A color-fixing protective glaze for hot-bending integrated basin and preparation method thereof
Ceramic glaze is solved by using color-fixed protective glazes such as feldspar, calcium borate, zinc oxide, tin oxide, iron oxide, zirconium oxide and 3-aminopropyltriethoxysilane grafted polyethylene glycol. The problem of pigment loss under high temperature conditions has improved the stability and aesthetics of the glaze layer.
Patent Information
- Application Number
- CN202410689851.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-30
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic glazes, and in particular to a color-fixing protective glaze for a hot-bent integrated basin and a preparation method thereof. Background Art
[0002] With the development of modern home decoration technology, the unique design and excellent performance of hot-bent one-piece basins have gradually gained favor among consumers. This technology bends the material into shape by heating, and can produce a variety of complex and beautiful shapes. However, the hot-bent one-piece basin needs to experience high temperatures of up to 1200°C during the production process. During this process, the pigment layer on the surface of the embryo can be easily burned off, resulting in fading or uneven color. In order to maintain the beauty of the product and the durability of the color during the process, a layer of protective glaze is usually applied to the surface of the pigment layer. However, the existing protective glaze is less effective in preventing the burning of pigments under high temperature conditions, so further improvements are needed to improve its protective effect.
[0003] CN 112358188 B discloses a ceramic thin plate inkjet underglaze color decorative glaze, which uses an organic solvent to produce an oily decorative glaze layer more suitable for the production of ceramic thin plates, replacing the water-based surface glaze layer applied after inkjet in the traditional process, and can solve the problems of "glaze shrinkage" and "glaze avoidance" commonly existing in the production of large-sized ceramic thin plates by the traditional process, reduce the phenomenon of explosion, cracking and warping, and broaden the application range of inkjet decoration. However, it has little effect on preventing the burning loss of pigments under high temperature conditions. Summary of the invention
[0004] In view of the shortcomings in the existing technology,
[0005] The present invention provides a color-fixing protective glaze for a hot-bent integrated basin, which comprises the following raw materials in parts by mass:
[0006] Feldspar: 35-45 parts;
[0007] Calcium borate: 5-15 parts;
[0008] Zinc oxide: 5-15 parts;
[0009] Tin oxide: 1-10 parts;
[0010] Iron oxide: 1-5 parts;
[0011] Zirconia: 10-20 parts;
[0012] Silicon oxide: 15-20 parts;
[0013] High molecular weight polymer: 1-3 parts.
[0014] The high molecular polymer is at least one of polyethylene glycol, 3-aminopropyl triethoxysilane grafted polyethylene glycol, and poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-grafted-poly(ethylene glycol) methyl ether; preferably, the high molecular polymer is 3-aminopropyl triethoxysilane grafted polyethylene glycol.
[0015] The preparation method of 3-aminopropyltriethoxysilane grafted polyethylene glycol comprises the following steps:
[0016] Polyethylene glycol and 3-aminopropyltriethoxysilane are mixed to obtain a reaction raw material, and the reaction raw material is added to a solvent with stirring, and sodium hydroxide is added at the same time, and heated to 60-80° C. for reaction for 1-2 hours. After the reaction is completed, the solution is cooled and concentrated under reduced pressure to obtain 3-aminopropyltriethoxysilane grafted polyethylene glycol.
[0017] The solvent is one of toluene or ethanol; preferably, the solvent is ethanol.
[0018] The polyethylene glycol is low molecular weight polyethylene glycol (molecular weight <1000Da), medium molecular weight polyethylene glycol (molecular weight 1000-10000Da), high molecular weight polyethylene glycol (molecular weight>10000Da); preferably, the polyethylene glycol is medium molecular weight polyethylene glycol; more preferably, the molecular weight of the polyethylene glycol is 4000-8000Da.
[0019] The mass ratio of the polyethylene glycol to 3-aminopropyltriethoxysilane is (4-20):1.
[0020] The mass ratio of the reaction raw materials to the solvent is (1-20):100.
[0021] The mass ratio of the reaction raw materials to sodium hydroxide is 1:(0.01-0.1).
[0022] The preparation method of the color-fixing protective glaze comprises the following steps:
[0023] By weight, 35-45 parts of feldspar, 5-15 parts of calcium borate, 5-15 parts of zinc oxide, 1-10 parts of tin oxide, 1-5 parts of iron oxide, 10-20 parts of zirconium oxide, 15-20 parts of silicon oxide and 1-3 parts of high molecular polymer are mixed, 30-50 parts of water are added for ball milling, the mixture is sieved through a 350-450 mesh sieve and dried to obtain the color fixing protective glaze.
[0024] When the color fixing protective glaze is used, water accounting for 40-60% of the weight of the glaze itself is added for grinding to obtain glaze slurry, and then the glazing operation is performed on the surface of the hot-bent integrated basin.
[0025] Feldspar (K2O·Al2O3·6SiO2): Feldspar is the basic additive of glaze and provides the main structural components of glaze. At high temperatures, feldspar arranges to form K2O, Al2O3 and SiO2, which can cooperate with other materials to form a stable glass phase, enhancing the mechanical strength and wear resistance of the glaze layer.
[0026] Calcium borate (CaO·B2O3): Calcium borate decomposes at high temperatures to generate CaO and B2O3. CaO is a filler stabilizer that can improve the chemical resistance of the glaze, while B2O3 acts as a flux to enhance the fluidity and uniformity of the glaze, increase the viscosity and adsorption of the glaze layer, and enhance the color stability.
[0027] Zinc oxide (ZnO): ZnO plays a role in fluxing and melting in the material. ZnO can improve the gloss and hardness of the material at high temperatures, and adhere to zinc silicate to improve the hardness and wear resistance of the metal.
[0028] Tin oxide (SnO2): SnO2 acts as an opacifier and antioxidant, which can prevent the oxidation series of fluorescent agents at high temperatures, while providing good white hiding power and color fixing properties, enhancing the color stability of the glaze.
[0029] Iron Oxide (Fe2O3): Fe2O3 acts as a colorant at high temperatures, providing a reddish-brown hue while enhancing the antioxidant capacity of the pigment layer.
[0030] Zirconium oxide (ZrO2): ZrO2 has extremely high chemical stability and wear resistance, which can enhance the mechanical strength and heat resistance of the glaze at high temperatures and prevent the glaze layer from cracking and falling off.
[0031] Silicon oxide (SiO2): As the main component of glaze, SiO2 provides the reconstructed structure of glaze. At high temperature, SiO2 cross-links with other components of silicate glass to enhance the hardness and chemical resistance of glaze.
[0032] Polyethylene glycol (PEG): PEG, as a surfactant, can improve the moisture and fluidity of the glaze during the glaze preparation process, so that the glaze can be more evenly covered on the substrate surface. At high temperatures, PEG will decompose, but at low temperatures it will act to form a uniform glaze layer.
[0033] Furthermore, the present invention finds that not all molecular weight polyethylene glycols are suitable as raw materials for protective glazes. Low molecular weight polyethylene glycol is more volatile, high molecular weight polyethylene glycol has poor protective effect and large pigment loss on ignition; the viscosity is too high and it is difficult to cover evenly, which affects the performance of the glaze. Polyethylene glycol with a molecular weight of 4000-8000Da is most suitable.
[0034] Furthermore, the present invention further adopts 3-aminopropyl triethoxysilane grafted polyethylene glycol. The present invention finds that grafting triethoxysilane groups onto polyethylene glycol (PEG) can effectively reduce the burning loss rate of pigments. The present invention believes that this is because the triethoxysilane group has unique chemical properties and can form a stable network structure with other silicon oxides at high temperatures to prevent adverse chemical reactions at high temperatures, while polyethylene glycol can improve the fluidity of the glaze, so that the glaze is more evenly covered on the surface of the substrate, and acts to form a uniform glaze layer at a low temperature stage. 3-aminopropyl triethoxysilane grafted polyethylene glycol has the properties of both, which can enhance the protective effect of the protective glaze to a greater extent and reduce the burning loss of pigments.
[0035] Beneficial effects of the present invention:
[0036] The protective glaze formula of the present invention, which uses feldspar, calcium borate, zinc oxide, tin oxide, iron oxide, zirconium oxide, silicon oxide, and 3-aminopropyltriethoxysilane grafted polyethylene glycol as raw materials, is suitable for the hot-bending one-piece basin process that requires high-temperature treatment, can minimize the burning loss of pigments, and increase the beauty of the hot-bending one-piece basin. DETAILED DESCRIPTION
[0037] PEG-600: Product number: 60361ES76; PEG-6000: Product number: 60366ES76; PEG-10000: Product number: 60367ES76; purchased from Yisheng Biotechnology (Shanghai) Co., Ltd.
[0038] Poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-graft-poly(ethylene glycol) methyl ether: CAS: 68938-54-5.
[0039] When the color-fixing protective glaze is used, 50% of the weight of the glaze itself is added to the water for grinding to obtain the glaze slurry, and then the glazing operation is performed on the surface of the hot-bent integrated basin.
[0040] Example 1
[0041] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0042] Feldspar: 40 parts;
[0043] Calcium borate: 10 parts;
[0044] Zinc oxide: 10 parts;
[0045] Tin oxide: 5 parts;
[0046] Iron oxide: 3 parts;
[0047] Zirconia: 15 parts;
[0048] Silicon oxide: 17 parts;
[0049] 3-Aminopropyltriethoxysilane grafted polyethylene glycol: 2 parts.
[0050] The preparation method of 3-aminopropyltriethoxysilane grafted polyethylene glycol comprises the following steps:
[0051] Polyethylene glycol and 3-aminopropyltriethoxysilane are mixed to obtain a reaction raw material, and the reaction raw material is added to a solvent with stirring, and sodium hydroxide is added at the same time, and heated to 70° C. for reaction for 2 hours. After the reaction is completed, the solution is cooled and concentrated under reduced pressure to obtain 3-aminopropyltriethoxysilane grafted polyethylene glycol.
[0052] The solvent is ethanol.
[0053] The polyethylene glycol is PEG-6000.
[0054] The mass ratio of the polyethylene glycol to 3-aminopropyltriethoxysilane is 16:1.
[0055] The mass ratio of the reaction raw materials to the solvent is 15:100.
[0056] The mass ratio of the reaction raw materials to sodium hydroxide is 1:0.06.
[0057] The preparation method of the color-fixing protective glaze comprises the following steps:
[0058] By mass, 40 parts of feldspar, 10 parts of calcium borate, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide, 17 parts of silicon oxide, and 2 parts of 3-aminopropyltriethoxysilane grafted polyethylene glycol are mixed, 40 parts of water are added for ball milling, the mixture is sieved through a 400-mesh sieve, and dried to obtain the color-fixing protective glaze.
[0059] Example 2
[0060] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0061] Feldspar: 40 parts;
[0062] Calcium borate: 10 parts;
[0063] Zinc oxide: 10 parts;
[0064] Tin oxide: 5 parts;
[0065] Iron oxide: 3 parts;
[0066] Zirconia: 15 parts;
[0067] Silicon oxide: 17 parts;
[0068] Polyethylene glycol: 2 parts.
[0069] The polyethylene glycol is PEG-6000.
[0070] The preparation method of the color-fixing protective glaze comprises the following steps:
[0071] By mass, 40 parts of feldspar, 10 parts of calcium borate, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide, 17 parts of silicon oxide and 2 parts of polyethylene glycol are mixed, 40 parts of water are added for ball milling, the mixture is passed through a 400-mesh sieve and dried to obtain the color-fixing protective glaze.
[0072] Example 3
[0073] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0074] Feldspar: 40 parts;
[0075] Calcium borate: 10 parts;
[0076] Zinc oxide: 10 parts;
[0077] Tin oxide: 5 parts;
[0078] Iron oxide: 3 parts;
[0079] Zirconia: 15 parts;
[0080] Silicon oxide: 17 parts;
[0081] Poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-graft-poly(ethylene glycol) methyl ether: 2 parts.
[0082] The preparation method of the color-fixing protective glaze comprises the following steps:
[0083] By mass, 40 parts of feldspar, 10 parts of calcium borate, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide, 17 parts of silicon oxide, and 2 parts of poly[dimethylsiloxane-co-methyl(3-hydroxypropyl)siloxane]-graft-poly(ethylene glycol) methyl ether are mixed, 40 parts of water are added for ball milling, the mixture is sieved through a 400-mesh sieve, and dried to obtain the color-fixing protective glaze.
[0084] Example 4
[0085] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0086] Feldspar: 40 parts;
[0087] Calcium borate: 10 parts;
[0088] Zinc oxide: 10 parts;
[0089] Tin oxide: 5 parts;
[0090] Iron oxide: 3 parts;
[0091] Zirconia: 15 parts;
[0092] Silicon oxide: 17 parts;
[0093] 3-Aminopropyltriethoxysilane: 2 parts.
[0094] The preparation method of the color-fixing protective glaze comprises the following steps:
[0095] By mass, 40 parts of feldspar, 10 parts of calcium borate, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide, 17 parts of silicon oxide and 2 parts of 3-aminopropyltriethoxysilane are mixed, 40 parts of water are added for ball milling, the mixture is passed through a 400-mesh sieve and dried to obtain the color-fixing protective glaze.
[0096] Example 5
[0097] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0098] Feldspar: 40 parts;
[0099] Zinc oxide: 10 parts;
[0100] Tin oxide: 5 parts;
[0101] Iron oxide: 3 parts;
[0102] Zirconia: 15 parts;
[0103] Silicon oxide: 17 parts;
[0104] 3-Aminopropyltriethoxysilane grafted polyethylene glycol: 2 parts.
[0105] The preparation method of 3-aminopropyltriethoxysilane grafted polyethylene glycol comprises the following steps:
[0106] Polyethylene glycol and 3-aminopropyltriethoxysilane are mixed to obtain a reaction raw material, and the reaction raw material is added to a solvent with stirring, and sodium hydroxide is added at the same time, and heated to 70° C. for reaction for 2 hours. After the reaction is completed, the solution is cooled and concentrated under reduced pressure to obtain 3-aminopropyltriethoxysilane grafted polyethylene glycol.
[0107] The solvent is ethanol.
[0108] The polyethylene glycol is PEG-6000.
[0109] The mass ratio of the polyethylene glycol to 3-aminopropyltriethoxysilane is 16:1.
[0110] The mass ratio of the reaction raw materials to the solvent is 15:100.
[0111] The mass ratio of the reaction raw materials to sodium hydroxide is 1:0.06.
[0112] The preparation method of the color-fixing protective glaze comprises the following steps:
[0113] By mass, 40 parts of feldspar, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide, 17 parts of silicon oxide, and 2 parts of 3-aminopropyltriethoxysilane grafted polyethylene glycol are mixed, 40 parts of water are added for ball milling, the mixture is passed through a 400-mesh sieve, and dried to obtain the color-fixing protective glaze.
[0114] Comparative Example 1
[0115] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0116] Feldspar: 40 parts;
[0117] Calcium borate: 10 parts;
[0118] Zinc oxide: 10 parts;
[0119] Tin oxide: 5 parts;
[0120] Iron oxide: 3 parts;
[0121] Zirconia: 15 parts;
[0122] Silicon oxide: 17 parts;
[0123] 3-Aminopropyltriethoxysilane grafted polyethylene glycol: 2 parts.
[0124] The preparation method of 3-aminopropyltriethoxysilane grafted polyethylene glycol comprises the following steps:
[0125] Polyethylene glycol and 3-aminopropyltriethoxysilane are mixed to obtain a reaction raw material, and the reaction raw material is added to a solvent with stirring, and sodium hydroxide is added at the same time, and heated to 70° C. for reaction for 2 hours. After the reaction is completed, the solution is cooled and concentrated under reduced pressure to obtain 3-aminopropyltriethoxysilane grafted polyethylene glycol.
[0126] The solvent is ethanol.
[0127] The polyethylene glycol is PEG-600.
[0128] The mass ratio of the polyethylene glycol to 3-aminopropyltriethoxysilane is 16:1.
[0129] The mass ratio of the reaction raw materials to the solvent is 15:100.
[0130] The mass ratio of the reaction raw materials to sodium hydroxide is 1:0.06.
[0131] The preparation method of the color-fixing protective glaze comprises the following steps:
[0132] By mass, 40 parts of feldspar, 10 parts of calcium borate, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide, 17 parts of silicon oxide, and 2 parts of 3-aminopropyltriethoxysilane grafted polyethylene glycol are mixed, 40 parts of water are added for ball milling, the mixture is sieved through a 400-mesh sieve, and dried to obtain the color-fixing protective glaze.
[0133] Comparative Example 2
[0134] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0135] Feldspar: 40 parts;
[0136] Calcium borate: 10 parts;
[0137] Zinc oxide: 10 parts;
[0138] Tin oxide: 5 parts;
[0139] Iron oxide: 3 parts;
[0140] Zirconia: 15 parts;
[0141] Silicon oxide: 17 parts;
[0142] 3-Aminopropyltriethoxysilane grafted polyethylene glycol: 2 parts.
[0143] The preparation method of 3-aminopropyltriethoxysilane grafted polyethylene glycol comprises the following steps:
[0144] Polyethylene glycol and 3-aminopropyltriethoxysilane are mixed to obtain a reaction raw material, and the reaction raw material is added to a solvent with stirring, and sodium hydroxide is added at the same time, and heated to 70° C. for reaction for 2 hours. After the reaction is completed, the solution is cooled and concentrated under reduced pressure to obtain 3-aminopropyltriethoxysilane grafted polyethylene glycol.
[0145] The solvent is ethanol.
[0146] The polyethylene glycol is PEG-10000.
[0147] The mass ratio of the polyethylene glycol to 3-aminopropyltriethoxysilane is 16:1.
[0148] The mass ratio of the reaction raw materials to the solvent is 15:100.
[0149] The mass ratio of the reaction raw materials to sodium hydroxide is 1:0.06.
[0150] The preparation method of the color-fixing protective glaze comprises the following steps:
[0151] By mass, 40 parts of feldspar, 10 parts of calcium borate, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide, 17 parts of silicon oxide, and 2 parts of 3-aminopropyltriethoxysilane grafted polyethylene glycol are mixed, 40 parts of water are added for ball milling, the mixture is sieved through a 400-mesh sieve, and dried to obtain the color-fixing protective glaze.
[0152] Comparative Example 3
[0153] A color fixing protective glaze for a hot-bent integrated basin, comprising the following raw materials in parts by mass:
[0154] Feldspar: 40 parts;
[0155] Calcium borate: 10 parts;
[0156] Zinc oxide: 10 parts;
[0157] Tin oxide: 5 parts;
[0158] Iron oxide: 3 parts;
[0159] Zirconia: 15 parts;
[0160] Silicon oxide: 17 parts.
[0161] The preparation method of the color-fixing protective glaze comprises the following steps:
[0162] By mass, 40 parts of feldspar, 10 parts of calcium borate, 10 parts of zinc oxide, 5 parts of tin oxide, 3 parts of iron oxide, 15 parts of zirconium oxide and 17 parts of silicon oxide are mixed, 40 parts of water are added for ball milling, the mixture is passed through a 400-mesh sieve and dried to obtain the color-fixing protective glaze.
[0163] Test Example 1:
[0164] A conventional black pigment and the color fixing protective glaze prepared in each embodiment of the present invention and the comparative example were mixed in a mass ratio of 1:2, and placed in a thermogravimetric analyzer for thermogravimetric treatment under air atmosphere. In the first stage, the room temperature was raised to 680°C at a heating rate of 15°C / min; in the second stage, the temperature was raised to 850°C at a heating rate of 10°C / min; in the third stage, the temperature was raised to 1205°C at 3°C / min and kept warm for 240 minutes; in the fourth stage, the temperature was cooled to room temperature at 5°C / min, pigment+protective glaze=90 mg, and the total ignition loss was obtained.
[0165] Another 60 mg of the protective glaze was taken and subjected to thermogravimetric treatment in the same manner to obtain the ignition loss of the protective glaze.
[0166] (Total loss on ignition - loss on ignition of protective glaze) / 30mg = loss on ignition of pigment
[0167] Table 1: Pigment loss on ignition
[0168] Pigment loss on ignition / % Example 1 0.42 Example 2 0.61 Example 3 0.54 Example 4 0.97 Example 5 0.69 Comparative Example 1 0.81 Comparative Example 2 0.72 Comparative Example 3 0.93
[0169] Test Example 2
[0170] A method for preparing a thermally bent rock plate integrated basin, characterized in that it comprises the following steps:
[0171] (1) taking raw materials for a green body layer, preparing a green body layer, and firing the raw materials to obtain a green body;
[0172] (2) performing inkjet printing decoration on the surface of the blank to obtain a printed blank;
[0173] (3) applying a color fixing protective glaze to the surface of the printed blank to obtain a hot-bent rock plate;
[0174] (4) The portion of the hot-bend rock slab to be bent is subjected to hot-bending treatment to obtain the hot-bend rock slab integrated basin.
[0175] The sintering temperature in step (1) is 1250° C. and the sintering time is 80 min.
[0176] The hot bending in step (4) is divided into four stages: in the first stage, the temperature is put into the kiln to 680°C, and the heating rate is 15°C / min; in the second stage, the temperature is increased to 850°C at a heating rate of 10°C / min; in the third stage, the temperature is increased to 1205°C at 3°C / min and kept warm for 240 minutes; in the fourth stage, the temperature is cooled to room temperature at 5°C / min.
[0177] When the color fixing protective glaze is used, water accounting for 50% of the weight of the glaze itself is added for grinding to obtain glaze slurry, and then the glazing operation is performed on the surface of the hot-bent integrated basin.
[0178] Observe whether the inkjet printing is blurred by naked eyes
[0179] Table 2: Changes in inkjet printing before and after heat bending
[0180] Inkjet printing changes Example 1 Clarity Example 2 With rough edges Example 3 Clarity Example 4 Vague Example 5 With rough edges Comparative Example 1 Vague Comparative Example 2 Vague Comparative Example 3 Vague
[0181] As can be seen from Table 1, the protective glaze formula of Example 1 with feldspar, calcium borate, zinc oxide, tin oxide, iron oxide, zirconium oxide, silicon oxide, and 3-aminopropyl triethoxysilane grafted polyethylene glycol as raw materials can reduce the burning loss of pigments to the greatest extent. The burning loss of pigments in Example 2 and Example 4 is increased compared with Example 1. The present invention believes that this is because the triethoxysilane group has unique chemical properties and can form a stable network structure with other silicon oxides at high temperatures to prevent adverse chemical reactions at high temperatures. Polyethylene glycol can improve the fluidity of the glaze, so that the glaze can be more evenly covered on the surface of the substrate, and it acts to form a uniform glaze layer at a low temperature. 3-aminopropyl triethoxysilane grafted polyethylene glycol has the properties of both, which can enhance the protective effect of the protective glaze to a greater extent and reduce the burning loss of pigments. Example 3 uses a copolymer of polyol and polysiloxane as an additive, and its effect is also slightly worse than that of Example 1. The present invention believes that this is because its fluidity and connectivity are not as good as 3-aminopropyl triethoxysilane grafted polyethylene glycol. Example 5 does not add calcium borate. Calcium borate decomposes at high temperature to generate CaO and B2O3. CaO is a stabilizer, which can reduce the impact of polyethylene glycol burning loss, and B2O3 acts as a flux to enhance the fluidity and uniformity of the glaze, and improve the viscosity and adsorption of the glaze layer, which helps to enhance the stability of the pigment. Comparative Example 1 uses PEG-600, which is more volatile at high temperatures and has a poor protective effect. Comparative Example 2 uses PEG-10000, which has too high viscosity and is not easy to cover evenly, affecting the performance of the glaze. The performance of the finished product of Test Example 2 also confirms the test results of Test Example 1.
[0182] The protective glaze formula of the present invention, which uses feldspar, calcium borate, zinc oxide, tin oxide, iron oxide, zirconium oxide, silicon oxide, and 3-aminopropyltriethoxysilane grafted polyethylene glycol as raw materials, is suitable for the hot-bending one-piece basin process that requires high-temperature treatment, can minimize the burning loss of pigments, and increase the beauty of the hot-bending one-piece basin.
Claims
1. A color fixing protective glaze for hot-bending integrated basins, characterized in that: The following raw materials are included by mass: Feldspar: 35-45 parts; Calcium borate: 5-15 parts; Zinc oxide: 5-15 parts; Tin oxide: 1-10 parts; Iron oxide: 1-5 parts; Zirconia: 10-20 parts; Silicon oxide: 15-20 parts; 3-Aminopropyltriethoxysilane grafted polyethylene glycol: 1-3 parts; The preparation method of 3-aminopropyl triethoxysilane grafted polyethylene glycol comprises the following steps: mixing polyethylene glycol and 3-aminopropyl triethoxysilane to obtain a reaction raw material, adding the reaction raw material into a solvent and stirring, adding sodium hydroxide at the same time, and heating to 60-80° C. to react for 1-2 hours, and after the reaction is completed, cooling the solution, and concentrating under reduced pressure to obtain 3-aminopropyl triethoxysilane grafted polyethylene glycol; The molecular weight of the polyethylene glycol is 4000-8000 Da; The mass ratio of the polyethylene glycol to 3-aminopropyltriethoxysilane is (4-20):
1.
2. The color fixing protective glaze for hot-bending integrated basins according to claim 1, characterized in that: The solvent is one of toluene or ethanol.
3. The color fixing protective glaze for hot-bending integrated basins according to claim 1, characterized in that: The mass ratio of the reaction raw materials to the solvent is (1-20):
100.
4. The color fixing protective glaze for hot-bending integrated basins according to claim 1, characterized in that: The mass ratio of the reaction raw materials to sodium hydroxide is 1:(0.01-0.1).
5. A method for preparing a color-fixing protective glaze for a hot-bending integrated basin according to any one of claims 1 to 4, characterized in that: The following steps are involved: By weight, 35-45 parts of feldspar, 5-15 parts of calcium borate, 5-15 parts of zinc oxide, 1-10 parts of tin oxide, 1-5 parts of iron oxide, 10-20 parts of zirconium oxide, 15-20 parts of silicon oxide and 1-3 parts of 3-aminopropyl triethoxysilane grafted polyethylene glycol are mixed, 30-50 parts of water are added for ball milling, the mixture is sieved through a 350-450 mesh sieve and dried to obtain the color fixing protective glaze.