An oxygen-deficient Bi5O7I-loaded polytriazine imide composite material and its preparation method and application

Through the heterojunction structure of the oxygen-deficient Bi5O7I supported polytriazine imide composite material, the problem of selectivity and efficiency of photocatalytic materials in the degradation of PFOA is solved, and efficient selective enrichment and defluorination of PFOA is achieved. Suitable for the treatment of complex water bodies.

CN118491540BActive Publication Date: 2024-10-18TONGJI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410953849.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-18
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Existing photocatalytic materials have problems with poor selectivity and low degradation efficiency when degrading perfluorooctanoic acid (PFOA). In particular, due to the polarity difference and mismatched energy band structure of semiconductor materials, the defluorination effect of PFOA is poor.

Method used

Develop an oxygen-deficient Bi5O7I-loaded polytriazineimide composite material. The spherical Bi5O7I is used as a carrier and combined with abundant amine-based polytriazineimide to form a binary heterojunction structure to improve the selectivity for PFOA. Adsorption and efficient degradation capabilities.

Benefits of technology

It achieves rapid photocatalytic degradation and defluorination of PFOA under simulated sunlight conditions, significantly improves the degradation ability of trace amounts of PFOA, and remains efficient in the presence of high salt and organic matter, making it suitable for the treatment of complex actual water systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118491540B_ABST
    Figure CN118491540B_ABST
Patent Text Reader

Abstract

The present invention discloses an oxygen-deficient Bi5O7I-loaded polytriazineimide composite material, and a preparation method and application thereof. The present invention reduces part of the bismuth-structured oxygen vacancies in Bi5O7I by a solvothermal method, and further calcines it to form a heterojunction with PTI, while increasing the oxygen vacancy density. The PTI in the present invention is prepared by calcining a mixture of melamine and a eutectic salt under anaerobic conditions. The oxygen-deficient Bi5O7I-loaded polytriazineimide composite material achieves selective enrichment of organic fluorine through abundant amino groups on the surface. Under the excitation of simulated sunlight, the material simultaneously reduces and oxidizes perfluorooctanoic acid, greatly improving the degradation and defluorination efficiency of perfluorooctanoic acid. The selective enrichment and efficient degradation capabilities make the material highly active for perfluorooctanoic acid in actual wastewater and municipal sludge, reflecting the broad application prospects of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of environmental pollution control, and in particular to an oxygen-deficient Bi5O7I-loaded polytriazine imide composite material and a preparation method and application thereof. Background Art

[0002] Perfluoroalkyl and polyfluoroalkyl substances (PFAS) are a class of man-made compounds that exhibit excellent thermal and chemical stability due to their large number of high-energy CF bonds (485 kJ / mol). This chemical stability has led to their widespread use in industrial applications, but it has also led to the widespread presence of PFAS in environmental media around the world, posing significant environmental risks. Perfluorooctanoic acid (PFOA) is one of the most representative substances among PFAS and is widely present in surface water and groundwater around the world. In recent years, PFOA removal technology has attracted a lot of research interest. Although existing technologies have been applied, it remains challenging to find more efficient and environmentally friendly methods.

[0003] Photocatalysis has been demonstrated to be an environmentally friendly technology with the potential to degrade PFOA using renewable solar energy. Although a variety of photocatalytic materials have been widely used in the study of PFAS pollution control, their degradation efficiency still needs to be improved. Due to the negative impact of the perfluorination effect on electron transfer, the PFOA degradation performance of typical semiconductor photocatalysts is largely suppressed, which greatly limits the application of photocatalysis in the field of PFOA purification. Although traditional inorganic semiconductor catalysts can meet the requirements of the band structure, they usually have poor affinity for organic fluorine due to the difference in polarity between the two. On the other hand, although organic semiconductors have a strong affinity for organic fluorine and can capture PFOA on the surface of the material, their photocatalytic performance is poor due to the mismatched band structure and inherent wide band gap.

[0004] Therefore, the key to solving the PFOA pollution problem is to develop new photocatalytic materials that have both PFOA affinity and efficient degradation capabilities by combining organic and inorganic semiconductors. In the reported patents on bismuth iodide-based composite materials (patent publication numbers CN 118002208 A, CN 117983253 A), the materials have shown strong PFOA degradation capabilities, but due to their polarity differences, the materials have poor defluorination effects on PFOA. In response to this technical problem, the present invention aims to develop a new method that can achieve selective enrichment and efficient degradation and defluorination of PFOA, and apply it to the degradation of PFOA in actual wastewater by simulated sunlight. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an oxygen-deficient Bi5O7I-loaded polytriazineimide composite material and its preparation method and application. The photocatalytic composite material provided by the present invention not only has the ability to selectively enrich PFOA, but also can achieve efficient degradation and defluorination of PFOA, and is successfully applied for the first time to catalytically degrade perfluorooctanoic acid in actual wastewater under simulated sunlight conditions.

[0006] The first object of the present invention is to provide an oxygen-deficient Bi5O7I-loaded polytriazineimide composite material as a flower ball-loaded fiber structure, wherein the oxygen-deficient Bi5O7I-loaded polytriazineimide composite material uses flower ball-shaped Bi5O7I as a carrier, and there are a large number of oxygen vacancies on the surface of the flower ball-shaped Bi5O7I. At the same time, polytriazineimide with rich amino groups is loaded on the surface of the flower ball-shaped Bi5O7I material.

[0007] The oxygen-deficient Bi5O7I-loaded polytriazineimide composite material (composite material PTI / Bi / Bi5O7I photocatalyst) provided by the present invention is a binary heterojunction oxygen-deficient Bi5O7I-loaded polytriazineimide (PTI / Bi / Bi5O7I) composite photocatalytic material derived from flower-ball-shaped Bi5O7I as a carrier. The composite photocatalytic material has excellent selective adsorption capacity for PFOA, good simulated sunlight absorption capacity, high surface charge transfer rate and photogenerated carrier separation efficiency, thereby achieving excellent photocatalytic degradation efficiency, and can be used for rapid photocatalytic degradation and defluorination of ultra-trace PFOA in complex actual water systems.

[0008] In some embodiments of the present invention, the loading amount of the polytriazine imide is 10 wt % to 30 wt %.

[0009] The second object of the present invention is to provide a method for preparing the oxygen-deficient Bi5O7I-loaded polytriazine imide composite material, comprising the following steps:

[0010] Providing a polytriazine imide material;

[0011] dissolving a bismuth source in ethylene glycol to obtain a bismuth source solution;

[0012] dissolving an iodine source in ethylene glycol to obtain an iodine source solution;

[0013] The iodine source solution is added to the bismuth source solution and stirred for reaction, the polytriazine imide material is added and stirred, and then a solvent thermal reaction is carried out, and the solid material obtained by the reaction is calcined to obtain the oxygen-deficient Bi5O7I-loaded polytriazine imide composite material.

[0014] In some embodiments of the present invention, the polytriazine imide material is obtained by mixing and reacting a eutectic salt mixture with melamine;

[0015] The eutectic salt mixture is lithium chloride and potassium chloride; specifically, mixing means grinding the eutectic salt mixture and melamine together in a mortar until the mixture becomes a fine powder.

[0016] The molar ratio of lithium chloride, potassium chloride and melamine is (13-14): (16-17): 1;

[0017] The conditions of the mixed reaction are as follows: after being fully and evenly ground, heating at 550-600°C for 4-5 h in an inert atmosphere at a heating rate of 2-3°C / min.

[0018] In some embodiments of the present invention, the bismuth source is selected from Bi(NO3)3·5H2O; and the concentration of the bismuth source solution is 70-80 g / L.

[0019] In some embodiments of the present invention, the iodine source is selected from KI; and the concentration of the iodine source solution is 20-30 g / L.

[0020] In some embodiments of the present invention, the molar ratio of the bismuth source to the iodine source is (0.75~1):1.

[0021] In some embodiments of the present invention, the polytriazine imide material accounts for 10 wt % to 30 wt % of the total mass of the solvent thermal reaction product.

[0022] The conditions of the solvent thermal reaction are: reaction at 160-180°C for 6-8 hours; the solvent thermal reaction is carried out in a high-pressure reactor lined with polytetrafluoroethylene.

[0023] The calcination conditions are as follows: a heating rate of 2-4°C / min, a calcination temperature of 480-500°C, and a calcination time of 1-2 h. The calcination reaction is carried out in a muffle furnace.

[0024] In some embodiments of the present invention, the generation of the solid material further comprises washing and drying the solid material, wherein the washing and drying both refer to washing with deionized water and ethanol, and drying at 50-80° C. overnight.

[0025] The third object of the present invention is to provide the use of the oxygen-deficient Bi5O7I-loaded polytriazine imide composite material in the photocatalytic degradation of perfluorooctanoic acid.

[0026] In some embodiments of the present invention, the photocatalytic degradation method is as follows: the pH value of the perfluorooctanoic acid solution is adjusted to 2-4, the oxygen-deficient Bi5O7I-loaded polytriazine imide composite material is added, and the reaction is carried out for 30-60 minutes under dark conditions to reach adsorption equilibrium, and then the reaction is carried out under simulated sunlight conditions with a wavelength of 320 nm-2500 nm for more than 3 hours.

[0027] Specifically, the prepared oxygen-deficient Bi5O7I-loaded polytriazine imide composite material was used as a photocatalyst, and 0.5 g·L -1 PTI / Bi / Bi5O7I was added to the -1 PFOA was degraded in an aqueous solution of PFOA under simulated sunlight conditions, and PFOA and its intermediates were quantitatively detected and qualitatively screened using ultra-performance liquid chromatography (UPLC) and ultra-performance liquid chromatography-quadrupole time-of-flight mass spectrometry (Q-TOF-MS), respectively.

[0028] In order to explore the effects of other substances in actual wastewater and municipal sludge extract on the prepared oxygen-deficient Bi5O7I-loaded polytriazineimide composites, 0.5 g·L -1 The PTI / Bi / Bi5O7I was added to the actual wastewater and municipal sludge extract without any pretreatment, and PFOA was degraded under simulated sunlight conditions. The concentrations of PFOA and fluoride ions were quantitatively detected by ultra-performance liquid chromatography (UPLC) and ion chromatography (IC), respectively.

[0029] In some embodiments of the present invention, when treating PFOA-containing water, wastewater and sludge extract, the dosage of the oxygen-deficient Bi5O7I-loaded polytriazine imide composite material includes but is not limited to 0.2-1.25 g·L -1 .

[0030] In some embodiments of the present invention, when treating water, wastewater and sludge extract containing PFOA, the concentration of PFOA can be as low as 3.02 µg·L -1 Ultra trace levels.

[0031] Preferably, when the material is used to treat wastewater and sludge extract containing PFOA, the high salt and organic matter in the wastewater will not have a significant effect on the degradation of PFOA by the oxygen-deficient Bi5O7I-loaded polytriazine imide composite material.

[0032] The present invention discloses an oxygen-deficient Bi5O7I-loaded polytriazine imide composite photocatalyst, and applies it for the first time to the catalytic degradation of PFOA in water by simulated sunlight, which not only solves the problem of mismatched energy band structures of organic semiconductor catalysts and poor affinity of inorganic semiconductors, but also provides new insights into the design of composite photocatalytic materials.

[0033] The present invention found that even in the presence of high concentrations of salt and organic matter, the abundant secondary amine groups in the oxygen-deficient Bi5O7I-loaded polytriazine imide composite material will interact with the carboxyl groups in PFOA, causing it to be selectively enriched on the surface of the composite material, as a precondition for the subsequent in-situ photocatalytic reaction. Subsequently, under the irradiation of simulated sunlight, the conduction band and valence band of Bi / Bi5O7I are higher than those of PTI, so the electrons on the conduction band of Bi / Bi5O7I flow into PTI, while the holes on PTI are enriched on the valence band surface of Bi / Bi5O7I, achieving effective separation of photogenerated electron-hole pairs, thereby enhancing the photocatalytic activity of the material.

[0034] The above technical solution of the present invention has the following advantages compared with the prior art:

[0035] 1. The present invention combines the advantages of organic semiconductors and inorganic semiconductors, greatly improving the ability to degrade trace amounts of PFOA in environmental water.

[0036] 2. The present invention increases the oxygen vacancy density in the material by combining a solvent thermal method and a calcination method, thereby greatly improving the surface exciton yield and the electron transmission capacity.

[0037] 3. The heterojunction constructed in the present invention can greatly improve the separation efficiency of photogenerated carriers and extend the life of photogenerated carriers.

[0038] 4. The present invention is the first to use oxygen-deficient Bi5O7I-loaded polytriazineimide composite materials for the rapid photocatalytic degradation of perfluorooctanoic acid in water under simulated sunlight. It can also achieve efficient degradation and defluorination of trace PFOA in municipal wastewater and sludge extracts, providing a technical reference for the design of heterojunction photocatalytic materials and reflecting the prospects for practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0040] Figure 1 This is a SEM characterization image of the composite material PTI / Bi / Bi5O7I photocatalyst prepared in Example 1 of the present invention.

[0041] Figure 2 XRD characterization diagrams of the composite material PTI / Bi / Bi5O7I photocatalyst prepared in Example 1 of the present invention, the PTI obtained in Comparative Example 1, the Bi5O7I obtained in Comparative Example 3, and the Bi / Bi5O7I obtained in Comparative Example 2.

[0042] Figure 3The XPS characterization diagram of the composite material PTI / Bi / Bi5O7I photocatalyst prepared in Example 1 of the present invention. Among them, a is the XPS spectrum diagram; b is the two sharp peaks at 617.1eV and 632.1eV and the I in the synthetic material - Corresponding; c is N 1s located at 398.8 eV and 401 eV. The two peaks are respectively attributed to C─N═C in the ring nitrogen and the terminal -NH x group; d is the three combined peaks located at 292.5, 287.7 and 284.8 eV, corresponding to O─C═O, N─C═N and sp 3 C; e is O 1s with three combined peaks; f is the corrected Bi 4f spectrum.

[0043] Figure 4 This is a comparison chart of the removal rate curves of PFOA by the composite material PTI / Bi / Bi5O7I photocatalyst prepared in Example 1 of the present invention, the PTI prepared in Comparative Example 1, and the Bi / Bi5O7I prepared in Comparative Example 2.

[0044] Figure 5 This is a comparison chart of the PFOA removal rate and defluorination rate of the composite material PTI / Bi / Bi5O7I photocatalyst prepared in Example 1 of the present invention in municipal wastewater and municipal sludge extract. DETAILED DESCRIPTION

[0045] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0046] The processes and methods not described in detail in the following examples are conventional methods known in the art, and the reagents used in the examples are all analytically pure or chemically pure and can be purchased commercially or prepared by methods well known to those skilled in the art. The following examples all achieve the purpose of the present invention.

[0047] Example 1

[0048] The eutectic salt mixture LiCl (4.52 g) and KCl (10 g) and melamine (1 g) were poured into a mortar and ground together for 30 min until the mixture became a fine powder. The mixture was then transferred to a magnetic boat and heated under a nitrogen atmosphere (flow rate of 20 cm 3 / min) in a tube furnace at 550 °C for 4 h, with a heating rate of 2.3 °C / min. It was washed with 500 mL of hot water at 80 °C for 12 h to remove the incompletely reacted salts, and the solid product was filtered out. Finally, the solid product obtained by filtration was washed with ultrapure water and ethanol three times each, and dried in air at 80 °C overnight to obtain PTI.

[0049] 2.91 g of Bi(NO3)3⋅5H2O was completely dissolved in 40 mL of ethylene glycol and stirred for 30 minutes to obtain an ethylene glycol solution of Bi(NO3)3. 1.0 g of KI was added to 40 mL of ethylene glycol and stirred until completely dissolved. It was slowly added dropwise to the vigorously stirred ethylene glycol solution of Bi(NO3)3 and stirred for 30 minutes until the mixed solution became an orange-yellow clear liquid. 0.4 g of PTI was added and stirred for 30 minutes. The mixture was sealed in a 100 mL high-pressure reactor lined with polytetrafluoroethylene and kept at 180 °C for 6 h. Then it was naturally cooled to room temperature. The reaction samples were washed three times with ultrapure water and ethanol respectively. Finally, it was dried at 80 °C overnight. The dried sample was then calcined at 500 °C for 1 h (heating rate of 3 °C / min) to obtain a composite material PTI / Bi / Bi5O7I photocatalyst with a PTI content of 25%. The structure of the obtained composite material PTI / Bi / Bi5O7I (25%) was characterized and the results are shown in Figure 2-3 .

[0050] Figure 3 This is the XPS characterization diagram of the composite material PTI / Bi / Bi5O7I photocatalyst prepared in Example 1. Figure 3 As shown in (a), the XPS spectrum can clearly show the chemical states of the elements contained in the synthesized material, including the signals of Bi, O, I, C and N elements. All XPS data were calibrated using the C 1s band energy. Figure 3 As shown in (b), the two sharp peaks at 617.1 and 632.1 eV correspond to the I - Corresponding. Figure 3 The N 1s peaks of c in the middle are located at 398.8 and 401 eV, which are respectively attributed to the C─N═C in the ring nitrogen and the terminal -NH x The absence of the corresponding signal peak of NC3 in the N 1s spectrum proves that the basic unit of PTI is a triazine ring with abundant secondary amine structures. Figure 3 As shown in (d), the three combined peaks at 292.5, 287.7, and 284.8 eV correspond to O─C═O, N─C═N, and sp 3 C. Figure 3 As shown in (e), O 1s has three binding peaks, and the three peaks near 528.9, 530.3 and 532.2 eV correspond to Bi-O bonds, oxygen defects and OH bonds, respectively. Figure 3 f is the corrected Bi 4f spectrum, which includes peaks at 164 eV and 157.5 eV, corresponding to the trivalent oxidation state Bi 4f 7 / 2 and Bi 4f 5 / 2 Bi-state signal at 164.0eV and 157.5eV3+ The reduction peak proves the existence of 3+ The transformation process to metallic Bi.

[0051] Example 2

[0052] The eutectic salt mixture LiCl (4.7 g) and KCl (9.61 g) and melamine (1 g) were poured into a mortar and ground together for 30 min until the mixture became a fine powder. The mixture was then transferred to a magnetic boat and heated under a nitrogen atmosphere (flow rate of 20 cm 3 / min) in a tube furnace at 580 °C for 4 h, with a heating rate of 2.5 °C / min. It was washed with 500 mL of hot water at 80 °C for 12 h to remove the incompletely reacted salts, and the solid product was filtered out. Finally, the solid product obtained by filtration was washed with ultrapure water and ethanol three times each, and dried in air at 80 °C overnight to obtain PTI.

[0053] 2.91 g of Bi(NO3)3⋅5H2O was completely dissolved in 40 mL of ethylene glycol and stirred for 30 minutes to obtain a Bi(NO3)3 ethylene glycol solution. 1.0 g of KI was added to 40 mL of ethylene glycol and stirred until completely dissolved. It was slowly added dropwise to the vigorously stirred Bi(NO3)3 ethylene glycol solution and stirred for 30 minutes until the mixed solution became an orange-yellow clear liquid. 0.24 g of PTI was added and stirred for 30 minutes. The mixture was sealed in a 100 mL polytetrafluoroethylene-lined autoclave and kept at 160°C for 6 h. Then it was naturally cooled to room temperature. The reaction samples were washed three times with ultrapure water and ethanol respectively. Finally, it was dried at 60°C overnight. The dried sample was then calcined at 480°C for 1 h (heating rate of 3°C / min) to obtain a composite material PTI / Bi / Bi5O7I photocatalyst with a PTI content of 15%.

[0054] Example 3

[0055] The eutectic salt mixture LiCl (4.41 g) and KCl (10.13 g) and melamine (1 g) were poured into a mortar and ground together for 30 min until the mixture became a fine powder. The mixture was then transferred to a magnetic boat and heated under a nitrogen atmosphere (flow rate of 20 cm 3 The reaction mixture was heated at 550 °C for 4 h in a tube furnace at 400 °C / min (3 °C / min). The reaction mixture was washed with 500 mL of hot water at 80 °C for 12 h to remove the incompletely reacted salts, and the solid product was filtered off. The solid product was washed with ultrapure water and ethanol three times each, and dried in air at 60 °C overnight to obtain PTI.

[0056] 2.91 g of Bi(NO3)3⋅5H2O was completely dissolved in 40 mL of ethylene glycol and stirred for 30 minutes to obtain an ethylene glycol solution of Bi(NO3)3. 1.0 g of KI was added to 40 mL of ethylene glycol and stirred until completely dissolved. It was slowly added dropwise to the vigorously stirred ethylene glycol solution of Bi(NO3)3 and stirred for 30 minutes until the mixed solution became an orange-yellow clear liquid. Then 0.48 g of PTI was added and stirred for 30 minutes. The mixture was sealed in a 100 mL high-pressure reactor lined with polytetrafluoroethylene and kept at 180°C for 6 h. Then it was naturally cooled to room temperature. The samples obtained by the reaction were washed three times with ultrapure water and ethanol respectively. Finally, it was dried at 80°C overnight. After that, the dried sample was calcined at 480°C for 1 h (heating rate of 3°C / min) to obtain a composite material PTI / Bi / Bi5O7I photocatalyst with a PTI content of 30%.

[0057] Comparative Example 1

[0058] The eutectic salt mixture LiCl (4.52 g) and KCl (10 g) and melamine (1 g) were poured into a mortar and ground together for 30 min until the mixture became a fine powder. The mixture was then transferred to a magnetic boat and heated under a nitrogen atmosphere (flow rate of 20 cm 3 The reaction mixture was heated at 550 °C for 4 h in a tube furnace at 400 °C / min (100 °C / min) with a heating rate of 2.3 °C / min. The mixture was washed with 500 mL of hot water at 80 °C for 48 h to remove the incompletely reacted salts, and the solid product was filtered out. Finally, the solid product obtained by filtration was washed with ultrapure water and ethanol three times each, and dried in air at 80 °C overnight to obtain PTI.

[0059] Comparative Example 2

[0060] 2.91 g of Bi(NO3)3⋅5H2O was completely dissolved in 40 mL of ethylene glycol and magnetically stirred for 30 minutes to obtain an ethylene glycol solution of Bi(NO3)3. 1.0 g of KI was added to 40 mL of ethylene glycol and stirred until completely dissolved. It was slowly added dropwise to the vigorously stirred ethylene glycol solution of Bi(NO3)3 and stirred for 30 minutes until the mixed solution became an orange-yellow clear liquid. The mixed solution was sealed in a 100 mL polytetrafluoroethylene-lined autoclave and kept at 180 °C for 6 h, then cooled naturally to room temperature, and the reaction samples were washed three times with ultrapure water and ethanol respectively. Finally, it was dried at 80 °C overnight. The dried sample was then calcined at 500 °C for 1 h (heating rate of 3 °C / min) to obtain Bi / Bi5O7I.

[0061] Comparative Example 3

[0062] 2.19 g of Bi(NO3)3⋅5H2O was dissolved in 60 mL of deionized water and stirred until completely dissolved. 1.0 g of KI was added to the aqueous solution and stirred for 30 minutes. The mixed solution was sealed in a 100 mL polytetrafluoroethylene-lined autoclave and kept at 180 °C for 6 h, then naturally cooled to room temperature. The sample obtained by the reaction was washed three times with ultrapure water and ethanol respectively and dried at 60 °C overnight. The dried sample was then calcined at 500 °C for 1 h (heating rate of 3 °C / min) to obtain Bi5O7I. (Because there is no process of producing oxygen vacancies by reducing Bi in this comparative example, the amount of Bi(NO3)3⋅5H2O is different, and ethylene glycol is not required as a reducing agent.)

[0063] The composite material PTI / Bi / Bi5O7I photocatalyst obtained in Example 1 and the PTI and Bi / Bi5O7I and Bi5O7I materials obtained in Comparative Examples 1-3 were characterized by scanning electron microscopy and X-ray diffraction. The results are as follows: Figure 1 and Figure 2 shown.

[0064] Figure 1 The scanning electron microscope image of the composite material PTI / Bi / Bi5O7I photocatalyst obtained in Example 1 is shown, from which the combination of fibrous PTI and flower ball-shaped Bi / Bi5O7I can be clearly observed.

[0065] Figure 2 The XRD patterns of PTI, Bi5O7I, Bi / Bi5O7I and composite PTI / Bi / Bi5O7I photocatalysts are shown respectively. The characteristic peaks at 2θ = 30.2°, 31.9°, 32.8°, 45.8° and 56.7° are attributed to Bi5O7I (ICDD certificate number PDF#38-0669). The characteristic peaks at 2θ = 12.2° and 26.8° are attributed to polytriazine imide. At the same time, the XRD pattern of partial bismuth reduction (Bi / Bi5O7I) shows characteristic peaks at 2θ = 24.1°, 35.8° and 39.4°, which are attributed to metallic element Bi (PDF#44-1246). The characteristic diffraction peaks of PTI, Bi and Bi5O7I can be clearly observed in the XRD pattern of the composite PTI / Bi / Bi5O7I, among which the diffraction peak intensity of Bi5O7I is the highest.

[0066] The results of SEM and XRD showed that PTI and Bi / Bi5O7I were successfully combined, which meant the successful synthesis of heterojunction composite materials.

[0067] Performance Testing

[0068] In order to investigate the photocatalytic activity of the materials prepared in Example 1 and Comparative Examples 1-3, PFOA was used as the target. The catalytic performance of the composite photocatalyst was evaluated on a CEL-HXF300 photocatalytic device (Beijing Zhongjiao Jinyuan Scientific Instrument Co., Ltd., China), which was used to perform photocatalytic degradation of PFOA under simulated sunlight conditions under the irradiation of a xenon lamp with a wavelength of 320 nm-2500 nm. In each degradation experiment, 0.5 g·L -1 The catalyst was added to 50 mL of PFOA ultrapure water solution (30 mg·L -1 ), and reacted in dark conditions for 30 minutes before turning on the light to reach adsorption-desorption equilibrium. After the dark reaction was completed, 2 mL of the reaction suspension was taken out from the reaction vessel each time at a given interval and filtered with a 0.22 μm filter membrane. The residual PFOA and intermediate degradation products in the filtrate were detected by ultra-high phase liquid chromatography (Premier UPLC, Waters) coupled with its tandem quadrupole time-of-flight mass spectrometry (UPLC / Q-TOF-MS) (Impact Ⅱ, Bruker). The fluoride ion concentration in the filtrate was measured using an ion chromatograph (ICS-5000, Dionex), and the experimental results are shown in Figure 4 .

[0069] Figure 4 The degradation performance of the catalyst synthesized under simulated sunlight on PFOA was demonstrated. During the 30-minute adsorption process, both PTI and the composite PTI / Bi / Bi5O7I photocatalysts showed significant adsorption capacity for PFOA, further proving that the selective enrichment ability of the composite PTI / Bi / Bi5O7I photocatalyst for PFOA was dominated by PTI. With the increase of illumination time, the composite PTI / Bi / Bi5O7I photocatalyst showed excellent degradation ability for PFOA. The rate constant was calculated by the first-order kinetic equation ln(C0 / C t ) = K t , where K is the first-order rate constant, C0, C t are the concentrations of PFOA at reaction time 0 h and th, respectively. The composite PTI / Bi / Bi5O7I photocatalyst obtained in Example 1 exhibits the highest degradation rate constant (K = 2.96), which is 5.02 times that of Bi / Bi5O7I (K = 0.59) and 3.44 times that of PTI (K = 0.86). This indicates that the photocatalytic activity of the composite PTI / Bi / Bi5O7I photocatalyst is significantly improved by the heterogeneous structure.

[0070] In order to verify the photocatalytic degradation and defluorination effect of the composite material PTI / Bi / Bi5O7I prepared in Example 1 on PFOA in actual wastewater and municipal sludge extract, the prepared oxygen-deficient Bi5O7I-loaded polytriazine imide composite material was used as a photocatalyst. 0.5 g·L -1 The composite material PTI / Bi / Bi5O7I photocatalyst was added to the actual wastewater and municipal sludge extract without any pretreatment, and PFOA was degraded under simulated sunlight. The concentrations of PFOA and fluoride ions were quantitatively detected by ultra-high performance liquid chromatography (UPLC) and ion chromatography (IC). Table 1 shows the concentrations of anions, cations, organic matter (TOC) and PFOA in the actual wastewater and municipal sludge extract. The experimental results are shown in Figure 5 .

[0071] Table 1 Concentrations of different anions, cations, TOC and PFOA in municipal wastewater and municipal sludge extracts

[0072]

[0073] like Figure 5 As shown, even in actual industrial wastewater and municipal sludge extract, the composite material PTI / Bi / Bi5O7I still exhibits excellent degradation (96.45%, 99.01%) and defluorination capabilities (71.41%, 68.33%) for PFOA. It can be found in Table 1 that the concentrations of organic matter and salt in the two actual waters far exceed the concentration of PFOA, up to 41,000 times, reflecting that the composite material PTI / Bi / Bi5O7I photocatalyst still exhibits a strong photocatalytic degradation ability for PFOA even in the presence of high concentrations of salt and organic matter, proving that the composite material PTI / Bi / Bi5O7I photocatalyst is not affected by high concentrations of salt and organic matter, and exhibits a strong selectivity for PFOA.

[0074] The present invention provides a novel PTI / Bi / Bi5O7I composite material, which can realize the selective enrichment and efficient degradation and defluorination of PFOA, and provides an effective technical means for solving the PFOA pollution problem.

[0075] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. An oxygen-deficient Bi 5 O 7 I loaded polytriazine imide composite material, It is characterized in that The oxygen-deficient Bi 5 O 7 I-loaded polytriazine imide composite material is a flower ball-like loaded fiber structure, and the flower ball-like Bi 5 O 7 I is a carrier, in the flower ball-shaped Bi 5 O 7 There are a lot of oxygen vacancies on the surface of I. 5 O 7 The surface of material I is loaded with polytriazineimide having abundant amine groups.

2. The oxygen-deficient Bi according to claim 1 5 O 7 I loaded polytriazine imide composite material, It is characterized in that The loading amount of the polytriazine imide is 10wt%-30wt%.

3. The oxygen-deficient Bi according to claim 1 or 2 5 O 7 I Preparation method of loaded polytriazine imide composite material, It is characterized in that The following steps are involved: Provide a polytriazine imide material; dissolving a bismuth source in ethylene glycol to obtain a bismuth source solution; dissolving an iodine source in ethylene glycol to obtain an iodine source solution; The iodine source solution is added to the bismuth source solution and stirred for reaction, the polytriazine imide material is added and stirred, and then a solvent thermal reaction is performed, and the solid material obtained by the reaction is calcined to obtain the oxygen-deficient Bi 5 O 7 I-loaded polytriazineimide composite material.

4. The preparation method according to claim 3, It is characterized in that The polytriazine imide material is obtained by mixing and reacting a eutectic salt mixture with melamine; The eutectic salt mixture is lithium chloride and potassium chloride; The molar ratio of lithium chloride, potassium chloride and melamine is (13-14): (16-17): 1; The conditions of the mixed reaction are as follows: after being fully ground and uniformly mixed, the mixture is heated at 550-600°C for 4-5 h in an inert atmosphere at a heating rate of 2-3°C / min.

5. The preparation method according to claim 3, It is characterized in that The bismuth source is selected from Bi(NO 3 ) 3 ·5H 2 O; the concentration of the bismuth source solution is 70~80 g / L.

6. The preparation method according to claim 3, It is characterized in that The iodine source is selected from KI; the concentration of the iodine source solution is 20-30 g / L.

7. The preparation method according to claim 3, It is characterized in that The molar ratio of the bismuth source to the iodine source is (0.75-1):

1.

8. The preparation method according to claim 3, It is characterized in that The polytriazine imide material accounts for 10wt% to 30wt% of the total mass of the solvent thermal reaction product; The conditions of the solvothermal reaction are: 160-180°C for 6-8 h; The calcination conditions are as follows: a heating rate of 2-4 °C / min, a calcination temperature of 480-500 °C, and a calcination time of 1-2 h.

9. The oxygen-deficient Bi according to claim 1 or 2 5 O 7 Application of I-loaded polytriazineimide composite materials in photocatalytic degradation of perfluorooctanoic acid.

10. The use according to claim 9, It is characterized in that The photocatalytic degradation method comprises adjusting the pH value of the perfluorooctanoic acid solution to 2-4, adding the oxygen-deficient Bi 5 O 7 I loaded polytriazine imide composite material, reacted for 30-60 minutes in dark conditions to reach adsorption equilibrium, and reacted for more than 3 h under light conditions with a wavelength of 320 nm-2500 nm.

Citation Information

Patent Citations

  • High-activity crystal face co-exposed ternary flower-shaped Bi0 / BiOI / ZCO wave-absorbing material as well as preparation method and application thereof

    CN117983253A

  • Ternary heterojunction photocatalytic material as well as preparation method and application thereof

    CN118002208A

  • Carbon / zinc oxide / polytriazineimine ternary composite visible-light-driven photocatalyst as well as preparation method and application thereof

    CN110975933A

  • Polytriazine imide / zinc ferrite photocatalytic composite material as well as preparation and application thereof

    CN117599825A