A highly adaptable sponge for household items and a preparation method thereof
By doping polyurethane sponge with halloysite nanotubes and using dopamine and glutaraldehyde technology to adhere to the surface of the sponge, combined with sodium alginate to form a dense layer, the problem of unstable flame retardant performance of sponges in the existing technology is solved. , achieving the long-lasting flame retardant performance of highly adaptable sponges.
Patent Information
- Application Number
- CN202410935283.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Existing polyurethane sponges lack long-lasting flame retardant properties in furniture manufacturing, and halloysite nanotubes easily fall off on the surface of the sponge, resulting in unstable flame retardant properties.
By reacting halloysite nanotubes with polyether polyol and toluene diisocyanate, halloysite nanotubes are internally doped, and using dopamine self-polymerization and glutaraldehyde cross-linking technology, halloysite nanotubes are adhered to sponges. On the surface, combined with sodium alginate, it is evenly dispersed to form a dense flame retardant protective layer.
The long-lasting flame retardant performance of the polyurethane sponge is achieved, ensuring the firm combination of halloysite nanotubes and the surface of the sponge, and improving the stability and density of the flame retardant performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of sponge materials, and in particular to a highly adaptable sponge for household items and a preparation method thereof. Background Art
[0002] Polyurethane sponge is a foam material made of polyurethane raw materials, which has the characteristics of lightness, softness, shock absorption, and insulation. It has a wide range of applications in the home furnishing field, especially in furniture manufacturing. Polyurethane sponge is widely used in furniture manufacturing, mainly for the production of furniture products such as sofas, seats, and mattresses. Due to its excellent elasticity and comfort, polyurethane sponge can provide good support and pressure dispersion, making users more comfortable when using these furniture. For example, in sofas and seats, polyurethane sponge not only increases the softness of the cushion, but also effectively absorbs impact and reduces the vibration to the human body. In addition, polyurethane sponge also has a long service life and a strong protective effect, which makes it widely promoted and applied in furniture manufacturing. In mattress manufacturing, polyurethane sponge can provide a better sleeping experience through its excellent shock absorption performance. In short, polyurethane sponge has been widely used in the home furnishing field, especially in furniture manufacturing, because of its lightness, softness, shock absorption, and insulation. Its excellent elasticity and comfort make it an ideal choice for furniture manufacturing, bringing users a better use experience.
[0003] Chinese Patent Publication No. CN106279608 discloses an wormwood polyurethane composite household foam sponge, which is prepared from the following raw materials in parts by weight: microcrystalline cellulose, soybean oil, diethylene glycol, potassium hydroxide, polyether polyol, foaming agent, foam stabilizer, catalyst, toluene diisocyanate, distilled water, tetraethyl orthosilicate, wormwood, and silicone oil. Although the foam sponge pad prepared by the present invention has good comfort, environmental protection, good resilience, high tensile strength and other characteristics, it does not have flame retardant properties as a furniture item and has safety hazards.
[0004] Chinese patent publication number CN109651643 discloses a flame-retardant polyurethane sponge and its preparation method and application. The method comprises the following specific steps: soaking the polyurethane sponge in a water dispersion of halloysite nanotubes, squeezing the polyurethane sponge with force, and stirring or ultrasonicating the halloysite nanotubes to evenly coat the polyurethane sponge; placing the polyurethane sponge in a drying device, turning the sponge over once every certain period of time; after the liquid gradually evaporates, removing the halloysite nanotubes that are not firmly bonded, and obtaining a flame-retardant polyurethane sponge modified by the halloysite nanotube coating. Although the sponge has certain flame retardant properties, the flame retardant components are easily detached from the sponge surface, and it does not have long-term flame retardant properties. Summary of the invention
[0005] In order to overcome the above problems of the prior art, the present invention provides a highly adaptable sponge for household products and a preparation method thereof. The sponge prepared by the present invention is used for household products, has high adaptability, and has long-lasting excellent flame retardant properties.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0007] A method for preparing a highly adaptable sponge for household items comprises the following steps:
[0008] S1, uniformly mixing polyether polyol, halloysite nanotubes and natural spar powder to obtain a first component;
[0009] S2, mixing dibutyltin diacetate and triethylamine uniformly to obtain a composite catalyst, and then adding foaming agent water and foam stabilizer silicone oil to the composite catalyst to obtain a second component;
[0010] S3, mixing the first component and the second component evenly to obtain a mixture, adding toluene diisocyanate to the mixture, and stirring until foaming;
[0011] S4, heating the foamed organic matter for maturation to obtain a polyurethane sponge;
[0012] S5, adding dopamine hydrochloride to Tris buffer, stirring and mixing to obtain a mixed solution, adding modified halloysite nanotubes to the mixed solution, stirring and mixing to obtain a dopamine reaction solution;
[0013] S6, soaking the polyurethane sponge obtained in step S4 in the dopamine reaction solution, heating for reaction, and after the reaction is completed, taking out the polyurethane sponge and drying it to obtain a highly adaptable sponge for household products.
[0014] The present invention mixes natural crystal powder into the sponge. The infrared rays emitted by the natural crystal powder produce a unique and stable frequency, which can enhance the immune system, promote the rapid discharge of toxins from the body and increase the oxygen level. Since this special frequency is at the same vibration frequency as humans, it has the functions of reducing muscle tension, slowing down the heartbeat, relaxing breathing, increasing the body's oxygen content, releasing stress and improving sleep.
[0015] The present invention uses polyether polyol and toluene diisocyanate as reaction monomers, and prepares polyurethane sponge under the action of a foaming agent and a foam stabilizer. The present invention combines polyurethane sponge with halloysite nanotubes, and uses the flame retardancy of halloysite nanotubes to give polyurethane sponge incidental flame retardancy. The flame retardancy of polyurethane sponge is specifically achieved through two aspects: on the one hand, halloysite nanotubes are added during the reaction of polyether polyol and toluene diisocyanate, so that the polyurethane sponge is doped with halloysite nanotubes; on the other hand, a layer of halloysite nanotubes is combined on the surface of polyurethane. Through the synergistic effect of the two aspects, the polyurethane sponge has good flame retardancy.
[0016] In the process of combining the halloysite nanotubes on the polyurethane surface, the halloysite nanotubes are easily detached from the sponge surface by using a common soaking method. Therefore, the present invention utilizes the self-polymerization reaction of dopamine to adhere the halloysite nanotubes to the polyurethane sponge surface, thereby improving the binding force between the halloysite nanotubes and the polyurethane sponge surface and improving the problem that the halloysite nanotubes are easily detached from the sponge surface.
[0017] Preferably, the natural spar powder in step S1 is mixed with the following substances:
[0018] Fluorite powder, orange crystal calcite powder, graphite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, amethyst powder, rose quartz powder, aventurine powder, citrine powder, red jasper powder, serpentine powder and soda stone powder.
[0019] Preferably, in step S2, the mass ratio of dibutyltin diacetate to triethylamine is 1:(2-3).
[0020] Preferably, the amount of toluene diisocyanate added in step S3 is 40-60wt% of the polyether polyol in step S1.
[0021] Preferably, the heating and aging temperature in S4 is controlled at 60-70°C.
[0022] Preferably, the method for preparing the modified halloysite nanotubes in step S5 comprises the following steps:
[0023] The silane coupling agent KH560 is added to a mixed solution of ethanol and water, wherein the volume ratio of ethanol to water is 10:1, and then the halloysite nanotubes are added, heated to 50° C., stirred and reacted at a constant temperature for 2 hours, and centrifuged, washed and dried to obtain coupling agent-modified halloysite nanotubes;
[0024] The hyperbranched polyethyleneimine is added into water and stirred to dissolve to prepare a hyperbranched polyethyleneimine solution with a mass concentration of 0.5%. The coupling agent-modified halloysite nanotubes obtained above are added into the hyperbranched polyethyleneimine solution, heated for reaction, and subjected to centrifugal separation, washing, and drying to obtain modified halloysite nanotubes.
[0025] Another problem in the process of combining halloysite nanotubes with the polyurethane surface is that the halloysite nanotubes are randomly dispersed in the Tris buffer, and the halloysite nanotubes dispersed near the surface of the polyurethane sponge are insufficient to combine with polydopamine to form a halloysite nanotube flame retardant protective layer. Therefore, the present invention performs surface modification treatment on the halloysite nanotubes, first grafts epoxy groups on the surface of the halloysite nanotubes, and then uses the epoxy groups to react with the amino groups on the hyperbranched polyethyleneimine to graft the hyperbranched polyethyleneimine to the halloysite nanotubes, so that the surface of the halloysite nanotubes is loaded with a large number of amino groups, and the amino groups on the surface of the halloysite nanotubes and the amino groups on the polydopamine on the surface of the polyurethane sponge form hydrogen bond interaction forces, so that the surface of the polyurethane sponge is combined with more halloysite nanotubes, and then the halloysite nanotube flame retardant protective layer is formed.
[0026] Preferably, glutaraldehyde is also added to the mixed solution in step S5.
[0027] As described above, in the technical solution of the present invention, the self-polymerization reaction of dopamine is utilized to adhere halloysite nanotubes to the surface of polyurethane sponge, thereby improving the binding force between the halloysite nanotubes and the surface of polyurethane sponge, and improving the problem that the halloysite nanotubes are easily detached from the surface of sponge. However, the above method is only a certain degree of improvement on the problem that the halloysite nanotubes are easily detached from the surface of sponge, and cannot completely solve the problem that the halloysite nanotubes are detached from the surface of sponge. Therefore, in order to further improve the binding force between halloysite nano and the surface of sponge, the present invention adds glutaraldehyde to Tris buffer, and utilizes glutaraldehyde to cross-link the amino groups on the polydopamine with the amino groups on the surface of halloysite nanotubes, so that the halloysite nanotubes are firmly bonded to the surface of polyurethane sponge, and completely solves the problem that the halloysite nanotubes are detached from the surface of sponge.
[0028] Preferably, sodium alginate is also added to the second component in step S2.
[0029] In the technical solution of the present invention, as described above, the amino groups on the surface of the halloysite nanotubes and the amino groups on the polydopamine on the surface of the polyurethane sponge form hydrogen bond interaction forces, so that more halloysite nanotubes are combined with the surface of the polyurethane sponge, thereby forming a halloysite nanotube flame retardant protective layer. However, the density of the halloysite nanotube flame retardant protective layer is uneven, that is, a dense halloysite nanotube flame retardant protective layer is formed on one part of the sponge surface, and the other part is exposed, which has a certain impact on the flame retardant properties of the polyurethane sponge. In order to solve this problem, the present invention adds sodium alginate during the preparation of the polyurethane sponge, and the sodium alginate is evenly dispersed on the polyurethane sponge, so that the polyurethane sponge is loaded with COO - The amino groups on the surface of halloysite nanotubes are positively charged, and through electrostatic interaction, the halloysite nanotubes are evenly combined with the surface of the polyurethane sponge, thereby forming a uniform flame-retardant and dense protective layer of halloysite nanotubes on the surface of the polyurethane sponge, further improving the flame retardant properties of the polyurethane sponge.
[0030] Preferably, the added amount of sodium alginate is 0.3-0.6wt% of the mass of the polyether polyol.
[0031] A highly adaptable sponge for household items is prepared by the method described above.
[0032] The present invention has the following beneficial effects:
[0033] 1) Natural crystal powder is mixed into the sponge. The infrared rays emitted by the natural crystal powder produce a unique and stable frequency, which can enhance the immune system, promote the rapid discharge of toxins from the body and increase oxygen levels. Since this special frequency is at the same vibration frequency as humans, it has the functions of reducing muscle tension, slowing down the heartbeat, relaxing breathing, increasing the body's oxygen content, releasing stress and improving sleep.
[0034] 2) On the one hand, by adding halloysite nanotubes during the reaction of polyether polyol and toluene diisocyanate, the polyurethane sponge is doped with halloysite nanotubes; on the other hand, a layer of halloysite nanotubes is combined on the surface of polyurethane. Through the synergistic effect of the two aspects, the polyurethane sponge has better flame retardant properties;
[0035] 3) Surface modification of halloysite nanotubes is performed to load a large number of amino groups on the surface of the halloysite nanotubes. The amino groups on the surface of the halloysite nanotubes and the amino groups on the polydopamine on the surface of the polyurethane sponge form hydrogen bond interaction forces, so that more halloysite nanotubes are combined with the surface of the polyurethane sponge, thereby forming a flame retardant protective layer of the halloysite nanotubes;
[0036] 4) Glutaraldehyde is used to cross-link the amino groups on the polydopamine with the amino groups on the surface of the halloysite nanotubes, so that the halloysite nanotubes are firmly bonded to the surface of the polyurethane sponge, completely solving the problem of the halloysite nanotubes falling off the sponge surface;
[0037] 5) Sodium alginate is added during the preparation of the polyurethane sponge, and the halloysite nanotubes are evenly bonded to the surface of the polyurethane sponge through electrostatic interaction, thereby forming a uniform flame-retardant dense protective layer of halloysite nanotubes on the surface of the polyurethane sponge, further improving the flame retardant properties of the polyurethane sponge. DETAILED DESCRIPTION
[0038] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0039] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0040] Example 1
[0041] Preparation of modified halloysite nanotubes:
[0042] The silane coupling agent KH560 is added to a mixed solution of ethanol and water at a mass volume ratio of 1 g / 300 mL, wherein the volume ratio of ethanol to water is 10:1, and then the halloysite nanotubes are added, wherein the mass ratio of the halloysite nanotubes to the silane coupling agent KH560 is 1:0.2, and the mixture is heated to 50° C. and stirred for constant temperature reaction for 2 h, and then centrifuged, washed, and dried to obtain coupling agent-modified halloysite nanotubes;
[0043] Hyperbranched polyethyleneimine was added into water and stirred to dissolve to prepare a hyperbranched polyethyleneimine solution with a mass concentration of 0.5%. The coupling agent-modified halloysite nanotubes obtained above were added into the hyperbranched polyethyleneimine solution, heated to 80° C., and kept warm for 5 hours. After centrifugal separation, washing, and drying, modified halloysite nanotubes were obtained.
[0044] A method for preparing a highly adaptable sponge for household items comprises the following steps:
[0045] S1, uniformly mixing polyether polyol 330N with a molecular weight of 5000, halloysite nanotubes and natural spar powder, wherein the mass ratio of polyether polyol to halloysite nanotubes is 1:0.04, and the mass ratio of polyether polyol to natural spar powder is 1:0.06, to obtain a first component;
[0046] The natural spar powder is made by mixing the following materials in equal quantities:
[0047] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, amethyst powder, rose quartz powder, aventurine powder, citrine powder, red jasper powder, serpentine powder and soda stone powder;
[0048] S2, dibutyltin diacetate and triethylamine are uniformly mixed, the mass ratio of dibutyltin diacetate to triethylamine is 1:3, to obtain a composite catalyst, the mass of the composite catalyst is 0.3% of the mass of the polyether polyol, and then 10 times the mass of the composite catalyst of foaming agent water, 5 times the mass of the composite catalyst of foam stabilizer silicone oil and sodium alginate are added to the composite catalyst, the addition amount of sodium alginate is 0.5% of the mass of the polyether polyol, to obtain a second component;
[0049] S3, mixing the first component and the second component evenly to obtain a mixture, adding toluene diisocyanate to the mixture, wherein the amount of toluene diisocyanate added is 55wt% of the polyether polyol, stirring until foaming, and continuing stirring for 30s after foaming;
[0050] S4, heating the foamed organic matter at 70° C. for aging, wherein the aging time is controlled within 5 hours to obtain a polyurethane sponge;
[0051] S5, adding dopamine hydrochloride and glutaraldehyde to Tris buffer, the mass ratio of dopamine hydrochloride to Tris buffer is 1:2, the amount of glutaraldehyde added is 1.0wt% of dopamine hydrochloride, stirring and mixing to obtain a mixed solution, adding modified halloysite nanotubes to the mixed solution, the mass ratio of modified halloysite nanotubes to dopamine hydrochloride is 1:3, stirring and mixing to obtain a dopamine reaction solution;
[0052] S6, soaking the polyurethane sponge obtained in step S4 in the dopamine reaction solution, heating to 60°C, and keeping the temperature to react for 10 hours. After the reaction is completed, taking out the polyurethane sponge, placing it in a 50°C oven to dry for 8 hours, and obtaining a highly adaptable sponge for household products.
[0053] Example 2
[0054] Preparation of modified halloysite nanotubes:
[0055] The silane coupling agent KH560 is added to a mixed solution of ethanol and water at a mass volume ratio of 1 g / 300 mL, wherein the volume ratio of ethanol to water is 10:1, and then the halloysite nanotubes are added, wherein the mass ratio of the halloysite nanotubes to the silane coupling agent KH560 is 1:0.2, and the mixture is heated to 50° C. and stirred for constant temperature reaction for 2 h, and then centrifuged, washed, and dried to obtain coupling agent-modified halloysite nanotubes;
[0056] Hyperbranched polyethyleneimine was added into water and stirred to dissolve to prepare a hyperbranched polyethyleneimine solution with a mass concentration of 0.5%. The coupling agent-modified halloysite nanotubes obtained above were added into the hyperbranched polyethyleneimine solution, heated to 80° C., and kept warm for 5 hours. After centrifugal separation, washing, and drying, modified halloysite nanotubes were obtained.
[0057] A method for preparing a highly adaptable sponge for household items comprises the following steps:
[0058] S1, uniformly mixing polyether polyol 330N with a molecular weight of 5000, halloysite nanotubes and natural spar powder, wherein the mass ratio of polyether polyol to halloysite nanotubes is 1:0.03, and the mass ratio of polyether polyol to natural spar powder is 1:0.06, to obtain a first component;
[0059] The natural spar powder is made by mixing the following materials in equal quantities:
[0060] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, amethyst powder, rose quartz powder, aventurine powder, citrine powder, red jasper powder, serpentine powder and soda stone powder;
[0061] S2, dibutyltin diacetate and triethylamine are uniformly mixed, the mass ratio of dibutyltin diacetate to triethylamine is 1:2, to obtain a composite catalyst, the mass of the composite catalyst is 0.3% of the mass of the polyether polyol, and then 10 times the mass of the composite catalyst of foaming agent water, 5 times the mass of the composite catalyst of foam stabilizer silicone oil and sodium alginate are added to the composite catalyst, the addition amount of sodium alginate is 0.4% of the mass of the polyether polyol, to obtain a second component;
[0062] S3, mixing the first component and the second component evenly to obtain a mixture, adding toluene diisocyanate to the mixture, wherein the amount of toluene diisocyanate added is 45wt% of the polyether polyol, stirring until foaming, and continuing stirring for 30s after foaming;
[0063] S4, heating the foamed organic matter at 60° C. for aging, wherein the aging time is controlled within 5 hours to obtain a polyurethane sponge;
[0064] S5, adding dopamine hydrochloride and glutaraldehyde to Tris buffer, the mass ratio of dopamine hydrochloride to Tris buffer is 1:2, the amount of glutaraldehyde added is 1.0wt% of dopamine hydrochloride, stirring and mixing to obtain a mixed solution, adding modified halloysite nanotubes to the mixed solution, the mass ratio of modified halloysite nanotubes to dopamine hydrochloride is 1:3, stirring and mixing to obtain a dopamine reaction solution;
[0065] S6, soaking the polyurethane sponge obtained in step S4 in the dopamine reaction solution, heating to 60°C, and keeping the temperature to react for 10 hours. After the reaction is completed, taking out the polyurethane sponge, placing it in a 50°C oven to dry for 8 hours, and obtaining a highly adaptable sponge for household products.
[0066] Example 3
[0067] Preparation of modified halloysite nanotubes:
[0068] The silane coupling agent KH560 is added to a mixed solution of ethanol and water at a mass volume ratio of 1 g / 300 mL, wherein the volume ratio of ethanol to water is 10:1, and then the halloysite nanotubes are added, wherein the mass ratio of the halloysite nanotubes to the silane coupling agent KH560 is 1:0.2, and the mixture is heated to 50° C. and stirred for constant temperature reaction for 2 h, and then centrifuged, washed, and dried to obtain coupling agent-modified halloysite nanotubes;
[0069] Hyperbranched polyethyleneimine was added into water and stirred to dissolve to prepare a hyperbranched polyethyleneimine solution with a mass concentration of 0.5%. The coupling agent-modified halloysite nanotubes obtained above were added into the hyperbranched polyethyleneimine solution, heated to 80° C., and kept warm for 5 hours. After centrifugal separation, washing, and drying, modified halloysite nanotubes were obtained.
[0070] A method for preparing a highly adaptable sponge for household items comprises the following steps:
[0071] S1, uniformly mixing polyether polyol 330N with a molecular weight of 5000, halloysite nanotubes and natural spar powder, wherein the mass ratio of polyether polyol to halloysite nanotubes is 1:0.03, and the mass ratio of polyether polyol to natural spar powder is 1:0.06, to obtain a first component;
[0072] The natural spar powder is made by mixing the following materials in equal quantities:
[0073] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, amethyst powder, rose quartz powder, aventurine powder, citrine powder, red jasper powder, serpentine powder and soda stone powder;
[0074] S2, dibutyltin diacetate and triethylamine are uniformly mixed, the mass ratio of dibutyltin diacetate to triethylamine is 1:2.5, to obtain a composite catalyst, the mass of the composite catalyst is 0.3% of the mass of the polyether polyol, and then 10 times the mass of the composite catalyst, foam stabilizer silicone oil and sodium alginate are added to the composite catalyst, and the addition amount of sodium alginate is 0.45% of the mass of the polyether polyol, to obtain a second component;
[0075] S3, mixing the first component and the second component evenly to obtain a mixture, adding toluene diisocyanate to the mixture, wherein the amount of toluene diisocyanate added is 50wt% of the polyether polyol, stirring until foaming, and continuing stirring for 30s after foaming;
[0076] S4, heating the foamed organic matter at 65° C. for aging, wherein the aging time is controlled within 5 hours to obtain a polyurethane sponge;
[0077] S5, adding dopamine hydrochloride and glutaraldehyde to Tris buffer, the mass ratio of dopamine hydrochloride to Tris buffer is 1:2, the amount of glutaraldehyde added is 1.0wt% of dopamine hydrochloride, stirring and mixing to obtain a mixed solution, adding modified halloysite nanotubes to the mixed solution, the mass ratio of modified halloysite nanotubes to dopamine hydrochloride is 1:3, stirring and mixing to obtain a dopamine reaction solution;
[0078] S6, soaking the polyurethane sponge obtained in step S4 in the dopamine reaction solution, heating to 60°C, and keeping the temperature to react for 10 hours. After the reaction is completed, taking out the polyurethane sponge, placing it in a 50°C oven to dry for 8 hours, and obtaining a highly adaptable sponge for household products.
[0079] Example 4
[0080] Preparation of modified halloysite nanotubes:
[0081] The silane coupling agent KH560 is added to a mixed solution of ethanol and water at a mass volume ratio of 1 g / 300 mL, wherein the volume ratio of ethanol to water is 10:1, and then the halloysite nanotubes are added, wherein the mass ratio of the halloysite nanotubes to the silane coupling agent KH560 is 1:0.2, and the mixture is heated to 50° C. and stirred for constant temperature reaction for 2 h, and then centrifuged, washed, and dried to obtain coupling agent-modified halloysite nanotubes;
[0082] Hyperbranched polyethyleneimine was added into water and stirred to dissolve to prepare a hyperbranched polyethyleneimine solution with a mass concentration of 0.5%. The coupling agent-modified halloysite nanotubes obtained above were added into the hyperbranched polyethyleneimine solution, heated to 80° C., and kept warm for 5 hours. After centrifugal separation, washing, and drying, modified halloysite nanotubes were obtained.
[0083] A method for preparing a highly adaptable sponge for household items comprises the following steps:
[0084] S1, uniformly mixing polyether polyol 330N with a molecular weight of 5000, halloysite nanotubes and natural spar powder, wherein the mass ratio of polyether polyol to halloysite nanotubes is 1:0.05, and the mass ratio of polyether polyol to natural spar powder is 1:0.06, to obtain a first component;
[0085] The natural spar powder is made by mixing the following materials in equal quantities:
[0086] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, amethyst powder, rose quartz powder, aventurine powder, citrine powder, red jasper powder, serpentine powder and soda stone powder;
[0087] S2, dibutyltin diacetate and triethylamine are uniformly mixed, the mass ratio of dibutyltin diacetate to triethylamine is 1:3, to obtain a composite catalyst, the mass of the composite catalyst is 0.3% of the mass of the polyether polyol, and then 10 times the mass of the composite catalyst of foaming agent water, 5 times the mass of the composite catalyst of foam stabilizer silicone oil and sodium alginate are added to the composite catalyst, the addition amount of sodium alginate is 0.6% of the mass of the polyether polyol, to obtain a second component;
[0088] S3, mixing the first component and the second component evenly to obtain a mixture, adding toluene diisocyanate to the mixture, wherein the amount of toluene diisocyanate added is 60wt% of the polyether polyol, stirring until foaming, and continuing stirring for 30s after foaming;
[0089] S4, heating the foamed organic matter at 70° C. for aging, wherein the aging time is controlled within 5 hours to obtain a polyurethane sponge;
[0090] S5, adding dopamine hydrochloride and glutaraldehyde to Tris buffer, the mass ratio of dopamine hydrochloride to Tris buffer is 1:2, the amount of glutaraldehyde added is 1.0wt% of dopamine hydrochloride, stirring and mixing to obtain a mixed solution, adding modified halloysite nanotubes to the mixed solution, the mass ratio of modified halloysite nanotubes to dopamine hydrochloride is 1:3, stirring and mixing to obtain a dopamine reaction solution;
[0091] S6, soaking the polyurethane sponge obtained in step S4 in the dopamine reaction solution, heating to 60°C, and keeping the temperature to react for 10 hours. After the reaction is completed, taking out the polyurethane sponge, placing it in a 50°C oven to dry for 8 hours, and obtaining a highly adaptable sponge for household products.
[0092] Example 5
[0093] Preparation of modified halloysite nanotubes:
[0094] The silane coupling agent KH560 is added to a mixed solution of ethanol and water at a mass volume ratio of 1 g / 300 mL, wherein the volume ratio of ethanol to water is 10:1, and then the halloysite nanotubes are added, wherein the mass ratio of the halloysite nanotubes to the silane coupling agent KH560 is 1:0.2, and the mixture is heated to 50° C. and stirred for constant temperature reaction for 2 h, and then centrifuged, washed, and dried to obtain coupling agent-modified halloysite nanotubes;
[0095] Hyperbranched polyethyleneimine was added into water and stirred to dissolve to prepare a hyperbranched polyethyleneimine solution with a mass concentration of 0.5%. The coupling agent-modified halloysite nanotubes obtained above were added into the hyperbranched polyethyleneimine solution, heated to 80° C., and kept warm for 5 hours. After centrifugal separation, washing, and drying, modified halloysite nanotubes were obtained.
[0096] A method for preparing a highly adaptable sponge for household items comprises the following steps:
[0097] S1, uniformly mixing polyether polyol 330N with a molecular weight of 5000, halloysite nanotubes and natural spar powder, wherein the mass ratio of polyether polyol to halloysite nanotubes is 1:0.02, and the mass ratio of polyether polyol to natural spar powder is 1:0.06, to obtain a first component;
[0098] The natural spar powder is made by mixing the following materials in equal quantities:
[0099] Fluorite powder, orange crystal calcite powder, shungite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, amethyst powder, rose quartz powder, aventurine powder, citrine powder, red jasper powder, serpentine powder and soda stone powder;
[0100] S2, dibutyltin diacetate and triethylamine are uniformly mixed, the mass ratio of dibutyltin diacetate to triethylamine is 1:2, to obtain a composite catalyst, the mass of the composite catalyst is 0.3% of the mass of the polyether polyol, and then 10 times the mass of the composite catalyst of foaming agent water, 5 times the mass of the composite catalyst of foam stabilizer silicone oil and sodium alginate are added to the composite catalyst, the addition amount of sodium alginate is 0.3% of the mass of the polyether polyol, to obtain a second component;
[0101] S3, mixing the first component and the second component evenly to obtain a mixture, adding toluene diisocyanate to the mixture, wherein the amount of toluene diisocyanate added is 40wt% of the polyether polyol, stirring until foaming, and continuing stirring for 30s after foaming;
[0102] S4, heating the foamed organic matter at 60° C. for aging, wherein the aging time is controlled within 5 hours to obtain a polyurethane sponge;
[0103] S5, adding dopamine hydrochloride and glutaraldehyde to Tris buffer, the mass ratio of dopamine hydrochloride to Tris buffer is 1:2, the amount of glutaraldehyde added is 1.0wt% of dopamine hydrochloride, stirring and mixing to obtain a mixed solution, adding modified halloysite nanotubes to the mixed solution, the mass ratio of modified halloysite nanotubes to dopamine hydrochloride is 1:3, stirring and mixing to obtain a dopamine reaction solution;
[0104] S6, soaking the polyurethane sponge obtained in step S4 in the dopamine reaction solution, heating to 60°C, and keeping the temperature to react for 10 hours. After the reaction is completed, taking out the polyurethane sponge, placing it in a 50°C oven to dry for 8 hours, and obtaining a highly adaptable sponge for household products.
[0105] Comparative Example 1
[0106] The difference between Comparative Example 1 and Example 1 is that:
[0107] In step S5, dopamine hydrochloride is not added.
[0108] The remaining steps are the same as those in Example 1.
[0109] Comparative Example 2
[0110] The difference between Comparative Example 2 and Example 1 is:
[0111] The modified halloysite nanotubes were replaced with ordinary halloysite nanotubes.
[0112] The remaining steps are the same as those in Example 1.
[0113] Comparative Example 3
[0114] The difference between Comparative Example 3 and Example 1 is that:
[0115] In step S5, glutaraldehyde is not added.
[0116] The remaining steps are the same as those in Example 1.
[0117] Comparative Example 4
[0118] The difference between Comparative Example 4 and Example 1 is that:
[0119] In step S2, sodium alginate is not added.
[0120] The remaining steps are the same as those in Example 1.
[0121] Comparative Example 5
[0122] The difference between Comparative Example 5 and Example 1 is that:
[0123] In step S1, no natural spar powder is added.
[0124] The remaining steps are the same as those in Example 1.
[0125] Performance Testing
[0126] 1. Flame retardant performance test: According to GB / T8333-1987-2008 "Test Method for Combustion Performance of Foam Plastics", the flame retardant performance of polyurethane sponge was tested. The higher the oxygen index in the test results, the better the flame retardant performance of the sponge, and vice versa, the worse the flame retardant performance of the sponge. The test results are shown in Table 1:
[0127] Table 1
[0128]
[0129] 2. To test the bonding strength between the flame retardant Halloysite nanotubes on the sponge surface and the sponge, the sponges prepared in Examples 1, 3 and 5 and Comparative Examples 1 and 3 were placed in an ultrasonic oscillator filled with water and ultrasonically oscillated at a frequency of 20 KHz for 5 hours. The sponges were taken out and placed in an oven to dry at 50°C. Then, the flame retardant properties of the polyurethane sponge were determined according to the test method of GB / T8333-19872008 "Test Method for Combustion Performance of Foam Plastics". The better the flame retardant properties, the higher the bonding strength between the flame retardant Halloysite nanotubes on the sponge surface and the sponge, and the better the durability of the flame retardant properties of the sponge. The test results are shown in Table 2:
[0130] Table 2
[0131]
[0132] By comparing Table 1 and Table 2 (before and after ultrasonic vibration), it can be seen that the flame retardant properties of the polyurethane sponges prepared in Examples 1-5 remain almost unchanged after ultrasonic vibration, while the flame retardant properties of the polyurethane sponges in Comparative Examples 1 and 3 are significantly reduced after ultrasonic vibration. This proves that the polyurethane sponges prepared in the examples are more firmly combined with the flame retardant substance halloysite nanotubes, and have more durable flame retardant properties than Comparative Examples 1 and 3.
[0133] 3. The tensile strength of polyurethane sponge was tested according to GB / T6344-2008 "Determination of tensile strength and tensile elongation at break of soft foam polymeric materials". The rebound rate of polyurethane sponge was tested according to GB / T6670-2008 "Determination of rebound performance of soft foam polymeric materials by falling ball method". The test results are shown in Table 3:
[0134] Table 3
[0135]
[0136] The far-infrared release performance of the sponge was tested using the GB / T30127-2013 method. The test results are shown in Table 4:
[0137] Table 4
[0138]
[0139] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a highly adaptable sponge for household products, characterized in that: The following steps are involved: S1, uniformly mixing polyether polyol, halloysite nanotubes and natural spar powder to obtain a first component; S2, mixing dibutyltin diacetate and triethylamine uniformly to obtain a composite catalyst, and then adding foaming agent water, foam stabilizer silicone oil and sodium alginate to the composite catalyst to obtain a second component; S3, mixing the first component and the second component evenly to obtain a mixture, adding toluene diisocyanate to the mixture, and stirring until foaming; S4, heating the foamed organic matter for maturation to obtain a polyurethane sponge; S5, adding dopamine hydrochloride and glutaraldehyde to a Tris buffer, stirring and mixing to obtain a mixed solution, adding modified halloysite nanotubes to the mixed solution, stirring and mixing to obtain a dopamine reaction solution; S6, soaking the polyurethane sponge obtained in step S4 in the dopamine reaction solution, heating for reaction, and after the reaction is completed, taking out the polyurethane sponge and drying it to obtain a highly adaptable sponge for household products; Wherein, the preparation method of modified halloysite nanotubes in step S5 comprises the following steps: The silane coupling agent KH560 is added to a mixed solution of ethanol and water, wherein the volume ratio of ethanol to water is 10:1, and then the halloysite nanotubes are added, heated to 50° C., stirred and reacted at a constant temperature for 2 hours, and centrifuged, washed and dried to obtain coupling agent-modified halloysite nanotubes; The hyperbranched polyethyleneimine is added into water and stirred to dissolve to prepare a hyperbranched polyethyleneimine solution with a mass concentration of 0.5%. The coupling agent-modified halloysite nanotubes obtained above are added into the hyperbranched polyethyleneimine solution, heated for reaction, and subjected to centrifugal separation, washing, and drying to obtain modified halloysite nanotubes.
2. The method for preparing a highly adaptable sponge for household products according to claim 1, characterized in that: The natural spar powder in step S1 is prepared by mixing the following substances: Fluorite powder, orange crystal calcite powder, graphite powder, bloodstone powder, gypsum powder, aragonite powder, tourmaline powder, white crystal powder, amethyst powder, rose quartz powder, aventurine powder, citrine powder, red jasper powder, serpentine powder and soda stone powder.
3. The method for preparing a highly adaptable sponge for household products according to claim 1, characterized in that: In step S2, the mass ratio of dibutyltin diacetate to triethylamine is 1:(2-3).
4. The method for preparing a highly adaptable sponge for household products according to claim 1, characterized in that: The amount of toluene diisocyanate added in step S3 is 40-60wt% of the polyether polyol in step S1.
5. The method for preparing a highly adaptable sponge for household products according to claim 1, characterized in that: The heating and aging temperature in S4 is controlled at 60-70°C.
6. The method for preparing a highly adaptable sponge for household products according to claim 1, characterized in that: The added amount of the sodium alginate is 0.3-0.6wt% of the mass of the polyether polyol.
7. A highly adaptable sponge for household items, characterized in that: The method is prepared by any one of claims 1 to 6.