A method for preparing silicon carbide ceramics by pressureless sintering
Through pressureless sintering technology, combined with silicon carbide pretreatment, coating and modification of aminated carbon fiber, a tight network structure of silicon carbide ceramics is formed, which solves the problems of brittleness and poor sintering performance of silicon carbide ceramic materials, and improves its Toughness and flexural strength ensure the strength performance after low temperature treatment.
Patent Information
- Application Number
- CN202410946779.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The brittleness, low fracture toughness, and poor sintering performance of silicon carbide ceramic materials limit their use in various applications. Existing modification methods have low toughness and flexural strength retention rates after low-temperature treatment.
Using a pressureless sintering method, coconut oil fatty acid diethanol is processed through silicon carbide pretreatment, coating, modification of coated particles, amination of carbon fibers, preparation of slurry, molding and sintering steps, including the use of sodium hydroxide solution to treat silicon carbide. Amide and polyvinylpyrrolidone ultrasonic treatment, silica coating, epoxidation treatment and chitosan combination, amination of carbon fiber and modified coating particles are closely combined to form a tight silicon carbide, silica and carbon fiber network.
Significantly improves the fracture toughness, flexural strength and stability of silicon carbide ceramics, allowing it to maintain high strength properties after low temperature treatment and extending its service life.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon carbide ceramics, and in particular relates to a method for preparing silicon carbide ceramics by pressureless sintering. Background Art
[0002] Silicon carbide ceramics are a type of ceramic with silicon carbide as the main component. They have good room temperature mechanical properties, such as bending strength, corrosion resistance, wear resistance, etc., and their high temperature mechanical properties are the best among known ceramic materials. They are widely used in the fields of petroleum, chemical industry, microelectronics, automobiles, aerospace, mining and lasers.
[0003] However, silicon carbide ceramics are brittle, have low fracture toughness, are highly sensitive to crack strength, and have poor sintering properties, which limits their application and development.
[0004] At present, in order to improve the fracture toughness and sintering performance, carbon fiber, alumina fiber, etc. are usually used as reinforcement phases to prepare composite ceramics with silicon carbide as the matrix. However, the fiber has poor wettability, low reaction activity, poor interface performance with the silicon carbide matrix, and poor compatibility, which ultimately affects the wear resistance and bending resistance of silicon carbide ceramics.
[0005] Therefore, modifying the fibers to improve their wettability and reactivity, thereby improving the interface properties with the silicon carbide matrix and enhancing the comprehensive properties of silicon carbide ceramics has become a new research direction.
[0006] To this end, the prior art discloses the following method:
[0007] CN113698221A discloses a preparation method of a modified carbon fiber toughened silicon carbide ceramic material and a modified carbon fiber toughened silicon carbide ceramic material, specifically disclosing that graphene oxide is first grafted on the surface of the carbon fiber, then aluminum oxide is deposited on the surface of the graphene oxide modified carbon fiber to form a graphene oxide modified carbon fiber coated with aluminum oxide, finally a silicon carbide layer is deposited on the surface of the graphene oxide modified carbon fiber by a chemical deposition method to obtain the modified carbon fiber, the modified carbon fiber is mixed with silicon carbide powder, a sintering aid, a phenolic resin, graphite powder, and deionized water, and the mixture is subjected to dry pressing, curing, and calcining to obtain the modified carbon fiber toughened silicon carbide ceramic material;
[0008] This patent improves the oxidation resistance of carbon fiber, thereby improving the toughness of silicon carbide ceramic materials and increasing their flexural strength. However, the ceramic material produced by this patent has poor stability. After low-temperature treatment, it loses a lot of toughness and flexural strength, which seriously affects its performance.
[0009] CN118047621A discloses a fiber-reinforced silicon carbide composite material and a preparation method thereof, specifically disclosing that the raw material components include modified silicon carbide powder, silicon powder, modified carbon fiber, phenolic resin, graphite powder, a stabilizing agent, and a sintering agent; wherein the modified silicon carbide powder is obtained by coating and modifying the surface of the silicon carbide powder using dispersants hydroxyethyl cellulose and calcium carbonate and polyacrylic acid; the modified carbon fiber is a modified carbon fiber coated with a graphene oxide layer, a silicon carbide layer, and a carbon nanotube layer in sequence from the inside to the outside;
[0010] This patent improves the problem of easy agglomeration of silicon carbide powder by modifying the silicon carbide powder, thereby improving the sintering performance of the composite material, and improving the fracture toughness and bending strength of the composite material, and reducing the mass loss at high temperature;
[0011] However, the silicon carbide ceramic composite material produced by this patent has poor wear resistance, and after low-temperature treatment, the toughness and bending strength retention rate are low, which limits the application of the composite material. Summary of the invention
[0012] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing silicon carbide ceramics by pressureless sintering, which improves the toughness of silicon carbide ceramics, enhances the bending strength, has good stability, and maintains high strength after low-temperature treatment.
[0013] In view of the above technical problems, the present invention adopts the following technical solutions:
[0014] A method for preparing silicon carbide ceramics by pressureless sintering includes silicon carbide pretreatment, coating, modified coated particles, amination of carbon fibers, slurry preparation, molding, and sintering steps. The specific operations are as follows:
[0015] 1. Silicon carbide pretreatment
[0016] The silicon carbide is placed in a sealed container, and a sodium hydroxide solution is introduced for soaking, the soaking time is 2.2-2.4 hours, the soaking temperature is 105-108° C., and after the soaking, the silicon carbide is washed to obtain alkali-leached silicon carbide, and the alkali-leached silicon carbide is placed in anhydrous ethanol, and coconut oil fatty acid diethanolamide and polyvinyl pyrrolidone are added for ultrasonic treatment, the ultrasonic time is 20-25 minutes, the ultrasonic power is 112-117W, and the ultrasonic frequency is 43-48kHz. After the ultrasonic treatment, the silicon carbide is dried to obtain pretreated silicon carbide;
[0017] The particle size of the silicon carbide is 135-145 nm;
[0018] The mass concentration of the sodium hydroxide solution is 8.5-8.9%;
[0019] The mass ratio of silicon carbide to sodium hydroxide solution is 28-32:145-154;
[0020] The mass ratio of silicon carbide, anhydrous ethanol, coconut oil fatty acid diethanolamide and polyvinyl pyrrolidone after alkali leaching is 18-22:63-67:1.0-1.2:0.7-1.0.
[0021] 2. Wrapping
[0022] The pretreated silicon carbide is placed in the mixed solution 1 for ultrasonic dispersion, the ultrasonic time is 14-16 minutes, the ultrasonic power is 204-215W, and the ultrasonic frequency is 25-29kHz. After the ultrasonic dispersion is completed, ammonia water and the mixed solution 2 are added at the same time, and stirred for 6.8-7.2 hours and a stirring speed of 215-224rpm. After the stirring is completed, the mixture is filtered and washed, and then placed in a vacuum freeze dryer for vacuum freeze drying, the cold trap temperature is -48 to -44°C, the drying time is 11-13 hours, and the vacuum degree is 92-96Pa. After the vacuum freeze drying is completed, the mixture is naturally restored to room temperature to obtain coated particles;
[0023] The mass volume ratio of the pretreated silicon carbide to the mixed solution 1, ammonia water and the mixed solution 2 is 16-18 g: 494-505 mL: 9.7-10.2 mL: 56-60 mL;
[0024] The mixed solution 1 is composed of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is 1.5-1.7:0.3;
[0025] The mass fraction of the ammonia water is 24-26%;
[0026] The second mixed solution is an ethanol solution of ethyl orthosilicate, and the mass fraction of ethyl orthosilicate is 24-27%.
[0027] 3. Modified coated particles
[0028] (1) One-time modification
[0029] The coated particles are placed in a muffle furnace, heated to 376-384°C at a rate of 4.7-5.3°C / min, calcined at 376-384°C for 3.3-3.7h, and naturally restored to room temperature after calcination. The particles are then placed in an ethanol solution, and tartaric acid and sodium dodecylbenzene sulfonate are added for ball milling. The ball milling time is 33-37min, the ball milling speed is 122-126rpm, the ball milling temperature is 67-69°C, and the ball-to-material ratio is 4-6:1. After the ball milling is completed, the particles are filtered and dried to obtain primary modified coated particles.
[0030] The mass ratio of the coated particles, ethanol solution, tartaric acid, and sodium dodecylbenzene sulfonate is 12-14:76-80:0.6-0.8:1.1-1.3;
[0031] The mass concentration of the ethanol solution is 36-40%;
[0032] (2) Secondary modification
[0033] The first modified coated particles are placed in an acetone solution, stirred evenly, and then epichlorohydrin and sodium hydroxide solution are added to react by stirring, the stirring speed is controlled to be 200-210rpm, the stirring time is 2.8-3.2h, the stirring temperature is 52-54°C, and the epoxidized coated particles are obtained after washing and drying; an acetic acid solution is introduced into a closed container, and then chitosan is added for stirring, the stirring time is 1.8-2.2h, the stirring speed is 312-326rpm, after the stirring is completed, the epoxidized coated particles are added, stirred evenly, the temperature is raised to 60-64°C at a rate of 1.7-2.3°C / min, the reaction is stirred for 3.4-3.6h, and the second modified coated particles are obtained after washing and drying;
[0034] The mass ratio of the primary modified coated particles, acetone solution, epichlorohydrin, and sodium hydroxide solution is 8-12:90-98:64-68:73-77;
[0035] The volume mass ratio of the acetic acid solution, chitosan, and epoxidized coated particles is 485-494 mL: 9.7-10.3 g: 2.2-2.4 g;
[0036] The mass concentration of the acetone solution is 30-34%;
[0037] The mass concentration of the sodium hydroxide solution is 26-29%;
[0038] The mass concentration of the acetic acid solution is 2.6-2.8%.
[0039] 4. Aminated carbon fiber
[0040] The carbon fiber is placed in deionized water, glyceryl monostearate and sodium hexadecyl sulfate are added and stirred evenly, and then subjected to microwave treatment, the microwave time is 8-12 minutes, the microwave power is 104-115W, and the microwave frequency is 17-23kHz. After the microwave is finished, an acid solution is added for stirring, the stirring temperature is 62-64°C, and the stirring time is 2.9-3.1 hours. After the stirring is finished, the acid-treated carbon fiber is filtered, washed, and dried to obtain the acid-treated carbon fiber. The acid-treated carbon fiber is placed in a sealed container, and then a triethylenetetramine solution is introduced, and dicyclohexylcarbodiimide is added dropwise, the pressure is controlled to be 0.11-0.14MPa, and the temperature is increased to 112-116°C at a rate of 1.3-1.7°C / min, and the reaction is refluxed at 112-116°C for 13-15 hours. After the reaction is finished, the carbon fiber is filtered, washed, and dried to obtain the amino carbon fiber.
[0041] The mass ratio of the carbon fiber, deionized water, glyceryl monostearate, sodium hexadecyl sulfate, acid solution, triethylenetetramine solution, and dicyclohexylcarbodiimide is 9-11 g: 33-37 g: 0.4-0.6 g: 0.7-0.9 g: 177-184 g: 495-504 mL: 10.2-10.4 g;
[0042] The diameter of the carbon fiber is 195-210 nm and the length is 0.02-0.04 mm;
[0043] The acid solution is a mixture of concentrated nitric acid solution and concentrated sulfuric acid solution, and the mass ratio of the concentrated nitric acid solution to the concentrated sulfuric acid solution is 1.2-1.5:1.0;
[0044] The mass concentration of the concentrated nitric acid solution is 70-74%; the mass concentration of the concentrated sulfuric acid solution is 78-82%;
[0045] The mass concentration of the triethylenetetramine solution is 11-13%.
[0046] 5. Preparation of slurry
[0047] Silicon carbide, secondary modified coated particles, amino carbon fibers, aluminum nitride, phenolic resin, sodium lignin sulfonate, polyethylene glycol 600, stearic acid and deionized water are mixed, and then stirred at a stirring speed of 743-755 rpm, a stirring time of 1.4-1.6 h, and a stirring temperature of 28-32° C. After the stirring is completed, a slurry is obtained;
[0048] The mass ratio of silicon carbide, secondary modified coated particles, amino carbon fiber, aluminum nitride, phenolic resin, sodium lignin sulfonate, polyethylene glycol 600, stearic acid and deionized water is 86-90:6.3-6.5:4.2-4.4:1.2-1.6:1.5-1.9:1.1-1.3:1.1-1.4:0.8-1.2:96-100;
[0049] The particle size of the silicon carbide particles is 0.3-0.5 μm;
[0050] The particle size of the aluminum nitride is 0.7-0.9 μm.
[0051] 6. Molding
[0052] The slurry was placed in a spray dryer for spray granulation, and then placed in a steel mold and maintained at a pressure of 33-35 MPa for 92-96 seconds to obtain a green body.
[0053] 7. Sintering
[0054] The green body is placed in a pressureless sintering furnace, and in a nitrogen atmosphere, the temperature is increased to 664-675°C at a rate of 4.8-5.2°C / min, and kept at 664-675°C for 13-17min, then the temperature is increased to 1250-1360°C at a rate of 3.2-3.8°C / min, and kept at 1250-1360°C for 18-22min, and then the temperature is increased to 2010-2050°C at a rate of 1.8-2.2°C / min, and kept at 2010-2050°C for 1.4-1.6h. After the insulation is completed, it is naturally cooled to room temperature to obtain silicon carbide ceramics.
[0055] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0056] 1. The present invention pre-treats silicon carbide by using a sodium hydroxide solution to improve the activation performance of silicon carbide particles. After being treated with coconut oil fatty acid diethanolamide and polyvinyl pyrrolidone, the attraction between silicon carbide particles can be weakened, a better dispersion effect is achieved, and a better steric effect is formed. Then, silicon carbide particles are coated with silicon dioxide to enhance the compatibility between silicon carbide and silicon dioxide. After a primary modification, the surface dispersion performance of the coated particles is improved and the aggregation between the coated particles is reduced. In the secondary modification step, epoxidation treatment is first performed, and then chitosan is added to allow the amino groups of chitosan to react with the epoxy groups on the surfaces of the coated particles. The modified coated particles are prepared by combining the silicon dioxide and the modified coated particles, which give full play to the reinforcing property of silicon carbide particles; the carbon fibers are aminated so that the surface of the carbon fibers is rich in amino groups, and the amino groups can be bonded with the hydroxyl groups on the surface of the modified coated particles, so that the carbon fibers and the modified coated particles are tightly combined and firmly connected, and finally the tight combination between silicon carbide, silicon dioxide and carbon fibers is achieved, and the reinforcing property of silicon carbide particles is fully exerted by silicon dioxide and carbon fibers, and the strength properties such as fracture toughness and flexural strength of silicon carbide ceramics are improved, and the stability of silicon carbide ceramics is guaranteed, so that silicon carbide ceramics can still maintain high strength properties after low-temperature treatment;
[0057] 2. The silicon carbide ceramics prepared by the method of the present invention have a tensile strength of 279-283 MPa and a fracture toughness of 8.14-8.29 MPa·m 1 / 2 , flexural strength is 482-490MPa, tensile strength is 338-348MPa;
[0058] 3. The silicon carbide ceramic prepared by the method of the present invention was cooled to -20°C at a rate of 2.0°C / min, allowed to stand at -20°C for 12 hours, then cooled to -40°C at a rate of 1.0°C / min, allowed to stand at -40°C for 24 hours, then cooled to -50°C at a rate of 0.5°C / min, allowed to stand at -50°C for 144 hours, and then naturally restored to room temperature. The tensile strength of the silicon carbide ceramic was measured again to be 271-276MPa, and the fracture toughness was 7.96-8.17MPa·m 1 / 2 , the flexural strength is 466-478MPa, and the tensile strength is 324-337MPa. DETAILED DESCRIPTION
[0059] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.
[0060] Example 1
[0061] 1. Silicon carbide pretreatment
[0062] 30 g of silicon carbide was placed in a sealed container, and 150 g of sodium hydroxide solution was introduced for soaking. The soaking time was 2.3 h and the soaking temperature was 107 ° C. After the soaking, the silicon carbide was washed to obtain alkali-leached silicon carbide. 20 g of the alkali-leached silicon carbide was placed in 70 g of anhydrous ethanol, and 1.1 g of coconut oil fatty acid diethanolamide and 0.8 g of polyvinyl pyrrolidone were added for ultrasonic treatment. The ultrasonic time was 23 min, the ultrasonic power was 115 W, and the ultrasonic frequency was 45 kHz. After the ultrasonic treatment, the silicon carbide was dried to obtain pretreated silicon carbide;
[0063] The particle size of the silicon carbide is 140 nm;
[0064] The mass concentration of the sodium hydroxide solution is 8.7%.
[0065] 2. Wrapping
[0066] 17g of pretreated silicon carbide was placed in 500mL of mixed solution 1 for ultrasonic dispersion, the ultrasonic time was 15min, the ultrasonic power was 210W, and the ultrasonic frequency was 27kHz. After the ultrasonic dispersion was completed, 10mL of ammonia water and 58mL of mixed solution 2 were added at the same time, and stirred for 7h at a stirring speed of 220rpm. After the stirring was completed, the mixture was filtered and washed, and then placed in a vacuum freeze dryer for vacuum freeze drying, the cold trap temperature was -46°C, the drying time was 12h, and the vacuum degree was 94Pa. After the vacuum freeze drying was completed, the mixture was naturally restored to room temperature to obtain coated particles;
[0067] The mixed solution 1 is composed of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is 1.6:0.3;
[0068] The mass fraction of the ammonia water is 25%;
[0069] The second mixed solution is an ethanol solution of ethyl orthosilicate, and the mass fraction of ethyl orthosilicate is 25%.
[0070] 3. Modified coated particles
[0071] (1) One-time modification
[0072] 13 g of coated particles were placed in a muffle furnace, heated to 380°C at a rate of 5.0°C / min, and calcined at 380°C for 3.5 h. After calcination, the particles were naturally restored to room temperature. Then, the particles were placed in 78 g of ethanol solution, 0.7 g of tartaric acid and 1.2 g of sodium dodecylbenzene sulfonate were added, and ball milling was performed. The ball milling time was 35 min, the ball milling speed was 124 rpm, the ball milling temperature was 68°C, and the ball-to-material ratio was 5:1. After the ball milling was completed, the particles were filtered and dried to obtain primary modified coated particles.
[0073] The mass concentration of the ethanol solution is 38%;
[0074] (2) Secondary modification
[0075] 10g of the primary modified coated particles were placed in 95g of acetone solution, and after stirring, 66g of epichlorohydrin and 75g of sodium hydroxide solution were added for stirring reaction, and the stirring speed was controlled to be 204rpm, the stirring time was 3.0h, and the stirring temperature was 53°C. After washing and drying, epoxidized coated particles were obtained; 490mL of acetic acid solution was introduced into a closed container, and then 10g of chitosan was added for stirring, the stirring time was 2.0h, and the stirring speed was 320rpm. After the stirring was completed, 2.3g of epoxidized coated particles were added, and after stirring, the temperature was raised to 62°C at a rate of 2.0°C / min, and the reaction was stirred for 3.5h, and then washed and dried to obtain secondary modified coated particles;
[0076] The mass concentration of the acetone solution is 32%;
[0077] The mass concentration of the sodium hydroxide solution is 28%;
[0078] The mass concentration of the acetic acid solution is 2.7%.
[0079] 4. Aminated carbon fiber
[0080] 10g of carbon fiber was placed in 35g of deionized water, 0.5g of monostearate glyceryl and 0.8g of sodium hexadecyl sulfate were added and stirred evenly, and then microwave treatment was performed, the microwave time was 10min, the microwave power was 110W, and the microwave frequency was 20kHz. After the microwave was finished, 180g of acid solution was added and stirred, the stirring temperature was 63°C, and the stirring time was 3.0h. After the stirring was finished, it was filtered, washed and dried to obtain acid-treated carbon fiber. The acid-treated carbon fiber was placed in a closed container, and then 500mL of triethylenetetramine solution was passed, 10.3g of dicyclohexylcarbodiimide was added dropwise, the pressure was controlled to 0.12MPa, and the temperature was raised to 114°C at a rate of 1.5°C / min. Reflux reaction was performed at 114°C for 14h. After the reaction was finished, it was filtered, washed and dried to obtain amino carbon fiber.
[0081] The diameter of the carbon fiber is 200nm and the length is 0.03mm;
[0082] The acid solution is a mixture of concentrated nitric acid solution and concentrated sulfuric acid solution, and the mass ratio of the concentrated nitric acid solution to the concentrated sulfuric acid solution is 1.3:1.0;
[0083] The mass concentration of the concentrated nitric acid solution is 72%; the mass concentration of the concentrated sulfuric acid solution is 80%;
[0084] The mass concentration of the triethylenetetramine solution is 12%.
[0085] 5. Preparation of slurry
[0086] 88 g of silicon carbide, 6.4 g of secondary modified coated particles, 4.3 g of amino carbon fiber, 1.4 g of aluminum nitride, 1.7 g of phenolic resin, 1.2 g of sodium lignin sulfonate, 1.3 g of polyethylene glycol 600, 1.0 g of stearic acid and 98 g of deionized water were mixed, and then stirred at a stirring speed of 750 rpm, a stirring time of 1.5 h, and a stirring temperature of 30° C. After the stirring was completed, a slurry was obtained;
[0087] The particle size of the silicon carbide particles is 0.4 μm;
[0088] The particle size of the aluminum nitride is 0.8 μm.
[0089] 6. Molding
[0090] The slurry was placed in a spray dryer for spray granulation, and then placed in a steel mold and maintained at a pressure of 34 MPa for 94 seconds to obtain a green body.
[0091] 7. Sintering
[0092] The green body was placed in a pressureless sintering furnace, and under a nitrogen atmosphere, the temperature was increased to 670°C at a rate of 5.0°C / min, and kept at 670°C for 15 minutes, then the temperature was increased to 1300°C at a rate of 3.5°C / min, and kept at 1300°C for 20 minutes, and then the temperature was increased to 2030°C at a rate of 2.0°C / min, and kept at 2030°C for 1.5 hours. After the insulation was completed, it was naturally cooled to room temperature to obtain silicon carbide ceramics.
[0093] Example 2
[0094] 1. Silicon carbide pretreatment
[0095] 28g of silicon carbide was placed in a sealed container, and 145g of sodium hydroxide solution was introduced for soaking. The soaking time was 2.2h and the soaking temperature was 105°C. After the soaking, the silicon carbide was washed to obtain alkali-leached silicon carbide. 18g of the alkali-leached silicon carbide was placed in 67g of anhydrous ethanol, and 1.0g of coconut oil fatty acid diethanolamide and 0.7g of polyvinyl pyrrolidone were added for ultrasonic treatment. The ultrasonic time was 20min, the ultrasonic power was 112W, and the ultrasonic frequency was 43kHz. After the ultrasonic treatment, the silicon carbide was dried to obtain pretreated silicon carbide.
[0096] The particle size of the silicon carbide is 135 nm;
[0097] The mass concentration of the sodium hydroxide solution is 8.5%.
[0098] 2. Wrapping
[0099] 16 g of pretreated silicon carbide was placed in 494 mL of mixed solution 1 for ultrasonic dispersion. The ultrasonic time was 14 min, the ultrasonic power was 204 W, and the ultrasonic frequency was 25 kHz. After the ultrasonic dispersion was completed, 9.7 mL of ammonia water and 56 mL of mixed solution 2 were added simultaneously and stirred. The stirring time was 6.8 h and the stirring speed was 215 rpm. After the stirring was completed, the mixture was filtered and washed, and then placed in a vacuum freeze dryer for vacuum freeze drying. The cold trap temperature was -48 ° C, the drying time was 11 h, and the vacuum degree was 92 Pa. After the vacuum freeze drying was completed, the mixture was naturally restored to room temperature to obtain coated particles.
[0100] The mixed solution 1 is composed of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is 1.5:0.3;
[0101] The mass fraction of the ammonia water is 24%;
[0102] The second mixed solution is an ethanol solution of ethyl orthosilicate, and the mass fraction of ethyl orthosilicate is 24%.
[0103] 3. Modified coated particles
[0104] (1) One-time modification
[0105] 12 g of coated particles were placed in a muffle furnace, heated to 376°C at a rate of 4.7°C / min, and calcined at 376°C for 3.3 h. After calcination, the particles were naturally restored to room temperature. Then, the particles were placed in 76 g of ethanol solution, 0.6 g of tartaric acid and 1.1 g of sodium dodecylbenzene sulfonate were added, and ball milling was performed. The ball milling time was 33 min, the ball milling speed was 122 rpm, the ball milling temperature was 67°C, and the ball-to-material ratio was 4:1. After the ball milling was completed, the particles were filtered and dried to obtain primary modified coated particles.
[0106] The mass concentration of the ethanol solution is 36%;
[0107] (2) Secondary modification
[0108] 8g of the primary modified coated particles were placed in 90g of acetone solution, and after stirring, 64g of epichlorohydrin and 73g of sodium hydroxide solution were added for stirring reaction, and the stirring speed was controlled to be 200rpm, the stirring time was 2.8h, and the stirring temperature was 52°C. After washing and drying, epoxidized coated particles were obtained; 485mL of acetic acid solution was introduced into a closed container, and then 9.7g of chitosan was added for stirring, the stirring time was 1.8h, and the stirring speed was 312rpm. After the stirring was completed, 2.2g of epoxidized coated particles were added, and after stirring, the temperature was raised to 60°C at a rate of 1.7°C / min, and the reaction was stirred for 3.4h, and then washed and dried to obtain secondary modified coated particles;
[0109] The mass concentration of the acetone solution is 30%;
[0110] The mass concentration of the sodium hydroxide solution is 26%;
[0111] The mass concentration of the acetic acid solution is 2.6%.
[0112] 4. Aminated carbon fiber
[0113] 9g of carbon fiber was placed in 33g of deionized water, 0.4g of monostearate glyceryl and 0.7g of sodium hexadecyl sulfate were added and stirred evenly, and then microwave treatment was performed, the microwave time was 8min, the microwave power was 104W, and the microwave frequency was 17kHz. After the microwave was finished, 177g of acid solution was added and stirred, the stirring temperature was 62°C, and the stirring time was 2.9h. After the stirring was finished, it was filtered, washed and dried to obtain acid-treated carbon fiber, the acid-treated carbon fiber was placed in a closed container, and then 495mL of triethylenetetramine solution was passed, 10.2g of dicyclohexylcarbodiimide was added dropwise, the pressure was controlled to 0.11MPa, the temperature was raised to 112°C at a rate of 1.3°C / min, and refluxed at 112°C for 13h. After the reaction was finished, it was filtered, washed and dried to obtain amino carbon fiber;
[0114] The diameter of the carbon fiber is 195nm and the length is 0.02mm;
[0115] The acid solution is a mixture of concentrated nitric acid solution and concentrated sulfuric acid solution, and the mass ratio of the concentrated nitric acid solution to the concentrated sulfuric acid solution is 1.2:1.0;
[0116] The mass concentration of the concentrated nitric acid solution is 70%; the mass concentration of the concentrated sulfuric acid solution is 78%;
[0117] The mass concentration of the triethylenetetramine solution is 11%.
[0118] 5. Preparation of slurry
[0119] 86 g of silicon carbide, 6.3 g of secondary modified coated particles, 4.2 g of amino carbon fiber, 1.2 g of aluminum nitride, 1.5 g of phenolic resin, 1.1 g of sodium lignin sulfonate, 1.1 g of polyethylene glycol 600, 0.8 g of stearic acid and 96 g of deionized water were mixed, and then stirred at a stirring speed of 743 rpm, a stirring time of 1.4 h, and a stirring temperature of 28° C. After the stirring was completed, a slurry was obtained;
[0120] The particle size of the silicon carbide particles is 0.3 μm;
[0121] The particle size of the aluminum nitride is 0.7 μm.
[0122] 6. Molding
[0123] The slurry was placed in a spray dryer for spray granulation, and then placed in a steel mold and maintained at a pressure of 33 MPa for 92 seconds to obtain a green body.
[0124] 7. Sintering
[0125] The green body was placed in a pressureless sintering furnace, and under a nitrogen atmosphere, the temperature was increased to 664°C at a rate of 4.8°C / min, and kept at 664°C for 13 minutes, then the temperature was increased to 1250°C at a rate of 3.2°C / min, and kept at 1250°C for 18 minutes, and then the temperature was increased to 2010°C at a rate of 1.8°C / min, and kept at 2010°C for 1.4 hours. After the insulation was completed, it was naturally cooled to room temperature to obtain silicon carbide ceramics.
[0126] Example 3
[0127] 1. Silicon carbide pretreatment
[0128] 32g of silicon carbide was placed in a sealed container, and 154g of sodium hydroxide solution was introduced for soaking. The soaking time was 2.4h and the soaking temperature was 108°C. After the soaking, the silicon carbide was washed to obtain alkali-leached silicon carbide. 22g of the alkali-leached silicon carbide was placed in 73g of anhydrous ethanol, and 1.2g of coconut oil fatty acid diethanolamide and 1.0g of polyvinyl pyrrolidone were added for ultrasonic treatment. The ultrasonic time was 25min, the ultrasonic power was 117W, and the ultrasonic frequency was 48kHz. After the ultrasonic treatment, the silicon carbide was dried to obtain pretreated silicon carbide.
[0129] The particle size of the silicon carbide is 145 nm;
[0130] The mass concentration of the sodium hydroxide solution is 8.9%.
[0131] 2. Wrapping
[0132] 18g of pretreated silicon carbide was placed in 505mL of mixed solution 1 for ultrasonic dispersion. The ultrasonic time was 16min, the ultrasonic power was 215W, and the ultrasonic frequency was 29kHz. After the ultrasonic dispersion was completed, 10.2mL of ammonia water and 60mL of mixed solution 2 were added simultaneously and stirred. The stirring time was 7.2h and the stirring speed was 224rpm. After the stirring was completed, the mixture was filtered and washed, and then placed in a vacuum freeze dryer for vacuum freeze drying. The cold trap temperature was -44°C, the drying time was 13h, and the vacuum degree was 96Pa. After the vacuum freeze drying was completed, the mixture was naturally restored to room temperature to obtain coated particles.
[0133] The mixed solution 1 is composed of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is 1.7:0.3;
[0134] The mass fraction of the ammonia water is 26%;
[0135] The second mixed solution is an ethanol solution of ethyl orthosilicate, and the mass fraction of ethyl orthosilicate is 27%.
[0136] 3. Modified coated particles
[0137] (1) One-time modification
[0138] 14 g of coated particles were placed in a muffle furnace, heated to 384°C at a rate of 5.3°C / min, and calcined at 384°C for 3.7 h. After calcination, the particles were naturally restored to room temperature. Then, the particles were placed in 80 g of ethanol solution, 0.8 g of tartaric acid and 1.3 g of sodium dodecylbenzene sulfonate were added, and ball milling was performed. The ball milling time was 37 min, the ball milling speed was 126 rpm, the ball milling temperature was 69°C, and the ball-to-material ratio was 6:1. After the ball milling was completed, the particles were filtered and dried to obtain primary modified coated particles.
[0139] The mass concentration of the ethanol solution is 40%;
[0140] (2) Secondary modification
[0141] 12g of the primary modified coated particles were placed in 98g of acetone solution, and after stirring, 68g of epichlorohydrin and 77g of sodium hydroxide solution were added for stirring reaction, and the stirring speed was controlled to be 210rpm, the stirring time was 3.2h, and the stirring temperature was 54°C. After washing and drying, epoxidized coated particles were obtained; 494mL of acetic acid solution was introduced into a closed container, and then 10.3g of chitosan was added for stirring, the stirring time was 2.2h, and the stirring speed was 326rpm. After the stirring was completed, 2.4g of epoxidized coated particles were added, and after stirring, the temperature was raised to 64°C at a rate of 2.3°C / min, and the reaction was stirred for 3.6h, and then washed and dried to obtain secondary modified coated particles;
[0142] The mass concentration of the acetone solution is 34%;
[0143] The mass concentration of the sodium hydroxide solution is 29%;
[0144] The mass concentration of the acetic acid solution is 2.8%.
[0145] 4. Aminated carbon fiber
[0146] 11g of carbon fiber was placed in 37g of deionized water, 0.6g of monostearate glyceryl and 0.9g of sodium hexadecyl sulfate were added and stirred evenly, and then microwave treatment was performed, the microwave time was 12min, the microwave power was 115W, and the microwave frequency was 23kHz. After the microwave was finished, 184g of acid solution was added for stirring, the stirring temperature was 64°C, and the stirring time was 3.1h. After the stirring was finished, it was filtered, washed and dried to obtain acid-treated carbon fiber, the acid-treated carbon fiber was placed in a closed container, and then 504mL of triethylenetetramine solution was passed, 10.4g of dicyclohexylcarbodiimide was added dropwise, the pressure was controlled to 0.14MPa, the temperature was raised to 116°C at a rate of 1.7°C / min, and refluxed at 116°C for 15h. After the reaction was finished, it was filtered, washed and dried to obtain amino carbon fiber;
[0147] The diameter of the carbon fiber is 210nm and the length is 0.04mm;
[0148] The acid solution is a mixture of concentrated nitric acid solution and concentrated sulfuric acid solution, and the mass ratio of the concentrated nitric acid solution to the concentrated sulfuric acid solution is 1.5:1.0;
[0149] The mass concentration of the concentrated nitric acid solution is 74%; the mass concentration of the concentrated sulfuric acid solution is 82%;
[0150] The mass concentration of the triethylenetetramine solution is 13%.
[0151] 5. Preparation of slurry
[0152] 90 g of silicon carbide, 6.5 g of secondary modified coated particles, 4.4 g of amino carbon fiber, 1.6 g of aluminum nitride, 1.9 g of phenolic resin, 1.3 g of sodium lignin sulfonate, 1.4 g of polyethylene glycol 600, 1.2 g of stearic acid and 100 g of deionized water were mixed, and then stirred at a stirring speed of 755 rpm, a stirring time of 1.6 h, and a stirring temperature of 32° C. After the stirring was completed, a slurry was obtained;
[0153] The particle size of the silicon carbide particles is 0.5 μm;
[0154] The particle size of the aluminum nitride is 0.9 μm.
[0155] 6. Molding
[0156] The slurry was placed in a spray dryer for spray granulation, and then placed in a steel mold and maintained at a pressure of 35 MPa for 96 seconds to obtain a green body.
[0157] 7. Sintering
[0158] The green body was placed in a pressureless sintering furnace, and under a nitrogen atmosphere, the temperature was increased to 675°C at a rate of 5.2°C / min, and kept at 675°C for 17 minutes, then the temperature was increased to 1360°C at a rate of 3.8°C / min, and kept at 1360°C for 22 minutes, and then the temperature was increased to 2050°C at a rate of 2.2°C / min, and kept at 2050°C for 1.6 hours. After the insulation was completed, it was naturally cooled to room temperature to obtain silicon carbide ceramics.
[0159] Comparative Example 1
[0160] Based on Example 1, the changes are as follows:
[0161] (1) The silicon carbide pretreatment step is omitted, and in the coating step, the pretreated silicon carbide is replaced by an equal amount of silicon carbide that has not been treated in any way, and the particle size of the silicon carbide is 140 nm;
[0162] (2) The secondary modification step of the modified coated particles is omitted, and in the slurry preparation step, the secondary modified coated particles are replaced with the primary modified coated particles in equal amounts;
[0163] The rest of the operations are the same.
[0164] Comparative Example 2
[0165] The changes on the basis of Example 1 are that the step of aminating carbon fiber is omitted, and in the step of preparing slurry, an equal amount of aminating carbon fiber is replaced by carbon fiber without any treatment, wherein the diameter of the carbon fiber is 200 nm and the length is 0.03 mm;
[0166] The rest of the operations are the same.
[0167] Test Example 1
[0168] The silicon carbide ceramics prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests, and the test results are as follows:
[0169]
[0170] Test Example 2
[0171] The silicon carbide ceramics prepared in Examples 1-3 and Comparative Examples 1-2 were cooled to -20°C at a rate of 2.0°C / min, allowed to stand at -20°C for 12 hours, then cooled to -40°C at a rate of 1.0°C / min, allowed to stand at -40°C for 24 hours, then cooled to -50°C at a rate of 0.5°C / min, allowed to stand at -50°C for 144 hours, and then naturally restored to room temperature. The tensile strength, fracture toughness, flexural strength and tensile strength of the silicon carbide ceramics were tested again. The test results are as follows:
[0172]
[0173] The present invention performs pretreatment on silicon carbide, wherein the silicon carbide is treated with a sodium hydroxide solution to improve the activation performance of silicon carbide particles, and is treated with coconut oil fatty acid diethanolamide and polyvinyl pyrrolidone to weaken the attraction between silicon carbide particles, achieve a better dispersion effect, and form a better steric effect; then, silicon carbide particles are coated with silicon dioxide to enhance the compatibility between silicon carbide and silicon dioxide; after a primary modification, the surface dispersion performance of the coated particles is improved, and the aggregation between the coated particles is reduced; in a secondary modification step, an epoxidation treatment is first performed, and then chitosan is added to allow the amino groups of the chitosan to react with the epoxy groups on the surfaces of the coated particles. The modified coated particles are prepared by combining the carbon fibers with the silicon carbide particles to give full play to the reinforcing effect of silicon dioxide on the silicon carbide particles; the carbon fibers are aminated to make the surface of the carbon fibers rich in amino groups, and the amino groups can bond with the hydroxyl groups on the surface of the modified coated particles, so that the carbon fibers and the modified coated particles are tightly bound and firmly connected, and finally the tight binding between silicon carbide, silicon dioxide and carbon fibers is achieved, and the reinforcing properties of silicon dioxide and carbon fibers for silicon carbide particles are fully exerted, and the strength properties of silicon carbide ceramics such as fracture toughness and flexural strength are improved, and the stability of silicon carbide ceramics is guaranteed, so that silicon carbide ceramics can still maintain high strength properties after low-temperature treatment.
[0174] Comparative Example 1 omits the pretreatment step of silicon carbide, and uses silicon dioxide to coat silicon carbide particles that have not been treated in any way. The silicon carbide particles are in a state of agglomeration. During the coating process, the coating is uneven, and the dispersion of silicon carbide and silicon dioxide is poor. In addition, Comparative Example 1 also omits the secondary modification step of modifying the coated particles. The primary modified coated particles obtained have poor compatibility with other components, which results in poor homogeneity of the slurry. After sintering, the strength and stability of the silicon carbide ceramic are affected, and the service life of the ceramic is shortened.
[0175] Comparative Example 2 omits the amination step for the carbon fiber. The untreated carbon fiber has poor compatibility with components such as the secondary modified coated particles. The carbon fiber cannot be evenly dispersed in the silicon carbide ceramic matrix, which affects the reinforcement performance of silicon carbide, resulting in the fracture toughness of the silicon carbide ceramic still being low, the strength performance still being poor, and the low-temperature resistance performance being poor.
[0176] Unless otherwise specified, all percentages used in the present invention are by mass.
[0177] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing silicon carbide ceramics by pressureless sintering, characterized in that: The method for preparing silicon carbide ceramics includes the steps of silicon carbide pretreatment, coating, modified coated particles, amination of carbon fibers, slurry preparation, molding, and sintering; The silicon carbide pretreatment step comprises placing the silicon carbide in a sealed container, introducing a sodium hydroxide solution for soaking, wherein the soaking time is 2.2-2.4 hours and the soaking temperature is 105-108° C. After the soaking, washing is performed to obtain alkali-soaked silicon carbide, placing the alkali-soaked silicon carbide in anhydrous ethanol, adding coconut oil fatty acid diethanolamide and polyvinyl pyrrolidone for ultrasonic treatment, and drying after the ultrasonic treatment to obtain pretreated silicon carbide; The coating step comprises placing the pretreated silicon carbide in a mixed solution 1 and performing ultrasonic dispersion, adding ammonia water and the mixed solution 2 at the same time after the ultrasonic dispersion is completed, stirring, filtering, washing, and then placing the mixed solution in a vacuum freeze dryer for vacuum freeze drying, wherein the cold trap temperature is -48 to -44°C, the drying time is 11 to 13 hours, and the vacuum degree is 92 to 96 Pa. After the vacuum freeze drying is completed, the mixture is naturally restored to room temperature to obtain coated particles; The second mixed solution is an ethanol solution of tetraethyl orthosilicate; The modified coated particles include a primary modification and a secondary modification step; The first modification step is to place the coated particles in a muffle furnace, heat the temperature to 376-384°C at a rate of 4.7-5.3°C / min, calcine at 376-384°C for 3.3-3.7h, and naturally return to room temperature after calcination. Then, the particles are placed in an ethanol solution, tartaric acid and sodium dodecylbenzene sulfonate are added, and ball milling is performed. The ball milling time is 33-37min, the ball milling speed is 122-126rpm, the ball milling temperature is 67-69°C, and the ball-to-material ratio is 4-6:
1. After the ball milling is completed, the particles are filtered and dried to obtain first modified coated particles. The secondary modification step is to place the primary modified coated particles in an acetone solution, stir evenly, add epichlorohydrin and sodium hydroxide solution, perform a primary stirring reaction, wash and dry, and obtain epoxidized coated particles; introduce acetic acid solution into a closed container, then add chitosan and perform secondary stirring, after the stirring is completed, add epoxidized coated particles, stir evenly, heat to 60-64°C at a rate of 1.7-2.3°C / min, react by stirring for 3.4-3.6h, wash and dry, and obtain secondary modified coated particles; The step of aminating the carbon fiber is as follows: placing the carbon fiber in deionized water, adding glyceryl monostearate and sodium hexadecyl sulfate and stirring evenly, then subjecting the carbon fiber to microwave treatment, adding an acid solution and stirring after the microwave treatment, filtering, washing, and drying after the stirring treatment to obtain the acid-treated carbon fiber, placing the acid-treated carbon fiber in a sealed container, then introducing a triethylenetetramine solution, adding dicyclohexylcarbodiimide dropwise, controlling the pressure to be 0.11-0.14 MPa, heating to 112-116° C. at a rate of 1.3-1.7° C. / min, reflux reaction at 112-116° C. for 13-15 hours, filtering, washing, and drying after the reaction treatment to obtain the aminating carbon fiber; The step of preparing the slurry is to mix silicon carbide, secondary modified coated particles, amino carbon fibers, aluminum nitride, phenolic resin, sodium lignin sulfonate, polyethylene glycol 600, stearic acid and deionized water, and then stir the mixture at a stirring speed of 743-755 rpm, a stirring time of 1.4-1.6 h, and a stirring temperature of 28-32° C. After the stirring is completed, the slurry is obtained; The mass ratio of the silicon carbide, the secondary modified coated particles, the amino carbon fibers, the aluminum nitride, the phenolic resin, the sodium lignin sulfonate, the polyethylene glycol 600, the stearic acid and the deionized water is 86-90:6.3-6.5:4.2-4.4:1.2-1.6:1.5-1.9:1.1-1.3:1.1-1.4:0.8-1.2:96-100.
2. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: In the step of pre-treating the silicon carbide, the particle size of the silicon carbide is 135-145 nm; The mass concentration of the sodium hydroxide solution is 8.5-8.9%; The mass ratio of silicon carbide to sodium hydroxide solution is 28-32:145-154; The mass ratio of the alkali-soaked silicon carbide, anhydrous ethanol, coconut oil fatty acid diethanolamide, and polyvinyl pyrrolidone is 18-22:63-67:1.0-1.2:0.7-1.0; The ultrasonic treatment has an ultrasonic time of 20-25 min, an ultrasonic power of 112-117 W, and an ultrasonic frequency of 43-48 kHz.
3. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: In the coating step, the mass volume ratio of the pretreated silicon carbide to the mixed solution 1, ammonia water and the mixed solution 2 is 16-18 g: 494-505 mL: 9.7-10.2 mL: 56-60 mL; The mixed solution 1 is composed of ethanol and deionized water, and the volume ratio of the ethanol to the deionized water is 1.5-1.7:0.3; The mass fraction of the ammonia water is 24-26%; In the second mixed solution, the mass fraction of ethyl orthosilicate is 24-27%; The ultrasonic dispersion has an ultrasonic time of 14-16 min, an ultrasonic power of 204-215 W, and an ultrasonic frequency of 25-29 kHz; The stirring time is 6.8-7.2h, and the stirring speed is 215-224rpm.
4. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: In the step of the primary modification, the mass ratio of the coated particles, the ethanol solution, the tartaric acid, and the sodium dodecylbenzene sulfonate is 12-14:76-80:0.6-0.8:1.1-1.3; The mass concentration of the ethanol solution is 36-40%.
5. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: In the step of secondary modification, the mass ratio of the primary modified coated particles, acetone solution, epichlorohydrin, and sodium hydroxide solution is 8-12:90-98:64-68:73-77; The volume mass ratio of the acetic acid solution, chitosan, and epoxidized coated particles is 485-494 mL: 9.7-10.3 g: 2.2-2.4 g; The mass concentration of the acetone solution is 30-34%; The mass concentration of the sodium hydroxide solution is 26-29%; The mass concentration of the acetic acid solution is 2.6-2.8%; The stirring reaction is performed at a speed of 200-210 rpm, a stirring time of 2.8-3.2 h, and a stirring temperature of 52-54 ° C. The secondary stirring has a stirring time of 1.8-2.2 hours and a stirring speed of 312-326 rpm.
6. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: In the step of aminating the carbon fiber, the mass ratio of the carbon fiber, deionized water, glyceryl monostearate, sodium hexadecyl sulfate, acid solution, triethylenetetramine solution, and dicyclohexylcarbodiimide is 9-11 g: 33-37 g: 0.4-0.6 g: 0.7-0.9 g: 177-184 g: 495-504 mL: 10.2-10.4 g; The diameter of the carbon fiber is 195-210 nm and the length is 0.02-0.04 mm; The acid solution is a mixture of concentrated nitric acid solution and concentrated sulfuric acid solution, and the mass ratio of the concentrated nitric acid solution to the concentrated sulfuric acid solution is 1.2-1.5:1.0; The mass concentration of the concentrated nitric acid solution is 70-74%; the mass concentration of the concentrated sulfuric acid solution is 78-82%; The mass concentration of the triethylenetetramine solution is 11-13%; The microwave treatment has a microwave time of 8-12 min, a microwave power of 104-115 W, and a microwave frequency of 17-23 kHz; The stirring temperature is 62-64° C. and the stirring time is 2.9-3.1 h.
7. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: In the step of preparing the slurry, the particle size of the silicon carbide particles is 0.3-0.5 μm; The particle size of the aluminum nitride is 0.7-0.9 μm.
8. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: The molding step is to place the slurry in a spray dryer for spray granulation, and then place it in a steel mold and maintain the pressure at 33-35 MPa for 92-96 seconds to obtain a green body.
9. The method for preparing silicon carbide ceramics by pressureless sintering according to claim 1, characterized in that: The sintering step comprises placing the green body in a pressureless sintering furnace, heating the green body to 664-675°C at a rate of 4.8-5.2°C / min in a nitrogen atmosphere, keeping the temperature at 664-675°C for 13-17min, then heating the green body to 1250-1360°C at a rate of 3.2-3.8°C / min, keeping the temperature at 1250-1360°C for 18-22min, then heating the green body to 2010-2050°C at a rate of 1.8-2.2°C / min, keeping the temperature at 2010-2050°C for 1.4-1.6h, and cooling the green body to room temperature naturally after the temperature is kept, so as to obtain silicon carbide ceramics.
Citation Information
Patent Citations
Preparation method of modified carbon fiber toughened silicon carbide ceramic material and modified carbon fiber toughened silicon carbide ceramic material
CN113698221A
Fiber-reinforced silicon carbide composite material and preparation method thereof
CN118047621A
composite material AND PROCESS FOR ITS MANUFACTURE
ATA3752003A
Manufacturing method of pressureless liquid-phase sintered silicon carbide ceramic grinding disc
CN114380610A