Coating material and preparation method thereof, coated modified lithium-rich manganese-based positive electrode material and preparation method thereof, battery

Through the coating technology of NaMF4, ZIF-8, and LiMnO2 nanoheterojunction composite layers, the problem of insufficient particle size and conduction rate of lithium-rich manganese-based positive electrode materials is solved, the structural stability and electrochemical performance of the material are improved, and the Improved battery capacity and performance.

CN118495600BActive Publication Date: 2024-11-01GANZHOU NOVA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410960088.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing lithium-rich manganese-based positive electrode materials have large particle sizes, poor electrochemically active sites and ion conduction rates, and limited active sites of conventional coatings, which cannot meet the ion and electron transport needs of the material.

Method used

The nanoheterojunction composite layer composed of NaMF4, ZIF-8, and LiMnO2 is used as the coating material, and is synthesized in situ by hydrothermal reaction and liquid phase method to form a nano-scale coating layer to improve the specific surface area and active sites of the material. , promotes rapid transmission of ions and electrons.

Benefits of technology

The structural stability and ion-electron transport performance of lithium-rich manganese-based positive electrode materials have been improved, and the battery capacity retention rate is high and the electrochemical performance is excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495600B_ABST
    Figure CN118495600B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery materials, and discloses a coating material and a preparation method thereof. The coating material is a nano-heterojunction composite layer composed of NaMF4, ZIF‑8, and LiMnO2; wherein M is at least one of Co, Sc, and Y. During the preparation process, NaMF4 nanoparticles are first synthesized by a hydrothermal method, and then NaMF4 / ZIF‑8 nanomaterials are synthesized in situ by a liquid phase method, and then NaMF4 / ZIF‑8 / LiMnO2 nano-heterojunction materials are directly synthesized by an in-situ liquid phase reaction method. The present invention provides a coating material, and a battery assembled with a lithium-rich manganese-based positive electrode material coated and modified by the coating material has a high capacity retention rate. In addition, the present invention discloses a lithium-rich manganese-based positive electrode material coated and modified by the above-mentioned coating material and a preparation method thereof, and discloses a battery including a coated and modified lithium-rich manganese-based positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and specifically relates to the modification research of lithium-rich manganese-based positive electrode materials, and especially to the research of coating materials. Background Art

[0002] Lithium-rich manganese-based cathode materials have the advantages of high specific capacity and high operating voltage, and are currently a hot topic in the research of battery cathode materials. However, the Mn in the Li2MnO3-like lattice structure of lithium-rich manganese-based materials is 4+ The local structure of lithium-rich manganese-based materials is electrically neutral, which leads to the easy formation of aggregates in the material. The synthesized lithium-rich manganese-based cathode materials are usually large in particle size, with poor electrochemical active sites and ion conductivity. A large number of studies have modified the surface of lithium-rich manganese-based cathode materials by coating them with compounds such as oxides and fast ion conductors. However, conventional coatings have limited active sites and insufficient specific surface area to meet the ion and electron transport requirements of lithium-rich manganese-based host materials. Summary of the Invention

[0003] In response to the problems existing in the prior art, the first purpose of the present invention is to provide a coating material and a preparation method thereof; the second purpose of the present invention is to provide a coated and modified lithium-rich manganese-based positive electrode material and a preparation method and application thereof.

[0004] First, the present invention provides a coating material, which is a nano-heterojunction composite layer composed of NaMF4, ZIF-8, and LiMnO2; wherein M is at least one of Co, Sc, and Y.

[0005] In a further preferred embodiment, the molar ratio of NaMF4, ZIF-8, and LiMnO2 in the coating material is 1:1~4:0.5~1.5.

[0006] Secondly, the present invention provides a method for preparing the above-mentioned coating material, comprising the following steps:

[0007] (1) A sodium source, an unsaturated fatty acid, and anhydrous ethanol are mixed to form a solution A; fluoride is dissolved in deionized water to form a solution B; solution B is added to solution A to form a solution C; a metal salt of M is added to solution C to carry out a hydrothermal reaction; M is at least one of Co, Sc, and Y; after the hydrothermal reaction is completed, the reaction product is washed to obtain NaMF4 particles;

[0008] (2) dispersing the NaMF4 particles in step (1) in methanol, adding a zinc source, and then adding a 2-methylimidazole solution dropwise to react; after the reaction is completed, washing and drying the reaction product to obtain a NaMF4 / ZIF-8 material;

[0009] (3) The NaMF4 / ZIF-8 nanomaterial in step (2) is dispersed in deionized water, potassium permanganate is added, and then a lithium source having an acidic aqueous solution is added to react; after the reaction is completed, the reaction product is washed and dried to obtain a NaMF4 / ZIF-8 / LiMnO2 material.

[0010] In a further preferred embodiment, the sodium source is at least one of sodium hydroxide, sodium methoxide, and sodium ethoxide; the unsaturated fatty acid is at least one of oleic acid, erucic acid, ricinoleic acid, and trans-oleic acid; the fluoride is at least one of sodium fluoride and ammonium fluoride; and the metal salt of M is at least one of nitrate and acetate.

[0011] In a further preferred embodiment, the molar ratio of sodium in the sodium source, unsaturated fatty acid, fluorine in the fluoride, and M is 1:1.1 to 1.5:4:1.

[0012] In a further preferred embodiment, the temperature of the hydrothermal reaction is 160-200° C.; and the time of the hydrothermal reaction is 12-36 hours.

[0013] In a further preferred embodiment, the zinc source is one or both of zinc nitrate and zinc acetate.

[0014] In a further preferred embodiment, the concentration of the 2-methylimidazole solution is 0.5-1 mol / L.

[0015] In a further preferred embodiment, the molar ratio of the NaMF4 particles, the zinc in the zinc source, and the 2-methylimidazole is 1:1-4:8-60.

[0016] In a further preferred embodiment, the lithium source is at least one of lithium nitrate, lithium sulfate, and lithium acetate.

[0017] In a further preferred embodiment, the molar ratio of the NaMF4 / ZIF-8 material, potassium permanganate, and lithium in the lithium source is 1:0.5~1.5:0.5~1.5.

[0018] The present invention further provides a coated modified lithium-rich manganese-based positive electrode material, comprising a lithium-rich manganese-based positive electrode material substrate and a coating layer located on at least a portion of the surface of the lithium-rich manganese-based positive electrode material substrate, wherein the coating layer is composed of the aforementioned coating material.

[0019] In a further preferred embodiment, the general chemical formula of the lithium-rich manganese-based cathode material matrix is ​​Li 1+m Mn 1-m- n X n O2, X is one or more of Ni, Co, Fe, Al, Zn, 0.1≤m≤0.5, 0 <n≤0.5。

[0020] Secondly, the present invention provides a method for preparing a coated and modified lithium-rich manganese-based positive electrode material, comprising:

[0021] The lithium-rich manganese-based positive electrode material matrix and the aforementioned coating material are added into ethanol, ball-milled and mixed, and then dried to obtain a coated and modified lithium-rich manganese-based positive electrode material.

[0022] In a further preferred embodiment, the mass ratio of the lithium-rich manganese-based positive electrode material matrix to the coating material is 1:0.03-0.1.

[0023] Based on the same inventive concept, the present invention provides a battery comprising the aforementioned coated and modified lithium-rich manganese-based positive electrode material.

[0024] The above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects:

[0025] The present invention provides a novel coating material, which broadens the scope of coating modification of positive electrode materials, especially lithium-rich manganese-based positive electrode materials.

[0026] The preparation method of the coating material provided by the invention has readily available raw materials and a simple and controllable process.

[0027] The coated and modified lithium-rich manganese-based positive electrode material provided by the present invention has good structural stability and good rapid transmission performance of ions and electrons. After the positive electrode material is assembled into a battery, the capacity retention rate of the battery is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 TEM image of NaCoF4 / ZIF-8 / LiMnO2 nanomaterials.

[0029] Figure 2 This is the HRTEM image of NaCoF4 / ZIF-8 / LiMnO2 material.

[0030] Figure 3 The lithium-rich manganese-based positive electrode material Li in Example 1 1.2 Mn 0.58 Ni 0.22 SEM image of O2.

[0031] Figure 4 This is the SEM image of the coated and modified lithium-rich manganese-based positive electrode material in Example 1.

[0032] Figure 5 This is the TEM image of the coated and modified lithium-rich manganese-based positive electrode material in Example 1.

[0033] Figure 6 The cycling performance diagram of the assembled battery. DETAILED DESCRIPTION

[0034] The current coating modification of lithium-rich manganese-based cathode materials is not enough to meet the ion and electron transport requirements of lithium-rich manganese-based host materials. For the coating modification of cathode materials, the coating material is the key.

[0035] First, some embodiments of the present invention provide a coating material, which is a nano-heterojunction composite layer composed of NaMF4, ZIF-8, and LiMnO2; wherein M is at least one of Co, Sc, and Y.

[0036] In some specific embodiments of the present invention, the molar ratio of NaMF4, ZIF-8, and LiMnO2 in the coating material is 1:1~4:0.5~1.5.

[0037] The coating material provided by the present invention is a nano heterojunction composite layer, and the chemical formula can be expressed as NaMF4 / ZIF-8 / LiMnO2.

[0038] Theoretically, the coating material can effectively adsorb irreversible products and provide multiple active sites and space for lithium ion transport. The coating material contains a fluorine source, which effectively inhibits irreversible reactions in the electrolyte. The high specific surface area and multiple active sites of ZIF-8 effectively adsorb irreversible reaction products during the electrochemical process. The LiMnO2 component provides an excess lithium source for the main material. The LiMnO2 particles form a stable Li-Mn-O bond with the main material, ensuring the stable coating of the composite layer on the surface of the main material and effectively mitigating irreversible structural changes such as oxygen precipitation in the main structure. Furthermore, the entire nanoheterojunction composite layer possesses its own intrinsic electric field, which effectively promotes the rapid transport of ions and electrons.

[0039] Secondly, some embodiments of the present invention provide a method for preparing the above-mentioned coating material, comprising the following steps:

[0040] (1) A sodium source, an unsaturated fatty acid, and anhydrous ethanol are mixed to form a solution A; fluoride is dissolved in deionized water to form a solution B; solution B is added to solution A to form a solution C; a metal salt of M is added to solution C to carry out a hydrothermal reaction; M is at least one of Co, Sc, and Y; after the hydrothermal reaction is completed, the reaction product is washed to obtain NaMF4 particles;

[0041] (2) dispersing the NaMF4 particles in step (1) in methanol, adding a zinc source, and then adding a 2-methylimidazole solution dropwise to react; after the reaction is completed, washing and drying the reaction product to obtain a NaMF4 / ZIF-8 material;

[0042] (3) The NaMF4 / ZIF-8 material in step (2) is dispersed in deionized water, potassium permanganate is added, and then a lithium source having an acidic aqueous solution is added to react; after the reaction is completed, the reaction product is washed and dried to obtain a NaMF4 / ZIF-8 / LiMnO2 material.

[0043] NaMF4 nanoparticles were first synthesized by a hydrothermal method, then NaMF4 / ZIF-8 nanomaterials were in situ synthesized by a liquid phase method, and finally NaMF4 / ZIF-8 / LiMnO2 nanoheterojunction materials were directly synthesized by an in situ liquid phase reaction method.

[0044] In step (1), sodium ions first react with the unsaturated fatty acid RCOO - Complexation, then with F in fluoride - After uniform mixing, complexation is carried out again to form a double complex; further addition of metal salt of M and RCOO - and F - The double complexation reaction is carried out to form a complex, and NaMF4 particles are obtained after hydrothermal reaction.

[0045] In step (2), NaMF4 particles are used as the substrate material, and the Zn in the zinc source 2+ The ZIF-8 was directly synthesized in situ on the substrate surface by complexation reaction with 2-methylimidazole.

[0046] In step (3), NaMF4 / ZIF-8 material is used as the base material, potassium permanganate is added, and then a lithium source with an acidic aqueous solution is added. In an acidic environment, potassium permanganate undergoes oxidation-reduction and reacts with Li + The reaction proceeds to generate LiMnO2 directly on the surface of the NaMF4 / ZIF-8 material, thereby ultimately forming a nano-heterojunction NaMF4 / ZIF-8 / LiMnO2 material.

[0047] In some specific embodiments of the present invention, the sodium source is at least one of sodium hydroxide, sodium methoxide, and sodium ethoxide.

[0048] In some specific embodiments of the present invention, the unsaturated fatty acid is at least one of oleic acid, erucic acid, ricinoleic acid, and trans-oleic acid.

[0049] In some specific embodiments of the present invention, the fluoride is at least one of sodium fluoride and ammonium fluoride.

[0050] In some specific embodiments of the present invention, the metal salt of M is at least one of nitrate and acetate.

[0051] Those skilled in the art will appreciate that the sodium source, unsaturated fatty acid, fluoride, and metal salt of M in the specific embodiments of the present invention are merely examples. Those skilled in the art, inspired by the technical concept of the present invention, may select other types of raw materials, which constitute equivalent substitutions for the raw materials and are also within the scope of protection of the present invention.

[0052] In some specific embodiments of the present invention, the molar ratio of sodium in the sodium source, unsaturated fatty acid, fluorine in fluoride, and M is 1:1.1~1.5:4:1. Unsaturated fatty acid as a complexing agent should be appropriately excessive so that it can fully react with Na + When there are too few unsaturated fatty acids, the sodium ions cannot be completely complexed; if there are too many unsaturated fatty acids, the subsequent solution solubility will be affected, affecting the formation of reaction products.

[0053] In some specific embodiments of the present invention, the temperature of the hydrothermal reaction is 160-200° C., for example, 160° C., 180° C., 200° C., etc. The hydrothermal reaction time is adaptively determined according to the temperature of the hydrothermal reaction, and is generally 12-36 hours.

[0054] In some specific embodiments of the present invention, the zinc source is one or both of zinc nitrate and zinc acetate. It should be known to those skilled in the art that other zinc salts are also conventional choices of zinc sources.

[0055] In some specific embodiments of the present invention, the concentration of the 2-methylimidazole solution is 0.5-1 mol / L.

[0056] In some specific embodiments of the present invention, the molar ratio of the NaMF4 particles, the zinc in the zinc source, and the 2-methylimidazole is 1:1-4:8-60. The ratio of the zinc in the zinc source to the 2-methylimidazole enables the full synthesis of ZIF-8, ensuring the yield of the product. When the amount ratio of the zinc source to the 2-methylimidazole is too small, less ZIF-8 is generated, and the composite effect is poor. When the amount ratio of the zinc in the zinc source to the 2-methylimidazole is too large, more ZIF-8 is generated, affecting the conductivity of the entire coating layer.

[0057] In some specific embodiments of the present invention, the lithium source is at least one of lithium nitrate, lithium sulfate, and lithium acetate. The present invention specifically selects lithium salts that are acidic when dissolved in water. Those skilled in the art will appreciate that other lithium salts that can achieve the objectives of the present invention are also conventional choices for lithium sources.

[0058] In some specific embodiments of the present invention, the molar ratio of the NaMF4 / ZIF-8 material, potassium permanganate, and lithium in the lithium source is 1:0.5-1.5:0.5-1.5. It should be noted that the molecular weight of the NaMF4 / ZIF-8 material can be inferred based on the dosage ratio of the reaction raw materials in step (2) and the reaction equation. In the specific reaction process, potassium permanganate reacts with the lithium in the lithium source in a ratio of 1:1. The appropriate amount of the reaction raw materials is selected to ensure that LiMnO2 is uniformly formed on the surface of the NaMF4 / ZIF-8 material.

[0059] In addition, some embodiments of the present invention also disclose lithium-rich manganese-based positive electrode materials coated and modified with the aforementioned coating materials.

[0060] To facilitate understanding of the present invention, the present invention will be described in more comprehensive and detailed form below in conjunction with the accompanying drawings and preferred embodiments. However, the protection scope of the present invention is not limited to the following specific embodiments.

[0061] Unless otherwise defined, all technical terms used hereinafter have the same meanings as those generally understood by those skilled in the art. The technical terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0062] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0063] Example 1

[0064] (1) Dissolve 0.01 mol sodium hydroxide and 0.014 mol oleic acid in 3.5 ml of anhydrous ethanol to form solution A. Dissolve 0.04 mol ammonium fluoride in 80 ml of deionized water to form solution B. Add solution B to solution A to form solution C. Add 0.01 mol cobalt nitrate to solution C, stir evenly at room temperature, then transfer to a polytetrafluoroethylene liner and hydrothermally react at 200°C for 12 h. Wash the product obtained by the hydrothermal reaction to obtain NaCoF4 nanoparticles.

[0065] (2) The NaCoF4 nanoparticles prepared in step (1) were dispersed in 50 ml of methanol, 0.03 mol of zinc nitrate was added and stirred evenly, and then 240 ml of 1 mol / L 2-methylimidazole solution was added dropwise. After stirring for 1 h, the reaction product was washed and dried to obtain NaCoF4 / ZIF-8 nanomaterials.

[0066] (3) The NaCoF4 / ZIF-8 nanomaterial prepared in step (2) was dispersed in 100 ml of deionized water, 0.01 mol of potassium permanganate was added and the mixture was stirred continuously, and then 0.01 mol of lithium nitrate was added. The mixture was reacted at room temperature for 3 h. The reaction product was centrifuged, washed, and dried to obtain NaCoF4 / ZIF-8 / LiMnO2 nanomaterial.

[0067] Figure 1 This is the TEM image of NaCoF4 / ZIF-8 / LiMnO2 nanomaterial. It can be seen from the figure that the material has a nanostructure.

[0068] Figure 2 This is the HRTEM image of NaCoF4 / ZIF-8 / LiMnO2 material. Based on the lattice fringes in the image, it can be calculated that there are three phases of NaCoF4, ZIF-8, and LiMnO2 in the structure, and the three phases are seamlessly connected to form a nanostructured heterojunction.

[0069] (4) 5g of lithium-rich manganese-based positive electrode material Li 1.2 Mn 0.58 Ni 0.22 O2 was dispersed in ethanol, and 0.4 g of the NaCoF4 / ZIF-8 / LiMnO2 nanomaterial from step (3) was added and ball milled for 1 h. After drying, a coated and modified lithium-rich manganese-based positive electrode material was obtained. The SEM images of the lithium-rich manganese-based positive electrode material before and after coating are shown in FIG. Figure 3 and 4 As shown, Figure 3 This is the SEM image of the lithium-rich manganese-based positive electrode material before coating. It can be seen from the image that the material is in the form of micron blocks, the particle size is evenly distributed, and there are secondary particles connected. Figure 4 This SEM image shows a coated and modified lithium-rich manganese-based cathode material. The resulting cathode material exhibits micron-sized aggregates, a uniform particle size distribution, and a smooth surface, demonstrating a successful composite. Ball milling during the coating process effectively separated the interconnected particles of the lithium-rich manganese-based cathode material. In the presence of the NaCoF4 / ZIF-8 / LiMnO2 nanomaterial, the aggregated particles were separated and an in-situ surface composite coating was achieved.

[0070] In addition, the TEM images of the coated modified lithium-rich manganese-based cathode materials are as follows: Figure 5 As shown in the figure, it can be seen that the surface of the positive electrode material is coated with a nano-scale composite layer with a thickness of 1-2nm. The coating layer is evenly distributed and the coating effect is good.

[0071] Comparative Example 1

[0072] (1) Dissolve 0.01 mol sodium hydroxide and 0.014 mol oleic acid in 3.5 ml of anhydrous ethanol to form solution A. Dissolve 0.04 mol ammonium fluoride in 80 ml of deionized water to form solution B. Add solution B to solution A to form solution C. Add 0.01 mol cobalt nitrate to solution C, stir evenly at room temperature, then transfer to a polytetrafluoroethylene liner and hydrothermally react at 200°C for 12 h. Wash the product obtained by the hydrothermal reaction to obtain NaCoF4 nanomaterials.

[0073] (2) 5g of lithium-rich manganese-based positive electrode material Li 1.2 Mn 0.58 Ni 0.22 O2 is dispersed in ethanol, 0.4 g of the NaCoF4 nanomaterial in step (1) is added, and the mixture is ball-milled for 1 h; after drying, a coated and modified lithium-rich manganese-based positive electrode material is obtained.

[0074] Comparative Example 2

[0075] (1) Dissolve 0.01 mol sodium hydroxide and 0.014 mol oleic acid in 3.5 ml of anhydrous ethanol to form solution A. Dissolve 0.04 mol ammonium fluoride in 80 ml of deionized water to form solution B. Add solution B to solution A to form solution C. Add 0.01 mol cobalt nitrate to solution C, stir evenly at room temperature, then transfer to a polytetrafluoroethylene liner and hydrothermally react at 200°C for 12 h. Wash the product obtained by the hydrothermal reaction to obtain NaCoF4 nanomaterials.

[0076] (2) The NaCoF4 nanoparticles prepared in step (1) were dispersed in 50 ml of methanol, 0.03 mol of zinc nitrate was added and stirred evenly, and then 240 ml of 1 mol / L 2-methylimidazole solution was added dropwise. After stirring for 1 h, the reaction product was washed and dried to obtain NaCoF4 / ZIF-8 nanomaterials.

[0077] (3) 5g of lithium-rich manganese-based positive electrode material Li 1.2 Mn 0.58 Ni 0.22 O2 was dispersed in ethanol, 0.4 g of the NaCoF4 / ZIF-8 nanomaterial in step (2) was added, and the mixture was ball-milled for 1 h; after drying, a coated and modified lithium-rich manganese-based positive electrode material was obtained.

[0078] Comparative Example 3

[0079] Lithium-rich manganese-based cathode material Li 1.2 Mn 0.58 Ni 0.22 O2, not coated or modified.

[0080] Example 2

[0081] (1) Dissolve 0.01 mol sodium methoxide and 0.011 mol trans-oleic acid in 3.5 ml of anhydrous ethanol to form solution A. Dissolve 0.04 mol ammonium fluoride in 80 ml of deionized water to form solution B. Add solution B to solution A to form solution C. Add 0.01 mol yttrium nitrate to solution C, stir evenly at room temperature, transfer to a polytetrafluoroethylene liner, and hydrothermally react at 160°C for 36 h. Wash the product obtained by the hydrothermal reaction to obtain NaYF4 nanoparticles.

[0082] (2) The NaYF4 nanoparticles prepared in step (1) were dispersed in 50 ml of methanol, 0.01 mol of zinc acetate was added and stirred evenly, and then 80 ml of 1 mol / L 2-methylimidazole solution was added dropwise. After stirring for 1 h, the reaction product was washed and dried to obtain NaYF4 / ZIF-8 nanomaterials.

[0083] (3) The NaYF4 / ZIF-8 nanomaterial prepared in step (2) was dispersed in 100 ml of deionized water, 0.005 mol of potassium permanganate was added and the mixture was stirred continuously, and then 0.0025 mol of lithium sulfate was added. The mixture was reacted at room temperature for 3 h. The reaction product was centrifuged, washed, and dried to obtain the NaYF4 / ZIF-8 / LiMnO2 nanomaterial.

[0084] (4) 5g of lithium-rich manganese-based positive electrode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 was dispersed in ethanol, and 0.15 g of the NaYF4 / ZIF-8 / LiMnO2 nanomaterial in step (3) was added and ball milled for 1 h; after drying, a coated and modified lithium-rich manganese-based positive electrode material was obtained.

[0085] Example 3

[0086] (1) Dissolve 0.01 mol sodium ethoxide and 0.015 mol erucic acid in 3.5 ml of anhydrous ethanol to form solution A. Dissolve 0.04 mol sodium fluoride in 80 ml of deionized water to form solution B. Add solution B to solution A to form solution C. Add 0.01 mol scandium nitrate to solution C, stir evenly at room temperature, transfer to a polytetrafluoroethylene liner, and hydrothermally react at 180°C for 26 h. Wash the product obtained by the hydrothermal reaction to obtain NaScF4 nanoparticles.

[0087] (2) The NaScF4 nanoparticles prepared in step (1) were dispersed in 50 ml of methanol, 0.04 mol of zinc nitrate was added and stirred evenly, and then 600 ml of 1 mol / L 2-methylimidazole solution was added dropwise. The mixture was stirred for reaction, and the reaction product was washed and dried to obtain NaScF4 / ZIF-8 nanomaterials.

[0088] (3) The NaScF4 / ZIF-8 nanomaterial prepared in step (2) was dispersed in 100 ml of deionized water, 0.015 mol of potassium permanganate was added and the mixture was stirred continuously, and then 0.015 mol of 1 mol / L lithium acetate was added. The mixture was reacted at room temperature. The reaction product was centrifuged, washed, and dried to obtain the NaScF4 / ZIF-8 / LiMnO2 nanomaterial.

[0089] (4) 5g of lithium-rich manganese-based positive electrode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 was dispersed in ethanol, and 0.5 g of the NaScF4 / ZIF-8 / LiMnO2 nanomaterial in step (3) was added and ball milled for 1 h; after drying, a coated and modified lithium-rich manganese-based positive electrode material was obtained.

[0090] Complete battery assembly by:

[0091] The positive electrode materials obtained in Examples 1-3 and Comparative Examples 1-3 were used as the positive electrode active material for the battery. They were mixed with a conductive agent, acetylene black (AB), and a binder, polyvinylidene fluoride (PVDF), in a mass ratio of 8:1:1. N-methylpyrrolidone (NMP) was used as the solvent, and the mixture was stirred in a small beaker at 800 rpm for 2 hours to obtain a slurry. The slurry was coated on a current collector aluminum foil using an automatic coating machine, placed flat on tempered glass, and dried in a vacuum drying oven at 85°C for 4 hours. The slurry was punched into a 12 mm diameter electrode sheet, which was then dried in a vacuum drying oven at 105°C for 4 hours. The sheet was then placed in an argon atmosphere in a glove box with a moisture and oxygen content of less than 0.1 ppm for 4 hours to reduce moisture adsorbed by the electrode sheet during transfer. The slurry was then assembled into CR2032 button cells in the glove box. The battery uses a pure metal lithium sheet with a diameter of 16mm and a thickness of 0.5mm as the negative electrode, and a porous polyethylene membrane of model Celgard2300 with a diameter of 18mm as the separator.

[0092] After the battery was assembled and aged for 12 hours, the charge and discharge test was carried out. The battery was activated at a voltage of 2-4.6V, a current density of 0.1C for 3 cycles, and then cycled at a current density of 1C for 100 cycles. The discharge specific capacity results are shown in Table 1 and Figure 6 shown.

[0093] Table 1

[0094]

[0095] From Table 1 and Figure 6 It can be seen that:

[0096] A comparative analysis of Comparative Example 1, Comparative Example 2 and Comparative Example 3 shows that compared with the uncoated lithium-rich manganese-based positive electrode material, the lithium-rich manganese-based positive electrode material coated with NaCoF4 and NaCoF4 / ZIF-8 makes the battery initial specific capacity and capacity retention rate higher.

[0097] Analysis and comparison of Example 1, Comparative Example 1 and Comparative Example 2 show that compared with the coated NaCoF4 and NaCoF4 / ZIF-8, the coating layer of NaCoF4 / ZIF-8 / LiMnO2 nanomaterial makes the electrical properties of the lithium-rich manganese-based positive electrode material better.

[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A coating material, characterized in that: The coating material is a nano-heterojunction composite layer composed of NaMF4, ZIF-8 and LiMnO2; wherein M is at least one of Co, Sc and Y.

2. The coating material according to claim 1, characterized in that The molar ratio of NaMF4, ZIF-8 and LiMnO2 in the coating material is 1:1~4:0.5~1.

5.

3. A method for preparing a coating material, characterized in that: The following steps are involved: (1) Mixing a sodium source, unsaturated fatty acid and anhydrous ethanol to form a solution A; Dissolve fluoride in deionized water to form solution B; Solution B is added to solution A to form solution C; Adding a metal salt of M to solution C to perform a hydrothermal reaction; M is at least one of Co, Sc, and Y; after the hydrothermal reaction is completed, washing the reaction product to obtain NaMF4 particles; (2) dispersing the NaMF4 particles in step (1) in methanol, adding a zinc source, and then adding a 2-methylimidazole solution dropwise to react; after the reaction is completed, washing and drying the reaction product to obtain a NaMF4 / ZIF-8 material; (3) dispersing the NaMF4 / ZIF-8 nanomaterial in step (2) in deionized water, adding potassium permanganate, and then adding a lithium source to react; after the reaction is completed, washing and drying the reaction product to obtain a NaMF4 / ZIF-8 / LiMnO2 coated material; The molar ratio of NaMF4, ZIF-8 and LiMnO2 in the coating material is 1:1~4:0.5~1.5; The lithium source is at least one of lithium nitrate, lithium sulfate and lithium acetate.

4. The method for preparing the coating material according to claim 3, characterized in that: The sodium source is at least one of sodium hydroxide, sodium methoxide, and sodium ethoxide; the unsaturated fatty acid is at least one of oleic acid, erucic acid, ricinoleic acid, and trans-oleic acid; the fluoride is at least one of sodium fluoride and ammonium fluoride; the metal salt of M is at least one of nitrate and acetate; the zinc source is one or both of zinc nitrate and zinc acetate; and the concentration of the 2-methylimidazole solution is 0.5-1 mol / L.

5. The method for preparing the coating material according to claim 3 or 4, characterized in that: The molar ratio of sodium in the sodium source, unsaturated fatty acids, fluorine in fluoride, and M is 1:1.1~1.5:4:1; the molar ratio of the NaMF4 particles, zinc in the zinc source, and 2-methylimidazole is 1:1~4:8~60; the molar ratio of the NaMF4 / ZIF-8 material, potassium permanganate, and lithium in the lithium source is 1:0.5~1.5:0.5~1.

5.

6. The method for preparing the coating material according to claim 3, characterized in that: The temperature of the hydrothermal reaction is 160-200°C.

7. A coated and modified lithium-rich manganese-based positive electrode material, characterized in that: It comprises a lithium-rich manganese-based positive electrode material matrix and a coating layer located on at least a portion of the surface of the lithium-rich manganese-based positive electrode material matrix, wherein the coating layer is composed of the coating material according to claim 1 or 2 or a coating material prepared by the preparation method according to any one of claims 3 to 6.

8. The coated and modified lithium-rich manganese-based positive electrode material according to claim 7, characterized in that: The general chemical formula of the lithium-rich manganese-based positive electrode material matrix is ​​Li 1+m Mn 1-m-n X n O2, X is one or more of Ni, Co, Fe, Al, Zn, 0.1≤m≤0.5, 0 <n≤0.5。 9. The method for preparing the coated modified lithium-rich manganese-based positive electrode material according to claim 7 or 8, characterized in that: include: A lithium-rich manganese-based positive electrode material matrix, a coating material according to claim 1 or 2, or a coating material prepared by the preparation method according to any one of claims 3 to 6 is added to ethanol, ball-milled and mixed, and then dried to obtain a coated and modified lithium-rich manganese-based positive electrode material.

10. A battery, characterized in that: It includes the coated and modified lithium-rich manganese-based positive electrode material as described in claim 7 or 8.