A carbon fiber felt electrode with gradient stiffness and preparation method thereof

By gradient depositing solid carbon on the carbon fiber felt electrode to form a gradient stiffness structure, the impact of the carbon fiber felt electrode compression ratio on battery performance is solved, and efficient energy conversion and electrolyte flow optimization are achieved.

CN118472287BActive Publication Date: 2024-10-18HANGZHOU KAIKEN NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410920132.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-18
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

The high compression ratio of the carbon fiber felt electrode will increase the contact points between the fiber and the bipolar plate and reduce the contact resistance. However, an excessively high compression ratio will hinder the diffusion and mass transfer of the electrolyte, affecting the energy efficiency of the all-vanadium redox flow battery.

Method used

Carbon fiber felt electrodes are prepared using phenolic resin derivatives containing nitro groups through an electrospinning process, and solid carbon is gradiently deposited on one side of the carbon fiber electrode felt through a chemical vapor deposition process to form a gradient stiffness carbon fiber felt electrode to control carbon deposition. Thickness to increase outer rigidity and reduce inner rigidity to optimize the compression deformation characteristics of the electrode.

Benefits of technology

It achieves a good specific surface area and low resistivity of the carbon fiber felt electrode, improves the energy efficiency of the all-vanadium redox flow battery, reduces the contact resistance and promotes the flow of electrolyte through the combination of soft and hard.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118472287B_ABST
    Figure CN118472287B_ABST
Patent Text Reader

Abstract

The present invention discloses a carbon fiber felt electrode with gradient stiffness and a preparation method thereof, and relates to the field of battery materials. The carbon fiber felt electrode with gradient stiffness adopts a phenolic resin derivative containing a nitro group to prepare the carbon fiber felt electrode through an electrostatic spinning process, and then uses a carbon source gas as a raw material and adopts a chemical vapor deposition process to gradiently deposit solid carbon on any surface of the carbon fiber electrode felt; the obtained carbon fiber felt electrode with gradient stiffness has a good specific surface area and a low resistivity, and the battery prepared using the carbon fiber felt electrode has good energy efficiency. In addition, the present invention also adds 4-phenyl-3-thiosemicarbazide during the preparation process of the carbon fiber felt electrode with gradient stiffness, so that the carbon fiber felt electrode with gradient stiffness has a better specific surface area and a lower resistivity, and the battery prepared using the carbon fiber felt electrode with gradient stiffness also has a better energy efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of battery materials, and in particular relates to a carbon fiber felt electrode with gradient stiffness and a preparation method thereof. Background Art

[0002] All-vanadium redox flow batteries (VRFBs) are a type of large-capacity energy storage battery, mainly composed of an infusion pump, a storage tank and a battery stack. The battery stack is mainly assembled from a current collector, bipolar plates, electrodes and diaphragms.

[0003] Carbon fiber felt electrodes are key components of all-vanadium liquid flow batteries, and their performance directly affects the energy efficiency of liquid flow batteries. In the battery assembly, the carbon fiber felt electrodes are assembled between the diaphragm and the bipolar plate, and a certain assembly pressure is maintained. In this structure, the carbon fiber felt electrodes will maintain a certain compression ratio. On the one hand, the higher compression ratio of the carbon fiber felt electrode will increase the contact points between the fibers and the bipolar plate, thereby effectively reducing the contact resistance between the carbon fiber felt electrode and the bipolar plate. On the other hand, too high a compression ratio will hinder the diffusion and mass transfer of the electrolyte. Therefore, the present invention discloses a carbon fiber felt electrode with a good compression ratio. Summary of the invention

[0004] The object of the present invention is to provide a carbon fiber felt electrode with gradient stiffness, wherein the carbon fiber felt electrode with gradient stiffness has a good specific surface area and a low resistivity, and a battery made by using the carbon fiber felt electrode has good energy efficiency.

[0005] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:

[0006] A method for preparing a carbon fiber felt electrode with gradient stiffness comprises: preparing a carbon fiber felt electrode by an electrostatic spinning process using a nitro group-containing phenolic resin derivative, then using a carbon source gas as a raw material, introducing a carrier gas, and using a chemical vapor deposition (CVD) process to gradiently deposit solid carbon on any surface of the carbon fiber electrode felt to obtain a carbon fiber felt electrode with gradient stiffness.

[0007] The present invention adopts CVD vapor deposition process, uses methane (CH4) as carbon source gas, and deposits solid carbon from the surface of one side of the carbon fiber electrode felt to the inside in a gradient manner. The closer to the outside, the thicker the carbon deposition, and the closer to the inside, the less carbon deposition. The solid carbon produced by the cracking of CH4 can, on the one hand, strengthen the bonding strength of the carbon fiber intersection and increase the rigidity of the carbon fiber felt, and on the other hand, reduce the resistance of the carbon fiber felt. By controlling the thickness of carbon deposition, the rigidity of the carbon fiber electrode felt changes from one side to the other. The rigidity of the carbon fiber felt near the outside is large and not easy to be compressed and deformed, while the rigidity of the carbon fiber felt near the inside is small and easy to be compressed and deformed, thereby forming a carbon fiber felt electrode with a rigidity gradient change.

[0008] Specifically, the method for preparing the above-mentioned gradient stiffness carbon fiber felt electrode comprises the following steps:

[0009] A nitro-group-containing phenolic resin derivative is added to ethanol to prepare a solution with a concentration of 20-30wt%, and then polyvinyl butyral is added. After being mixed evenly, electrospinning is performed, and step-wise heating and curing is performed. Then, in a nitrogen atmosphere, the temperature is increased to 900-1100°C at a heating rate of 4-6°C / min. After carbonization for 25-35min, water vapor is introduced (the flow rate of nitrogen is 170-180mL / min, and the flow rate of water vapor is 20-30mL / min), and activation treatment is performed at 850-950°C for 35-45min, and then the temperature is cooled to room temperature and taken out to obtain a carbon fiber felt electrode; then, a carbon source gas is used as a raw material, and a carrier gas argon gas (the flow rate of the carrier gas is 0.15-0.18m 3 / h), chemical vapor deposition was carried out at a deposition temperature of 950-1100°C and a deposition time of 4-7h to obtain a carbon fiber felt electrode with gradient stiffness.

[0010] According to an embodiment of the present invention, the mass ratio of the nitro group-containing phenolic resin derivative to polyvinyl butyral is 1:0.01-0.05.

[0011] According to an embodiment of the present invention, the molecular weight of the polyvinyl butyral is 250,000-450,000.

[0012] According to an embodiment of the present invention, the process conditions of the electrospinning are as follows: the distance between the needle and the collecting plate is 20-25 cm, the spinning voltage is 23-30 kV, and the propulsion rate is 1-1.5 mL / h.

[0013] According to an embodiment of the present invention, the process conditions of the step-by-step heating curing are: heating to 68-72°C at a heating rate of 2-4°C / min, and heat preservation for 4.5-5.5h; then heating to 78-82°C at a heating rate of 2-4°C / min, and heat preservation for 4.5-5.5h; then heating to 88-92°C at a heating rate of 2-4°C / min, and heat preservation for 2-2.5h; heating to 98-10 ...78-82°C at a heating rate of 2-4°C / min, and heat preservation for 4.5-5.5h; heating to 88-92°C at a heating rate of 2-4°C / min, and heat preservation for 2-2.5h; heating to 98-102°C at a heating rate of 2-4°C / min, and heat preservation for 2-2.5h; heating to 78-82°C at a heating rate of 2-4°C / min, and heat preservation for 4.5-5.5h. / min, heat up to 108-112℃, and keep warm for 1-1.5h; heat up to 118-122℃ at a heating rate of 2-4℃ / min, and keep warm for 1-1.5h; heat up to 128-132℃ at a heating rate of 2-4℃ / min, and keep warm for 0.5-1h; heat up to 138-142℃ at a heating rate of 2-4℃ / min, and keep warm for 0.5-1h; heat up to 178-182℃ at a heating rate of 2-4℃ / min, and keep warm for 1-1.5h.

[0014] According to an embodiment of the present invention, the carbon source gas includes methane.

[0015] According to an embodiment of the present invention, the flow rate of methane is 0.08-0.12m 3 / h.

[0016] The invention also discloses the use of the gradient stiffness carbon fiber felt electrode prepared by the preparation method in the preparation of an all-vanadium redox flow battery.

[0017] When a carbon fiber felt electrode with gradient stiffness provided by the present invention is assembled into a liquid flow battery, the side with small stiffness contacts the bipolar plate. Under compression, the fiber is deformed and in close contact with the bipolar plate, thereby reducing the contact resistance. The side with large stiffness contacts the membrane, and the fiber is less deformed. A large porosity can be maintained during compression, and the mass transfer and flow of the electrolyte are relatively smooth, thereby reducing the concentration polarization.

[0018] The invention also discloses a method for preparing a nitro-group-containing phenolic resin derivative, comprising: carrying out polycondensation reaction of phenol, o-nitro-p-tert-butylphenol and formaldehyde to prepare the nitro-group-containing phenolic resin derivative.

[0019] The invention provides a method for preparing a nitro group-containing phenolic resin derivative. Ortho-nitro-p-tert-butylphenol is used as a modifier, which is mixed with phenol and formaldehyde to obtain the nitro group-containing phenolic resin derivative through a polycondensation reaction. The nitro group-containing phenolic resin derivative is then used to prepare a gradient stiffness carbon fiber felt electrode, so that the gradient stiffness carbon fiber felt electrode has a good specific surface area and a low resistivity, and a battery prepared by using the gradient stiffness carbon fiber felt electrode has a good energy efficiency.

[0020] Specifically, the preparation method of the above-mentioned nitro group-containing phenolic resin derivative comprises the following steps:

[0021] Add molten phenol and o-nitro-p-tert-butylphenol to a 35-40wt% formaldehyde solution, stir and mix, heat to 55-65°C, add 25-28wt% ammonia water as a catalyst, heat to 85-95°C, react for 3.5-5h, and distill under reduced pressure to obtain a nitro-group-containing phenolic resin derivative.

[0022] According to an embodiment of the present invention, the molar ratio of the above-mentioned phenol to o-nitro-p-tert-butylphenol is: 1:0.15-0.25.

[0023] According to an embodiment of the present invention, the molar ratio of the phenol to formaldehyde is 1:2-2.5.

[0024] According to an embodiment of the present invention, the amount of the ammonia water is 2.5-3.5wt% of the reactants.

[0025] The invention also discloses the use of the phenolic resin derivative prepared by the preparation method in preparing a carbon fiber felt electrode.

[0026] In order to further improve the performance of the gradient stiffness carbon fiber felt electrode, the present invention also adds 4-phenyl-3-thiosemicarbazide as an additive during the preparation process of the carbon fiber felt electrode.

[0027] The present invention uses 4-phenyl-3-thiosemicarbazide in the preparation process of the carbon fiber felt electrode with gradient stiffness, so that the carbon fiber felt electrode with gradient stiffness has a better specific surface area and a lower resistivity, and the battery prepared by the carbon fiber felt electrode with gradient stiffness has a better energy efficiency. The reason may be that due to the presence of sulfur in 4-phenyl-3-thiosemicarbazide, part of the sulfur is removed during the high-temperature carbonization process of preparing the carbon fiber felt electrode with gradient stiffness, so that a large number of micropores are formed on the surface of the carbon fiber, so that the carbon fiber felt electrode has a better specific surface area; and nitrogen doping improves the wettability of the material surface and reduces the transmission resistance of the electrolyte ions, so that the charge transfer resistance is small, so that the carbon fiber felt electrode with gradient stiffness has a lower resistivity; in addition, it may be due to the doping of sulfur in the carbon fiber felt electrode that CSC active sites are formed, which improves the oxygen reduction reaction catalytic performance of the carbon fiber, thereby further promoting the improvement of the battery energy efficiency.

[0028] According to an embodiment of the present invention, the 4-phenyl-3-thiosemicarbazide is added simultaneously with polyvinyl butyral during the preparation of the carbon fiber felt electrode with gradient stiffness.

[0029] According to an embodiment of the present invention, the mass ratio of the above-mentioned 4-phenyl-3-thiosemicarbazide to polyvinyl butyral is: 1:0.8-1.

[0030] The invention also discloses the use of the 4-phenyl-3-thiosemicarbazide in preparing a carbon fiber felt electrode.

[0031] The beneficial effects of the present invention include:

[0032] The present invention obtains a carbon fiber felt electrode with gradient stiffness and a preparation method thereof. The carbon fiber felt electrode with gradient stiffness adopts a phenolic resin derivative containing a nitro group to prepare the carbon fiber felt electrode through an electrostatic spinning process, and then uses a carbon source gas as a raw material and adopts a chemical vapor deposition process to gradiently deposit solid carbon on any surface of the carbon fiber electrode felt; the obtained carbon fiber felt electrode with gradient stiffness has a good specific surface area and a low resistivity, and the battery prepared by using the carbon fiber felt electrode has good energy efficiency. In addition, the present invention also adds 4-phenyl-3-thiosemicarbazide during the preparation process of the carbon fiber felt electrode with gradient stiffness, so that the carbon fiber felt electrode with gradient stiffness has a better specific surface area and a lower resistivity, and the battery prepared by using the carbon fiber felt electrode with gradient stiffness also has a better energy efficiency.

[0033] Therefore, the present invention provides a carbon fiber felt electrode with gradient stiffness and a preparation method thereof. The carbon fiber felt electrode with gradient stiffness has good specific surface area and low resistivity, and a battery made using the carbon fiber felt electrode has good energy efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram of the carbon fiber felt electrode prepared in Example 1;

[0035] Figure 2 This is an electron microscope image of the electrodeposition coating side of the carbon fiber felt prepared in Example 1;

[0036] Figure 3 This is an electron microscope image of the non-deposited coating side of the carbon fiber felt electrode prepared in Example 1;

[0037] Figure 4 These are the infrared spectra test results of the nitro-group-containing phenolic resin derivative prepared in Example 1 and the phenolic resin prepared in Example 5. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention is further described in detail below in conjunction with specific implementation methods:

[0039] Embodiment 1:

[0040] A method for preparing a carbon fiber felt electrode with gradient stiffness comprises the following steps:

[0041] A nitro-group-containing phenolic resin derivative was added to ethanol to prepare a solution with a concentration of 20 wt%, and then polyvinyl butyral was added. After being mixed evenly, electrospinning was performed, and step-wise heating and curing was performed. Then, the temperature was increased to 900°C at a heating rate of 4°C / min in a nitrogen atmosphere. After carbonization for 35 minutes, water vapor was introduced (the flow rate of nitrogen was 170 mL / min, and the flow rate of water vapor was 20 mL / min), and activation treatment was performed at 850°C for 45 minutes, and then the temperature was cooled to room temperature and taken out to obtain a carbon fiber felt electrode.

[0042] Take a 5mm thick carbon fiber felt electrode, put one side of it close to the graphite plate, and leave the other side untreated, and place it vertically in the CVD furnace; then use methane gas as the raw material (the flow rate of methane is 0.1m 3 / h), introduce carrier gas argon (the flow rate of carrier gas is 0.16m 3 / h), chemical vapor deposition was performed at a deposition temperature of 1000°C and a deposition time of 5h to obtain a carbon fiber felt electrode with gradient stiffness, as shown in the schematic diagram. Figure 1 As shown, the electron microscope image of the side with deposited coating is as follows Figure 2 The electron microscope image of the non-coated side (i.e. the side close to the graphite plate) is shown in Figure 3 As shown by Figure 2 , Figure 3 It can be seen that solid carbon is deposited gradiently from the surface of one side of the carbon fiber electrode felt to the inside. The closer to the outside, the thicker the carbon deposition is, and the closer to the inside, the less carbon deposition is. The solid carbon produced by methane cracking can strengthen the bonding of the carbon fiber intersections, thereby increasing the stiffness of the carbon fiber felt.

[0043] The mass ratio of the nitro group-containing phenolic resin derivative to polyvinyl butyral is 1:0.01; the molecular weight of polyvinyl butyral is 250,000.

[0044] The process conditions of electrospinning were as follows: the distance between the needle and the collecting plate was 20 cm, the spinning voltage was 23 kV, and the propulsion rate was 1 mL / h.

[0045] The process conditions of step heating curing are as follows: heating to 68°C at a heating rate of 2°C / min, and keeping warm for 5.5 hours; then heating to 78°C at a heating rate of 2°C / min, and keeping warm for 5.5 hours; then heating to 88°C at a heating rate of 2°C / min, and keeping warm for 2.5 hours; heating to 98°C at a heating rate of 2°C / min, and keeping warm for 2.5 hours; heating to 108°C at a heating rate of 2°C / min, and keeping warm for 1.5 hours; heating to 118°C at a heating rate of 2°C / min, and keeping warm for 1.5 hours; heating to 128°C at a heating rate of 2°C / min, and keeping warm for 1 hour; heating to 138°C at a heating rate of 2°C / min, and keeping warm for 1 hour; heating to 178°C at a heating rate of 2°C / min, and keeping warm for 1.5 hours.

[0046] The preparation method of the phenolic resin derivative containing a nitro group comprises the following steps:

[0047] Add molten phenol and o-nitro-p-tert-butylphenol to a 35wt% formaldehyde solution, stir and mix, heat to 55°C, add 25wt% ammonia water as a catalyst, heat to 85°C for 5h, and distill under reduced pressure to obtain a phenolic resin derivative. The molar ratio of phenol to o-nitro-p-tert-butylphenol is 1:0.15; the molar ratio of phenol to formaldehyde is 1:2; and the amount of ammonia water is 2.5wt% of the reactants.

[0048] Embodiment 2:

[0049] A method for preparing a carbon fiber felt electrode with gradient stiffness comprises the following steps:

[0050] A nitro-group-containing phenolic resin derivative was added to ethanol to prepare a solution with a concentration of 30 wt%, and then polyvinyl butyral was added. After being mixed evenly, electrospinning was performed, and step-wise heating and curing was performed. Then, the temperature was raised to 1100°C at a heating rate of 6°C / min in a nitrogen atmosphere. After carbonization for 25 minutes, water vapor was introduced (the flow rate of nitrogen was 180 mL / min, and the flow rate of water vapor was 30 mL / min), and activation treatment was performed at 950°C for 35 minutes, and then the temperature was cooled to room temperature and taken out to obtain a carbon fiber felt electrode.

[0051] Take a 5mm thick carbon fiber felt electrode, put one side of it close to the graphite plate, and leave the other side untreated, and place it vertically in the CVD furnace; then use methane gas as the raw material (the flow rate of methane is 0.12m 3 / h), introduce carrier gas argon (the flow rate of carrier gas is 0.18m 3 / h), chemical vapor deposition was carried out with a deposition temperature of 1100°C and a deposition time of 4h to obtain a carbon fiber felt electrode with gradient stiffness.

[0052] The mass ratio of the nitro group-containing phenolic resin derivative to polyvinyl butyral is 1:0.05; the molecular weight of polyvinyl butyral is 450,000.

[0053] The process conditions of electrospinning were as follows: the distance between the needle and the collecting plate was 25 cm, the spinning voltage was 30 kV, and the propulsion rate was 1.5 mL / h.

[0054] The process conditions of step heating curing are as follows: heating to 72°C at a heating rate of 4°C / min, and keeping warm for 4.5 hours; then heating to 82°C at a heating rate of 4°C / min, and keeping warm for 4.5 hours; then heating to 92°C at a heating rate of 4°C / min, and keeping warm for 2 hours; heating to 102°C at a heating rate of 4°C / min, and keeping warm for 2 hours; heating to 112°C at a heating rate of 4°C / min, and keeping warm for 1 hour; heating to 122°C at a heating rate of 4°C / min, and keeping warm for 1 hour; heating to 132°C at a heating rate of 4°C / min, and keeping warm for 0.5 hours; heating to 142°C at a heating rate of 4°C / min, and keeping warm for 0.5 hours; heating to 182°C at a heating rate of 4°C / min, and keeping warm for 1 hour.

[0055] The preparation method of the phenolic resin derivative containing a nitro group comprises the following steps:

[0056] Add molten phenol and o-nitro-p-tert-butylphenol to a 40wt% formaldehyde solution, stir and mix, heat to 65°C, add 28wt% ammonia water as a catalyst, heat to 95°C for 3.5h, and distill under reduced pressure to obtain a phenolic resin derivative. The molar ratio of phenol to o-nitro-p-tert-butylphenol is 1:0.15; the molar ratio of phenol to formaldehyde is 1:2; and the amount of ammonia water is 2.5wt% of the reactants.

[0057] Embodiment 3:

[0058] A method for preparing a carbon fiber felt electrode with gradient stiffness comprises the following steps:

[0059] A nitro-group-containing phenolic resin derivative was added to ethanol to prepare a solution with a concentration of 20 wt%, and then polyvinyl butyral and 4-phenyl-3-thiosemicarbazide were added, mixed evenly, and then electrospun, cured by stepwise heating, and then heated to 900°C at a heating rate of 4°C / min in a nitrogen atmosphere. After carbonization for 35 minutes, water vapor was introduced (nitrogen flow rate of 170 mL / min, water vapor flow rate of 20 mL / min), activated at 850°C for 45 minutes, cooled to room temperature and taken out to obtain a carbon fiber felt electrode;

[0060] Take a 5mm thick carbon fiber felt electrode, put one side of it close to the graphite plate, and leave the other side untreated, and place it vertically in the CVD furnace; then use methane gas as the raw material (the flow rate of methane is 0.1m 3 / h), introduce carrier gas argon (the flow rate of carrier gas is 0.16m 3 / h), chemical vapor deposition was carried out with a deposition temperature of 1000°C and a deposition time of 5h to obtain a carbon fiber felt electrode with gradient stiffness.

[0061] The mass ratio of the nitro group-containing phenolic resin derivative to polyvinyl butyral is 1:0.01; the molecular weight of polyvinyl butyral is 250,000; and the mass ratio of 4-phenyl-3-thiosemicarbazide to polyvinyl butyral is 1:0.8.

[0062] The electrospinning process is the same as that in Example 1.

[0063] The process conditions of step-by-step heating and curing are the same as those in Example 1.

[0064] The preparation method of the phenolic resin derivative containing a nitro group is the same as that in Example 1.

[0065] Embodiment 4:

[0066] The difference between the method for preparing a carbon fiber felt electrode with gradient stiffness and Example 3 is that the mass ratio of 4-phenyl-3-thiosemicarbazide to polyvinyl butyral is 1:1.

[0067] Embodiment 5:

[0068] The difference between the method for preparing a carbon fiber felt electrode with gradient stiffness and Example 1 is that phenolic resin is used to replace the phenolic resin derivative containing nitro groups.

[0069] The difference between the preparation method of the phenolic resin and the preparation method of the phenolic resin derivative containing a nitro group in Example 1 is that o-nitro-p-tert-butylphenol is not added during the preparation process.

[0070] Embodiment 6:

[0071] The difference between the method for preparing a carbon fiber felt electrode with gradient stiffness and Example 3 is that phenolic resin is used to replace the phenolic resin derivative containing nitro groups.

[0072] The preparation method of phenolic resin is the same as that in Example 5.

[0073] Test example:

[0074] 1. Infrared spectrum test

[0075] The test was carried out using a Fourier transform infrared spectrometer with a wavelength range of 400-4000cm -1 .

[0076] The above test was performed on the nitro-containing phenolic resin derivative prepared in Example 1 and the phenolic resin prepared in Example 5. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that compared with the infrared spectrum of phenolic resin, the infrared spectrum of phenolic resin derivatives containing nitro groups is at 1548 cm -1 、1349cm -1 There is a characteristic infrared absorption peak of nitro group at the position, indicating that o-nitro-p-tert-butylphenol participates in the formation reaction of phenolic resin derivatives.

[0077] 2. Energy efficiency test

[0078] Carbon fiber felt samples were used as electrodes, ion exchange membranes were used as separators between positive and negative electrodes, and two pieces of conductive plastic were used as current collectors. 2+ A mixed solution of (0.8 mol / L) + H2SO4 (0.8 mol / L) was used as the electrolyte to prepare a single cell. Then, according to the NB / T 42081-2016 all-vanadium liquid flow battery single cell performance test method, the current density was 80 mA / cm 2 Under the conditions, the energy efficiency was tested; the comparative sample used the carbon fiber felt electrode prepared in Example 1 (ie, the carbon fiber felt electrode without chemical vapor deposition).

[0079] Table 1 Energy efficiency test results

[0080]

[0081] The above test was performed on the gradient stiffness carbon fiber felt electrodes prepared in Examples 1 to 6, and the results are shown in Table 1. As can be seen from Table 1, compared with Example 5, Example 3 and Example 6, the energy efficiency is significantly improved, indicating that when the gradient stiffness carbon fiber felt electrode prepared by using a nitro-group-containing phenolic resin derivative is used to prepare the battery, the battery has good energy efficiency; compared with Example 1, Example 3, and Example 6 and Example 5, the energy efficiency is increased, indicating that when 4-phenyl-3-thiosemicarbazide is added during the preparation of the gradient stiffness carbon fiber felt electrode and then used in the preparation of the battery, the battery also has good energy efficiency; the reason may be that the doping of sulfur element in the carbon fiber felt electrode forms CSC active sites, which improves the oxygen reduction reaction catalytic performance of the carbon fiber, thereby further promoting the improvement of the battery energy efficiency.

[0082] 3. Resistivity test

[0083] The carbon fiber felt electrode samples were tested using an RTS-8 four-probe resistivity tester; the control sample was the carbon fiber felt electrode prepared in Example 1 (a carbon fiber felt electrode that was not subjected to chemical vapor deposition).

[0084] Table 2 Resistivity test results

[0085]

[0086] The above test was performed on the carbon fiber felt electrodes with gradient stiffness prepared in Examples 1 to 6, and the results are shown in Table 2. As can be seen from Table 2, compared with Example 5, Example 3 and Example 6, the resistivity is significantly reduced, indicating that when the carbon fiber felt electrode with gradient stiffness prepared by using a phenolic resin derivative containing a nitro group is used for the preparation of a battery, the battery has a lower resistivity; compared with Example 1, Example 6 and Example 5, the resistivity is also reduced, indicating that when 4-phenyl-3-thiosemicarbazide is added during the preparation of the carbon fiber felt electrode with gradient stiffness and then used in the preparation of the battery, the battery also has a lower resistivity; the reason may be that nitrogen doping improves the wettability of the material surface and reduces the transmission resistance of the electrolyte ions, thereby making the charge transfer resistance smaller, so that the carbon fiber felt electrode with gradient stiffness has a lower resistivity.

[0087] 4. Specific surface area test

[0088] The specific surface area and porosity analyzer was used to test and analyze the specific surface area of ​​the sample through the adsorption and desorption of N2.

[0089] Table 3 Specific surface area test results

[0090]

[0091] The above test was performed on the gradient stiffness carbon fiber felt electrodes prepared in Examples 1 to 6, and the results are shown in Table 3. As can be seen from Table 3, compared with Example 5, Example 3 and Example 6, the specific surface area is significantly improved, indicating that when the gradient stiffness carbon fiber felt electrode prepared by the phenolic resin derivative containing a nitro group is used for the preparation of the battery, the battery has a good specific surface area; compared with Example 1, Example 3, and Example 6 and Example 5, the specific surface area is increased, indicating that when 4-phenyl-3-thiosemicarbazide is added during the preparation of the gradient stiffness carbon fiber felt electrode and then used in the preparation of the battery, the battery also has a good specific surface area; the reason may be due to the presence of sulfur in 4-phenyl-3-thiosemicarbazide, part of the sulfur is removed during the high-temperature carbonization process of preparing the gradient stiffness carbon fiber felt electrode, so that a large number of micropores are formed on the surface of the carbon fiber, so that the carbon fiber felt electrode has a better specific surface area.

[0092] 5. Compression deformation test

[0093] The samples were tested at a pressure of 0.1 MPa using a computer compression tester RH-300.

[0094] Table 4 Compression deformation test results

[0095]

[0096] The above test was performed on the gradient stiffness carbon fiber felt electrode prepared in Example 1, and the results are shown in Table 4. As can be seen from Table 4, the coated side has a large stiffness, the fiber is not easily deformed, which is conducive to the circulation of electrolyte, can reduce the polarization internal resistance of the battery, and improve the energy efficiency of the battery as a whole; the fiber on the uncoated side (i.e., the side close to the graphite plate) is easily compressed and deformed during assembly, which increases the contact area with the bipolar plate, reduces the contact resistance, and improves the energy efficiency of the battery as a whole; therefore, through the combination of soft and hard, the energy efficiency of the battery assembled by this electrode can be greatly improved.

[0097] The conventional techniques in the above embodiments are prior arts known to those skilled in the art, and thus will not be described in detail here.

[0098] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a carbon fiber felt electrode with gradient stiffness, comprising: A carbon fiber felt electrode is prepared by electrospinning a phenolic resin derivative containing a nitro group, and then a carbon source gas is used as a raw material, a carrier gas is introduced, and a chemical vapor deposition process is used to gradiently deposit solid carbon on any surface of the carbon fiber electrode felt to obtain a carbon fiber felt electrode with gradient stiffness; In the preparation of the carbon fiber felt electrode with gradient stiffness, a phenolic resin derivative containing a nitro group is added to ethanol to prepare a solution with a concentration of 20-30wt%, and then polyvinyl butyral is added and mixed evenly, followed by electrospinning, step-by-step heating and curing, and then heated to 900-1100°C at a heating rate of 4-6°C / min in a nitrogen atmosphere. After carbonization for 25-35 minutes, water vapor is introduced, and the electrode is activated at 850-950°C for 35-45 minutes, cooled to room temperature and taken out to obtain a carbon fiber felt electrode; then, carbon source gas is used as a raw material, carrier gas argon is introduced, and chemical vapor deposition is carried out, the deposition temperature is 950-1100°C, and the deposition time is 4-7h to obtain a carbon fiber felt electrode with gradient stiffness; when water vapor is introduced, the flow rate of nitrogen is 170-180mL / min, the flow rate of water vapor is 20-30mL / min, and the flow rate of carrier gas argon is 0.15-0.18m 3 / h; The method for preparing the nitro-group-containing phenolic resin derivative comprises: carrying out polycondensation reaction of phenol, o-nitro-p-tert-butylphenol and formaldehyde to prepare the nitro-group-containing phenolic resin derivative.

2. The method for preparing a carbon fiber felt electrode with gradient stiffness according to claim 1, characterized in that: The carbon source gas includes methane.

3. The method for preparing a gradient stiffness carbon fiber felt electrode according to claim 2, characterized in that: The flow rate of methane is 0.08-0.12m 3 / h.

4. The method for preparing a carbon fiber felt electrode with gradient stiffness according to claim 1, characterized in that: The molar ratio of the phenol to o-nitro-p-tert-butylphenol is 1:0.15-0.

25.

5. The method for preparing a carbon fiber felt electrode with gradient stiffness according to claim 1, characterized in that: The process conditions of the electrospinning are: the distance between the needle and the collecting plate is 20-25 cm, the spinning voltage is 23-30 kV, and the propulsion rate is 1-1.5 mL / h.

Citation Information

Patent Citations

  • Preparing method of microporous carbon fiber with high specific surface area

    CN106521715A

  • Gradient electrode for flow batteries and application thereof

    CN106558704A