiber, polyvinyl alcohol, and anhydrous ethanol solution (in a mass ratio of 1:7:100) into a beaker, place the beaker in a magnetic stirring device to mix them evenly ((1500r, 1h)), then add the mixed solution to the sheet maker, add a filter screen to the bottom of the sheet maker, turn on the pneumatic homogenizer to make sheets. After the sheet is made, use filter paper to transfer the formed carbon fiber sheet.
[0058] S4. The carbon fiber sheet obtained above is placed in a vacuum drying oven and heated at 85° C. for 10 hours. After the excess anhydrous ethanol is volatilized, the heating is stopped.
[0059] S5. Place the dried carbon fiber sheet in a hot press at 105° C. for pressing to prepare a formed carbon fiber felt.
[0060] S6, placing the CFF in a graphitization furnace for graphitization treatment (1700° C.), thereby forming a graphitized carbon fiber felt. The graphitized carbon fiber felt is cut into certain specifications and stacked into 15 layers.
[0061] S7. Mix the resin and curing agent at a ratio of 2.5:1, stir for 6 minutes, and then prepare epoxy resin. The content ratio of epoxy resin to molded carbon fiber felt is 5wt%.
[0062] S8. After naturally impregnating the graphitized carbon fiber felt in the epoxy resin for 50 minutes, vacuum impregnation was performed for 15 minutes.
[0063] S9, after hot pressing and curing at 100°C for 1 hour, cooling and demolding were performed to prepare an epoxy resin / carbon fiber felt composite material (epoxy resin / graphitized carbon fiber felt) with excellent thermal conductivity.
[0064] Example 3 Epoxy resin / graphitized carbon fiber felt (Epoxy / G-CFF)-20L
[0065] S1. Soak the carbon fiber in 90% anhydrous ethanol to dissolve the sizing agent and other surface treatment additives on the fiber surface.
[0066] S2. Place the surface treated fiber and dispersant (in a mass ratio of 1:0.3) in a high-speed mixer and stir at 2750 r / min for 120 minutes to fully disperse the fiber, and then subject it to ultrasonic treatment for 30 minutes.
[0067] S3. Pour the fiber, polyvinyl alcohol, and anhydrous ethanol solution (in a mass ratio of 1:6:100) into a beaker, place the beaker in a magnetic stirring device to mix them evenly (2000r, 1h), then add the mixed solution to the sheet maker, add a filter screen to the bottom of the sheet maker, turn on the pneumatic homogenizer to make sheets. After the sheet is made, use filter paper to transfer the formed carbon fiber sheet.
[0068] S4. The carbon fiber sheet obtained above is placed in a vacuum drying oven and heated at 90° C. for 11 hours. After the excess anhydrous ethanol is volatilized, the heating is stopped.
[0069] S5. Place the dried carbon fiber sheet in a hot press at 110° C. for pressing to prepare a formed carbon fiber felt.
[0070] S6, placing the CFF in a graphitization furnace for graphitization treatment (1750° C.), thereby forming a graphitized carbon fiber felt. The graphitized carbon fiber felt is cut into a certain specification and stacked into 20 layers.
[0071] S7. Mix the resin and curing agent in a ratio of 3:1, stir for 8 minutes, and then prepare epoxy resin. The content ratio of epoxy resin to molded carbon fiber felt is 7wt%.
[0072] S8. After naturally impregnating the graphitized carbon fiber felt in the epoxy resin for 70 minutes, vacuum impregnation was performed for 20 minutes.
[0073] S9, after hot pressing and curing at 110°C for 1.5h, cooling and demolding were performed to prepare an epoxy resin / carbon fiber felt composite material with excellent thermal conductivity.
[0074] Example 4 Epoxy resin / graphitized carbon fiber felt (Epoxy / G-CFF)-25L
[0075] S1. Soak the carbon fiber in 95% anhydrous ethanol to dissolve the sizing agent and other surface treatment additives on the fiber surface.
[0076] S2. Place the surface treated fibers and dispersant (in a mass ratio of 1:0.4) in a high-speed mixer and stir at 3000 r / min for 150 minutes to fully disperse the fibers, and then subject them to ultrasonic treatment for 40 minutes.
[0077] S3. Pour the fiber, polyvinyl alcohol, and anhydrous ethanol solution (in a mass ratio of 1:5:100) into a beaker, place the beaker in a magnetic stirring device to mix them evenly (2000r, 1h), then add the mixed solution to the sheet maker, add a filter screen to the bottom of the sheet maker, and turn on the pneumatic homogenizer to make sheets. After the sheet is made, use filter paper to transfer the formed carbon fiber sheet.
[0078] S4. The carbon fiber sheet obtained above is placed in a vacuum drying oven and heated at 95° C. for 12 hours. After the excess anhydrous ethanol is volatilized, the heating is stopped.
[0079] S5. Place the dried carbon fiber sheet in a hot press at 115° C. for pressing to prepare a formed carbon fiber felt.
[0080] S6, placing the CFF in a graphitization furnace for graphitization treatment (1800° C.), thereby forming a graphitized carbon fiber felt. The graphitized carbon fiber felt is cut into certain specifications and stacked into 25 layers.
[0081] S7. Mix the resin and curing agent at a ratio of 3.5:1, stir for 10 minutes, and then prepare epoxy resin. The content ratio of epoxy resin to molded carbon fiber felt is 9wt%.
[0082] S8. After naturally impregnating the graphitized carbon fiber felt in the epoxy resin for 90 minutes, vacuum impregnation was performed for 25 minutes.
[0083] S9, after hot pressing and curing at 120°C for 2 hours, cooling and demolding were carried out to prepare an epoxy resin / carbon fiber felt composite material with excellent thermal conductivity.
[0084] Comparative Example 1:
[0085] The difference from Example 1 is that the thermally conductive composite material is prepared by combining ungraphitized carbon fiber felt with polyethylene glycol. At a carbon fiber felt loading of 47.73wt%, the thermal conductivity of the composite material is only 0.97W / mK.
[0086] Comparative Example 2:
[0087] The difference from Example 1 is that no 3D thermal conductive network is formed. Iron oxide nanoparticles (Fe3O4) are fixed on the surface of carbon fiber, magnetic carbon fiber is prepared by polydopamine technology, and the magnetized carbon fiber is vertically oriented and solidified under the action of an external magnetic field to prepare an oriented carbon fiber / polydimethylsiloxane composite material (OCF / PDMS). When filled with 20wt% CF@Fe3O4, the thermal conductivity of OCF / PDMS is as high as 1.51W / mK.
[0088] In order to verify the performance of the composite material obtained in the present invention, the standard samples obtained after the treatment of Examples 1-4 were tested, and the test results are as follows:
[0089] Figure 1 and Figure 2 The microscopic morphology of carbon fiber felt and graphitized carbon fiber felt is shown.
[0090] like Figure 1 As shown in (a)-(c), the carbon fibers are straight fibers and randomly distributed in the XY plane. Some carbon fibers appear to cross or overlap each other. Many overlapping fiber surfaces are adhered by polyvinyl alcohol. The adhesive improves the strength and stability of the carbon fiber mat.
[0091] from Figure 2 It can be seen from (d)-(f) that the morphology and distribution of carbon fibers in the XY plane have hardly changed after carbonization.
[0092] PVA decomposes into gas and evaporates during the graphitization process, causing the bonding points between the fibers to disappear.
[0093] contrast Figure 4 Middle (k) and Figure 4 In (l), it can be concluded that the diameter of the fiber changes after graphitization.
[0094] Before graphitization, the average diameter of the carbon fiber felt was about 6.27 μm, and the diameter distribution range varied slightly. In contrast, the diameter of the graphitized carbon fiber felt was about 6.07 μm.
[0095] Figure 3(g)-(j) show SEM images of epoxy / graphitized carbon fiber felt composites in different directions. In the XY plane, the graphitized carbon fiber felt maintains a randomly distributed structure, while the epoxy resin / graphitized carbon fiber felt presents a lamellar arrangement structure. This indicates that the microstructure of the graphitized carbon fiber felt did not change significantly during the molding process. After impregnation, the air space inside the graphitized carbon fiber felt was completely occupied by epoxy resin. The adhesion between the graphitized carbon fiber felt and the epoxy resin was good, and there were no obvious defects on the interface. As the number of graphitized carbon fiber felt layers increased, the distribution density of carbon fibers in the composite material also increased. Epoxy / graphitized carbon fiber felt-25L shows a denser structure. Carbon fibers provide sufficient thermal conduction channels for heat flow propagation. Phonons can propagate along the carbon chain with almost no thermal resistance. The denser carbon skeleton enriches the heat conduction pathway, thereby improving the heat conduction efficiency.
[0096] Figure 5 The microstructure of CFF and graphitized carbon fiber felt was analyzed. Figure 5 As shown in (a), the diffraction peaks of carbon fiber felt and graphitized carbon fiber felt mainly appear at 26 ◦ (002), 43 ◦ (100) and 53 ◦ (004). According to the Bragg equation, the interlayer spacing of graphitized carbon fiber felt is significantly smaller than that of carbon fiber felt. In addition, according to the Scherrer formula, the grain size of graphitized carbon fiber felt is also increased. Graphitization significantly increases the grain size and shortens the interlayer spacing, indicating that the graphitized structure after graphitization is more closely arranged.
[0097] like Figure 5 As shown in (b), the Raman spectra of carbon fiber felt and graphitized carbon fiber felt both show a peak at 1350 cm -1 The D peak and 1380cm -1 The intensity ratio of D peak to G peak (I D / I G ) is usually used to reflect the degree of defects in carbon materials. After calculation, the I D / I G The value is 1.03, which is significantly lower than 1.16 of CCF. In addition, in the Raman spectrum of graphitized carbon fiber felt, at 2700 cm -1 An additional 2D peak was observed at , indicating that it has transformed from amorphous carbon to a highly oriented graphite structure.
[0098] 3. Thermal properties of epoxy resin / graphitized carbon fiber felt composite materials Figure 6 As shown. Figure 6As shown in (a), the thermal conductivity of epoxy resin / graphitized carbon fiber felt increases significantly with the increase in the number of graphitized carbon fiber felt layers. The in-plane thermal conductivity of epoxy resin / graphitized carbon fiber felt-25L reaches a maximum value of 1.88W / mK, which is 889.47% higher than the thermal conductivity of epoxy resin. At this time, the corresponding carbon filler content is only 8.5wt%.
[0099] To better understand the anisotropy of graphitized carbon fiber mats, we calculated the thermal conductivity enhancement effect (TCE) of the in-plane and out-of-plane composites, as Figure 6 As shown in (b), with the increase of carbon fiber layers, the thermal conductivity enhancement effect of both the in-plane composite and the out-of-plane composite increases. Compared with the in-plane direction, the TCE in the out-of-plane direction decreases significantly, which is attributed to the anisotropy of carbon fibers. Figure 6 As can be seen in (c), the density of the composite material increases slightly with the increase in the number of graphitized carbon fiber felt layers. The density of the composite material is still low (1.1 g / cm 3 ), which shows that the composite material still has application prospects in the field of electronic packaging.
[0100] 4. In order to further study the actual thermal diffusion behavior, three samples of epoxy, epoxy / graphitized carbon fiber felt-15L and epoxy / graphitized carbon fiber felt-20L were placed on a constant temperature heating plate. The temperature distribution images and surface temperature curves at different times are shown in Figure 4. Figure 7 (a) and Figure 7 As shown in (b). As can be seen from the figure, all samples initially present a yellow area. As the heating progresses, the color gradually changes to pink. Compared with epoxy resin, the color change and surface temperature curve of the two composites are more obvious. When the heating time is 70s, the thermal response of epoxy / graphitized carbon fiber felt-20L (133.2 ◦ C) is significantly higher than epoxy / graphitized carbon fiber felt-15L (131.5 ◦ C). This indicates that adding graphitized carbon fiber felt can improve the thermal diffusion properties of epoxy resin / graphitized carbon fiber felt composites.
[0101] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An epoxy resin / graphitized carbon fiber felt composite material, characterized in that: A carbon fiber / epoxy composite material is prepared by using a three-dimensional layered carbon fiber felt as a thermal conductive filler and epoxy resin as a matrix through graphitization, stacking, vacuum impregnation and hot pressing molding processes; wherein the three-dimensional layered carbon fiber felt has a layered structure and an in-plane oriented structure; the surface density of the three-dimensional layered carbon fiber felt is 10-50g / m 2 ; The in-plane thermal conductivity of the epoxy resin / graphitized carbon fiber felt composite material reaches 1.88 W / mK at a loading of 8.5 wt%.
2. The method for preparing the epoxy resin / graphitized carbon fiber felt composite material according to claim 1, characterized in that: The preparation method comprises the following steps: S1. Carbon fiber surface treatment The carbon fiber is soaked in anhydrous ethanol to dissolve the sizing agent and other surface treatment additives on the surface of the carbon fiber; S2, dispersed carbon fiber The surface treated carbon fiber is mixed with a dispersant, stirred at high speed to fully disperse the fiber, and then subjected to ultrasonic treatment; S3. Preparation of formed carbon fiber sheets Mix carbon fiber, polyvinyl alcohol and anhydrous ethanol solution, then add the mixed solution into a sheet making machine, add a filter screen at the bottom of the sheet making machine, turn on the pneumatic homogenization to make sheets, and after the sheet making is completed, use filter paper to transfer the formed carbon fiber sheet; S4, drying, hot pressing Vacuum drying; hot pressing; S5. Graphitization and stacking treatment After graphitization, the carbon fiber is cut into certain specifications and stacked into different layers, ranging from 10 to 30 layers, to obtain a carbon fiber felt with a three-dimensional layered structure; S6. Vacuum impregnation The three-dimensional layered carbon fiber felt is naturally impregnated in an epoxy resin solution and then vacuum impregnated; S7, cooling and demoulding after hot pressing and curing An epoxy resin / graphitized carbon fiber felt composite material was prepared.
3. The preparation method according to claim 2, characterized in that: In step S3, during the vacuum impregnation process, the carbon fiber felt accounts for 3wt%-9wt% of the impregnation liquid.
4. The preparation method according to claim 2, characterized in that: In step S2, the stirring speed is 2000-3000 r / min, the time is 60-150 minutes, and the ultrasonic treatment time is 10-40 minutes.
5. The preparation method according to claim 2, characterized in that: In step S5, the graphitization temperature is 1700° C. to 2000° C., and the time is 24 to 48 hours.
6. The preparation method according to claim 2, characterized in that: In step S6, the natural impregnation time is 30 to 90 minutes, and the vacuum impregnation time is 10 to 25 minutes.
7. The preparation method according to claim 2, characterized in that: In step S7, the hot pressing temperature is 100-120°C and the time is 0.5-2 hours.