Self-excited hydrophobic industrial solid waste-based cementitious materials, their preparation methods and application methods
By using self-excited hydrophobic industrial solid waste-based cementitious materials, an interpenetrating network structure is formed by utilizing the inherent properties of industrial solid waste. This solves the problems of difficult co-disposal of industrial solid waste and hydrophilicity, thereby improving the early strength and durability of high-performance cementitious materials and reducing preparation and construction costs.
Patent Information
- Application Number
- CN202410563074.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-08
AI Technical Summary
Existing technologies are unable to effectively utilize industrial solid waste and solve the problems of easy frost heave, corrosion and low durability caused by its hydrophilicity. In addition, traditional activators have problems of environmental pollution and high energy consumption.
A self-activating hydrophobic industrial solid waste-based cementitious material is adopted. By rationally adjusting industrial solid waste, active components, catalysts and auxiliary agents, an interpenetrating network structure is formed, which reduces hydrophilicity and improves corrosion resistance. The self-activation of the material is achieved by utilizing the inherent properties of industrial solid waste.
This technology enables high-performance cementitious materials to achieve high early-stage strength, continuous enhancement of later-stage strength, low shrinkage, high density, good impermeability, and good hydrophobicity. It is suitable for various environments, reduces preparation and construction costs, and improves resource utilization efficiency and environmental benefits.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste recycling technology, and in particular to a self-excited hydrophobic industrial solid waste-based cementitious material, its preparation method, and its application method. Background Technology
[0002] While accelerating industrialization and promoting rapid economic and urban development, my country has generated a large amount of industrial solid waste, such as calcium carbide slag, red mud, tungsten ore slag, copper slag, and industrial by-product gypsum. Calcium carbide slag, a byproduct of acetylene production from calcium carbide hydrolysis, has a pH value exceeding 12 and is highly alkaline; my country's annual production exceeds 28 million tons. Tungsten ore slag is a solid material formed after dewatering of the tailings slurry with extremely low mineral content discharged from the grinding and fine selection of tungsten ore; as of 2020, the accumulated amount of tungsten ore slag in China reached 22.26 billion tons. Red mud is a type of harmful, highly alkaline industrial waste generated during alumina refining; China's accumulated red mud is approximately 600 million tons, with an annual new generation exceeding 70 million tons. Copper slag is a major solid waste discharged from pyrometallurgical copper refining; in recent years, China's annual increase in copper slag has averaged 14 million tons. Industrial by-product gypsum, primarily composed of calcium sulfate dihydrate, is a byproduct of industrial waste production. Currently, the total accumulated stockpile of industrial by-product gypsum in my country exceeds 500 million tons. The long-term accumulation of this industrial solid waste not only occupies vast amounts of land resources but also causes serious pollution and harm to water systems and the atmosphere, damaging the ecosystem, wasting resources, and drawing public attention. Solving the problem of industrial solid waste stockpiling and achieving its harmless treatment and resource utilization is an urgent issue that needs to be addressed.
[0003] For decades, both domestically and internationally, most methods have employed activators to revitalize these solid wastes for the preparation of alkali-activated cementitious materials. These activators include strongly alkaline sodium hydroxide and sodium silicate, as well as silicate cement clinker. However, the use of strongly alkaline activators like sodium hydroxide easily pollutes water resources and harms human health; the calcination process of silicate cement clinker not only consumes large amounts of resources but also easily produces toxic and harmful gases. These factors significantly limit its application in practical engineering. Furthermore, in actual use, the activation properties of different industrial solid wastes vary considerably. The aforementioned activator materials have limited activation effects on different industrial solid wastes, making it difficult to generate the target hydration products, thus hindering the co-processing of different industrial solid wastes.
[0004] Therefore, developing a high-performance industrial solid waste-based cementitious material that can utilize the inherent properties of industrial solid waste to achieve self-activation has significant economic and environmental benefits. Furthermore, both industrial solid waste-based cementitious materials and cement-based materials are hydrophilic, and water is the primary medium for frost heave and corrosive ion attack in concrete structures. Therefore, while ensuring the high performance of industrial solid waste-based cementitious materials, how to reduce their hydrophilicity to improve their durability is also a problem that needs to be studied and solved. Summary of the Invention
[0005] This invention provides a self-activated hydrophobic industrial solid waste-based cementitious material, its preparation method, and its application method. This cementitious material utilizes the inherent characteristics of industrial solid waste to achieve its self-activated activity, thereby solving the problems of difficulty in co-disposing of different industrial solid wastes and the high hydrophilicity of existing industrial solid waste-based cementitious materials, which leads to susceptibility to frost heave, erosion, and low durability.
[0006] In a first aspect, the present invention provides a self-activated hydrophobic industrial solid waste-based cementitious material comprising the following raw materials in parts by weight: 75-118 parts of component A and 3-6 parts of component B; component A comprises: industrial solid waste, active component and catalyst; component B comprises auxiliary agent.
[0007] The cementitious material obtained by this invention has the characteristics of high early strength, continuous enhancement of later strength, low shrinkage rate, high density, good impermeability, hydrophobicity, and high corrosion resistance (especially resistance to salt erosion). The 7-day compressive strength is not less than 40 MPa, and the 28-day compressive strength is not less than 70 MPa. At the same time, its 28-day volume shrinkage rate does not exceed 0.08%. Various raw materials complement each other and form a complementary advantage. They can be activated and reacted by utilizing their own characteristics. While ensuring the high performance of the cementitious material, the strength and durability of the cementitious material are improved. Moreover, the contact angle between the cementitious material and water is 90°-120°, which shows good hydrophobicity and resistance to corrosive media. It reduces its hydrophilicity to achieve the purpose of improving the service life of the project. It can be used and promoted as a substitute for silicate cementitious materials, reducing the use of commonly used high-consumption and high-carbon-emission cement. The main raw materials are made from bulk industrial solid waste, which improves environmental protection benefits and reduces preparation and construction costs.
[0008] Preferably, the active component includes one or more of silica fume, metakaolin, and glass powder.
[0009] Preferably, the catalyst comprises one or more of phosphates, carbonates, and alkanolamines. In addition to promoting the polymerization and grafting of the hydrolysis products of the auxiliary agent onto the molecular chains of the gel precursor, the catalyst can also accelerate the release of active ions (such as metal ions, silicate ions, etc.) from components in industrial solid waste, and form hydration products with an interpenetrating network structure in the gel, increasing the density inside the gel. Simultaneously, it also links itself within the gel structure, strengthening the bond strength between inorganic and organic components, thereby enhancing the cohesiveness within the cementitious material and improving its strength.
[0010] Preferably, the auxiliary agents include multiples selected from methyltrimethoxysilane, 3-aminopropyltriethoxysilane, γ-glycidyl etheroxypropyltrimethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane. In the later stages of the reaction, the hydrolysis products of the auxiliary agents, under the action of a catalyst, are grafted into the gel precursor system through polymerization. This introduces hydrophobic functional groups such as methyl groups at the ends of the molecular chains of the gel's three-dimensional network structure, reducing the affinity of the cementitious material for water and decreasing the diffusion coefficient of water and external ions within the cementitious material. This enhances the cementitious material's resistance to frost heave and erosion, while also preserving the internal environment of the cementitious material. It possesses good integrity and a dense porous structure, thus continuously providing strength development, with sustained strength enhancement in later stages, expanding its applicability.
[0011] Preferably, the industrial solid waste includes one or more of the following: carbide slag, tungsten slag, red mud, copper slag, mineral slag, and industrial by-product gypsum.
[0012] Preferably, component A comprises the following components in parts by weight: 50-70 parts of industrial solid waste, 20-40 parts of active component and 5-8 parts of catalyst.
[0013] Preferably, the phosphate includes one or more of sodium pyrophosphate, sodium tripolyphosphate, sodium polyphosphate, potassium phosphate, and ammonium phosphate.
[0014] Preferably, the alcoholamine includes one or more of monoethanolamine, diethanolamine, triethanolamine, and monoisopropanolamine.
[0015] Preferably, the carbonate includes one or more of sodium carbonate, potassium carbonate, calcium carbonate, and sodium bicarbonate.
[0016] Preferably, the industrial solid waste comprises the following components in parts by weight: 10-15 parts calcium carbide slag, 5-10 parts tungsten ore slag, 10-15 parts red mud, 5-10 parts copper slag, 20-60 parts ore slag, and 2-5 parts industrial by-product gypsum. More preferably, the moisture content of the industrial solid waste does not exceed 1%.
[0017] Preferably, the industrial by-product gypsum includes one or more of phosphogypsum, titanium gypsum, fluorogypsum, and desulfurized gypsum.
[0018] Preferably, the calcium oxide content in the carbide slag is not less than 60%, and the specific surface area is not less than 600 m². 2 / kg, moisture content not exceeding 1%.
[0019] Preferably, the specific surface area of tungsten slag is not less than 600 m². 2 / kg, moisture content not exceeding 1%.
[0020] Preferably, the red mud is Bayer process red mud with a specific surface area of not less than 600 m². 2 / kg, moisture content not exceeding 1%.
[0021] Preferably, the copper slag is high-temperature water-quenched slag, which has undergone magnetic separation pretreatment and has a specific surface area of not less than 600 m². 2 / kg, moisture content not exceeding 1%.
[0022] Preferably, the slag is granulated blast furnace slag with a specific surface area of not less than 600 m². 2 / kg, moisture content not exceeding 1%.
[0023] Preferably, the specific surface area of industrial by-product gypsum is not less than 600 m². 2 / kg, moisture content not exceeding 1%.
[0024] When the various components of the aforementioned industrial solid waste are used in combination, they can exert synergistic and self-activating effects. The sodalite-type silica slag (Na₂O·Al₂O₃·xSiO₂·nH₂O) and nepheline-type silica slag (Na₂O·Al₂O₃·xSiO₂·yCaCO₃·nH₂O) present in the Bayer process red mud have very high alkali concentrations. Under the interaction of carbide slag and industrial by-product gypsum, the CaO concentration in the cementitious material system increases significantly. 2+ and OH - Increased concentration. The combined effect of the above factors leads to increased alkalinity and calcium content in the system, accelerating the breaking of Si-O and Al-O bonds in several industrial solid wastes, thereby forming silicon and aluminum oligomers (-Si-O-Na, -Si-O-Ca-OH, Al(OH)4) in the system. - Al(OH)5 2- Al(OH)6 3- Calcium ions combine with oligomers to form CSH and CASH gels. In the CaO-SiO2-Al2O3 system of slag, FeO-SiO2 system of copper slag, and FeO-CaO-SiO2 system of tungsten slag, under the action of catalysts and industrial by-product gypsum, Fe... 2+ SiO3 2- Ca 2+ And Al 3+The gypsum polymerizes to form ferric hydration products, which then form an interpenetrating network structure with CSH and CASH gels, increasing the density of the cementitious material system. Simultaneously, industrial by-product gypsum provides Ca... 2+ and SO4 2- CSH reacts with it to form crystalline hydrated calcium sulfoaluminate, such as interlocking needle-like structures and highly water-bound AFt crystals, which interweave with the hydrated gel to provide strength, fill the pores, and improve the strength of the cementitious material.
[0025] A further advantage lies in the fact that, in environments with high salt content (such as marine environments and saline-alkali environments), the cementitious material of this invention, due to its poor hydrophilicity, makes it difficult for external corrosive ions to penetrate its interior through diffusion. The physicochemical environment inside the cementitious material system remains largely unchanged, the polymerization reaction to form a gel continues, the density of the cementitious material structure continuously increases, and its strength is significantly improved. Furthermore, the Na+ contained in the saline environment... + K + Ca 2+ Mg 2+ SO4 2- and HCO3 - CO3 2- Fe dissociated from industrial solid waste 2+ SiO3 2- Ca 2+ And Al 3+ Through polymerization reactions, gels are formed, which increases the gel content and density of the cementitious material system, improves the internal pore structure of the cementitious material, and especially reduces the loss rate of flexural and compressive strength in continuous immersion environments, thereby increasing the durability of the cementitious material and the service life of the project.
[0026] Preferably, the active component comprises the following components in parts by weight: 15-70 parts silica fume, 20-80 parts metakaolin, and 5-10 parts glass powder. When the various components of the active component are used in combination, the simultaneous introduction of silica fume, metakaolin, and glass powder can improve the silica-alumina ratio (Si / Al) in the gel system, particularly increasing the content of Si-O-Si bonds in the gel system, thereby further enhancing the strength of the cementitious material.
[0027] Preferably, the glass powder includes one or more of silicate glass, borate glass, and phosphate glass.
[0028] Preferably, the specific surface area of the active component is not less than 400 m². 2 / kg.
[0029] Preferably, the silica content in the silica ash is greater than 85%, and the moisture content is no more than 1%.
[0030] Preferably, the metakaolin contains not less than 52% silica, not less than 42% alumina, and has a moisture content of not more than 1%.
[0031] Preferably, the specific surface area of the glass powder is not less than 600 m². 2 / kg.
[0032] Preferably, there are at least two types of catalysts. Similarly, there are at least two types of auxiliary agents. It is preferable to use different types of catalysts and auxiliary agents in combination. Compared with using a single type, the combined catalyst and auxiliary agents can more fully activate different raw materials, promote more complete reaction of different raw material components, and thus further improve the strength and durability of the cementitious material.
[0033] Preferably, the above-mentioned self-excited hydrophobic industrial solid waste-based cementitious material is used as a cementitious material in building materials.
[0034] In a second aspect, the present invention provides a method for preparing a self-excited hydrophobic industrial solid waste-based cementitious material as described in the first aspect above, comprising the following steps: mixing industrial solid waste, active components and catalysts to obtain component A; and mixing at least two types of auxiliary agents to obtain component B.
[0035] The preparation method of the gelling material of the present invention is simple, and the preparation process does not require high-temperature calcination, resulting in low energy consumption and improved preparation efficiency. Furthermore, it uses industrial solid waste as raw material, enabling the synergistic utilization of multiple solid wastes without consuming natural mineral resources. The preparation and construction costs are low, and the relevant performance fully meets the requirements. It also reduces the volume of solid waste, increases the added value of industrial solid waste, and reduces carbon emissions. Under the dual-carbon background, it has significant economic, environmental, and social benefits.
[0036] Thirdly, the present invention provides a method for using a self-activated hydrophobic industrial solid waste-based cementitious material, wherein the cementitious material is the self-activated hydrophobic industrial solid waste-based cementitious material of the first aspect above, or the self-activated hydrophobic industrial solid waste-based cementitious material prepared by the preparation method of the second aspect above, comprising the following steps:
[0037] Step 1): Mix component A with water and stir for 5-10 minutes to obtain the cementitious material precursor;
[0038] Step 2): Mix component B with water and stir at a constant speed of 50-200 r / min for 10-30 min to obtain a mixture;
[0039] Step 3): Add the mixture to the cementitious material precursor, mix evenly, and then cure and solidify to complete the use of the self-excited hydrophobic industrial solid waste-based cementitious material.
[0040] When used, the cementitious material of the present invention has cementitious properties similar to those of traditional cement, and can be quickly cured and molded, which greatly shortens the construction period and improves work efficiency. Components A and B undergo dissolution and hydrolysis during the mixing process with water. During the mixing process of the cementitious material precursor and the mixture, a denser interpenetrating network structure is further formed through polymerization and grafting, so that the components complement each other and improve the strength, water resistance and durability of the cementitious material.
[0041] Preferably, in the above-described method of use, the ratio of total water consumption to the weight of the cementitious material is (0.2-0.3):1. More preferably, the ratio of total water consumption to the weight of the cementitious material during use is 0.25:1. During use, controlling an appropriate water-cement ratio can reduce the porosity inside the cementitious material, allowing it to exhibit optimal cohesiveness and adhesiveness. This results in the cementitious material having higher strength, impermeability, and durability after curing, thus extending its service life.
[0042] Preferably, in step 1), the water used for component A accounts for 65-75% of the total water used, and the remaining water is used in step 2) for preparing the mixture from component B. More preferably, the water used for component A accounts for 70% of the total water used.
[0043] Preferably, in step 3), the cementitious material precursor and the mixture are mixed for 5-15 minutes.
[0044] It should be noted that the curing of the gelling material of the present invention is not specifically limited, and it can be cured and solidified under conditions such as room temperature environment, water environment, and saline-alkali environment.
[0045] The self-activating hydrophobic industrial solid waste-based cementitious material provided by this invention, through the rational adjustment of the proportions of industrial solid waste, active components, catalysts and auxiliary agents, enables each component to fully utilize its own characteristics to activate and participate in the reaction. By introducing water-transporting groups into the gel system, the cementitious material's resistance to frost heave and erosion is enhanced. This results in a cementitious material with high early strength, continuously increasing strength in the later stage, low shrinkage, high density, good impermeability, hydrophobicity and high corrosion resistance (especially resistance to salt erosion), which can be used and promoted as a substitute for silicate cementitious materials.
[0046] The preparation method of this cementitious material does not require high-temperature calcination and has low energy consumption. While ensuring the high performance of industrial solid waste-based cementitious materials, it improves the durability of industrial solid waste-based cementitious materials by reducing their hydrophilicity. It also realizes the synergistic utilization of multiple solid wastes, with low preparation and construction costs, reducing the volume of solid waste and increasing the added value of industrial solid waste.
[0047] When using this cementitious material, components A and B are first reacted and hydrolyzed in water, and then they are mixed together to further react, polymerize, and / or graft to form a denser and stronger gel structure. In a salt environment, this cementitious material can continuously improve its strength and structural density, exhibiting excellent resistance to frost heave and corrosion, thus expanding its application range. It can be used in components with high strength requirements and in emergency repair projects, and / or in environments susceptible to salt corrosion, significantly improving the service life of projects and reducing construction costs. Detailed Implementation
[0048] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are also within the scope of protection of the present invention.
[0049] The following examples use conventional instruments and equipment in the art. Unless otherwise specified, the experimental materials and reagents used in the following examples are commercially available and conform to conventional specifications in the art. Any techniques or conditions not specifically described in the following examples can be performed according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0050] It should be noted that, in this invention and the following embodiments, unless otherwise specified, concentration, ratio, etc. are all weight concentration, weight ratio, etc., "%" all represent weight percentage, and "parts" all represent weight parts. These are common writing habits used by those skilled in the art, and therefore will not be repeated in this invention.
[0051] The present invention will be further described in detail below with reference to embodiments. However, it should be understood that the embodiments are for illustrative purposes only and are not intended to limit the scope of the present invention.
[0052] The materials used in all the following examples and comparative examples are consistent. Specifically, the moisture content of the industrial solid waste does not exceed 1%; wherein, the calcium oxide content in the calcium carbide slag is not less than 60%, and the specific surface area is not less than 600 m². 2 / kg; tungsten slag specific surface area not less than 600m² 2 / kg; the red mud is Bayer process red mud with a specific surface area of not less than 600 m². 2 / kg; the copper slag is high-temperature water-quenched slag, which has undergone magnetic separation pretreatment and has a specific surface area of not less than 600 m². 2 / kg; the slag is granulated blast furnace slag with a specific surface area of not less than 600 m². 2 / kg; Industrial by-product gypsum with a specific surface area of not less than 600m²2 / kg. Furthermore, the silica content in the silica fume is greater than 85%, and its specific surface area is not less than 400m². 2 / kg; the silica content in metakaolin is not less than 52%, the alumina content is not less than 42%, and its specific surface area is not less than 400 m². 2 / kg; the specific surface area of the glass powder is not less than 600m². 2 / kg.
[0053] Example 1:
[0054] A self-excited hydrophobic industrial solid waste-based cementitious material comprises the following raw materials in parts by weight: 95 parts of component A and 5 parts of component B; wherein, component A comprises: 60 parts of industrial solid waste, 30 parts of active component and 5 parts of catalyst; and component B comprises 5 parts of auxiliary agent.
[0055] More specifically, the industrial solid waste includes: 60 parts slag, 15 parts calcium carbide slag, 10 parts red mud, 5 parts copper slag, 5 parts tungsten slag, 3 parts phosphogypsum, and 2 parts fluorogypsum; the active components include: 15 parts silica fume, 75 parts metakaolin, and 10 parts silicate glass powder; the catalyst includes: 25% sodium phosphate, 25% sodium carbonate, 30% ammonium phosphate, and 20% potassium carbonate; the auxiliary agents include: 50% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane, and 30% γ-methacryloyloxypropyltrimethoxysilane.
[0056] The preparation method of the above-mentioned cementitious material includes the following steps:
[0057] 1) Mix 60 parts of industrial solid waste, 30 parts of active component and 5 parts of catalyst to obtain component A;
[0058] 2) Mix 50% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane and 30% γ-methacryloyloxypropyltrimethoxysilane to obtain component B.
[0059] The method of using the above-mentioned cementitious material includes the following steps:
[0060] Step 1): Mix component A with water accounting for 70% of the total water volume and stir for 8 minutes to obtain the cementitious material precursor;
[0061] Step 2): Mix component B with the remaining water, which accounts for 30% of the total water volume, and stir at a constant speed of 150 r / min for 20 min to obtain a mixture; the ratio of the total water volume to the weight of the cementitious material is 0.25:1.
[0062] Step 3): Add the mixture to the cementitious material precursor, mix for 8 minutes, and then cure and solidify to complete the use of the self-excited hydrophobic industrial solid waste-based cementitious material.
[0063] Example 2:
[0064] A self-excited hydrophobic industrial solid waste-based cementitious material comprises the following raw materials in parts by weight: 95 parts of component A and 5 parts of component B; wherein, component A comprises: 55 parts of industrial solid waste, 32 parts of active component and 8 parts of catalyst; and component B comprises 5 parts of auxiliary agent.
[0065] More specifically, the industrial solid waste includes: 56 parts slag, 10 parts calcium carbide slag, 10 parts red mud, 6 parts copper slag, 8 parts tungsten slag, and 5 parts titanium gypsum; the active components include: 20 parts silica fume, 70 parts metakaolin, and 10 parts borosilicate glass powder; the catalyst includes: 20% sodium phosphate and 80% sodium carbonate; the auxiliary agents include: 40% 3-aminopropyltriethoxysilane and 60% γ-glycidoxypropyltrimethoxysilane.
[0066] The preparation method of the above-mentioned cementitious material includes the following steps:
[0067] 1) Mix the above 55 parts of industrial solid waste, 32 parts of active component and 8 parts of catalyst to obtain component A;
[0068] 2) Mix 40% of 3-aminopropyltriethoxysilane and 60% of γ-glycidoxypropyltrimethoxysilane to obtain component B.
[0069] The method of using the above-mentioned cementitious material includes the following steps:
[0070] Step 1): Mix component A with water accounting for 65% of the total water volume and stir for 10 minutes to obtain the cementitious material precursor;
[0071] Step 2): Mix the above component B with the remaining water, which accounts for 35% of the total water volume, and stir at a constant speed of 100 r / min for 10 min to obtain a mixture; the ratio of the total water volume to the weight of the cementitious material is 0.2:1.
[0072] Step 3): Add the mixture to the cementitious material precursor, mix for 10 minutes, then cure and solidify to complete the use of the self-excited hydrophobic industrial solid waste-based cementitious material.
[0073] Example 3:
[0074] A self-excited hydrophobic industrial solid waste-based cementitious material comprises the following raw materials in parts by weight: 95 parts of component A and 5 parts of component B; wherein, component A comprises: 60 parts of industrial solid waste, 28 parts of active component and 7 parts of catalyst; and component B comprises 5 parts of auxiliary agent.
[0075] More specifically, the industrial solid waste includes: 55 parts slag, 15 parts calcium carbide slag, 15 parts red mud, 5 parts copper slag, 5 parts tungsten slag, 2 parts phosphogypsum, and 3 parts desulfurization gypsum; the active components include: 20 parts silica fume, 75 parts metakaolin, 3 parts phosphate glass powder, and 2 parts silicate glass powder; the catalyst includes: 25% sodium phosphate, 25% sodium carbonate, 30% ammonium phosphate, 10% potassium phosphate, and 10% potassium carbonate; the auxiliary agents include: 30% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane, 20% γ-glycidyl etheroxypropyltrimethoxysilane, and 30% γ-methacryloyloxypropyltrimethoxysilane.
[0076] The preparation method of the above-mentioned cementitious material includes the following steps:
[0077] 1) Mix the above 60 parts of industrial solid waste, 28 parts of active component and 7 parts of catalyst to obtain component A;
[0078] 2) Mix 30% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane, 20% γ-glycidoxypropyltrimethoxysilane and 30% γ-methacryloyloxypropyltrimethoxysilane to obtain component B.
[0079] The method of using the above-mentioned cementitious material includes the following steps:
[0080] Step 1): Mix component A with water accounting for 75% of the total water volume and stir for 10 minutes to obtain the cementitious material precursor;
[0081] Step 2): Mix the above component B with the remaining water, which accounts for 25% of the total water volume, and stir at a constant speed of 200 r / min for 30 min to obtain a mixture; the ratio of the total water volume to the weight of the cementitious material is 0.3:1.
[0082] Step 3): Add the mixture to the cementitious material precursor, mix for 6 minutes, then cure and solidify to complete the use of the self-excited hydrophobic industrial solid waste-based cementitious material.
[0083] Example 4:
[0084] A self-excited hydrophobic industrial solid waste-based cementitious material comprises the following raw materials in parts by weight: 95 parts of component A and 5 parts of component B; wherein, component A comprises: 65 parts of industrial solid waste, 25 parts of active component and 5 parts of catalyst; and component B comprises 5 parts of auxiliary agent.
[0085] More specifically, the industrial solid waste includes: 60 parts slag, 12 parts calcium carbide slag, 15 parts red mud, 5 parts copper slag, 6 parts tungsten slag, and 2 parts phosphogypsum; the active components include: 30 parts silica fume, 60 parts metakaolin, 5 parts phosphate glass powder, and 5 parts silicate glass powder; the catalyst includes: 25% sodium phosphate, 25% sodium carbonate, 15% ammonium phosphate, 10% potassium phosphate, 15% potassium carbonate, 5% monoethanolamine, and 5% diethanolamine; the auxiliary agents include: 40% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane, 20% γ-glycidoxypropyltrimethoxysilane, and 20% γ-methacryloyloxypropyltrimethoxysilane.
[0086] The preparation method of the above-mentioned cementitious material includes the following steps:
[0087] 1) Mix the above 65 parts of industrial solid waste, 25 parts of active component and 5 parts of catalyst to obtain component A;
[0088] 2) Mix 40% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane, 20% γ-glycidoxypropyltrimethoxysilane and 20% γ-methacryloyloxypropyltrimethoxysilane to obtain component B.
[0089] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 1.
[0090] Example 5:
[0091] A self-excited hydrophobic industrial solid waste-based cementitious material comprises the following raw materials in parts by weight: 95 parts of component A and 5 parts of component B; wherein, component A comprises: 70 parts of industrial solid waste, 20 parts of active component and 5 parts of catalyst; and component B comprises 5 parts of auxiliary agent.
[0092] More specifically, the industrial solid waste includes: 56 parts slag, 15 parts calcium carbide slag, 10 parts red mud, 9 parts copper slag, 7 parts tungsten slag, and 3 parts titanium gypsum; the active components include: 30 parts silica fume, 62 parts metakaolin, 4 parts phosphate glass powder, and 4 parts silicate glass powder; the catalyst includes: 20% sodium phosphate, 35% sodium carbonate, 15% ammonium phosphate, 10% potassium phosphate, 10% potassium carbonate, 5% monoethanolamine, and 5% diethanolamine; the auxiliary agents include: 40% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane, and 40% γ-methacryloyloxypropyltrimethoxysilane.
[0093] The preparation method of the above-mentioned cementitious material includes the following steps:
[0094] 1) Mix the above 70 parts of industrial solid waste, 20 parts of active component and 5 parts of catalyst to obtain component A;
[0095] 2) Mix 40% methyltrimethoxysilane, 20% 3-aminopropyltriethoxysilane and 40% γ-methacryloyloxypropyltrimethoxysilane to obtain component B.
[0096] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 1.
[0097] Example 6:
[0098] A self-excited hydrophobic industrial solid waste-based cementitious material, the raw materials and their weight parts are the same as in Example 5, the only difference being that the catalyst is 100% diethanolamine.
[0099] The preparation method of the above-mentioned cementitious material is the same as the preparation steps in Example 5.
[0100] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 5.
[0101] Example 7:
[0102] A self-excited hydrophobic industrial solid waste-based cementitious material, the raw materials and their weight parts are the same as in Example 5, the only difference being: the catalyst includes: 55% sodium phosphate, 25% ammonium phosphate, and 20% potassium phosphate.
[0103] The preparation method of the above-mentioned cementitious material is the same as the preparation steps in Example 5.
[0104] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 5.
[0105] Example 8:
[0106] A self-excited hydrophobic industrial solid waste-based cementitious material, the raw materials and their weight parts are the same as in Example 5, the only difference being that the catalyst includes: 55% sodium carbonate and 45% potassium carbonate.
[0107] The preparation method of the above-mentioned cementitious material is the same as the preparation steps in Example 5.
[0108] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 5.
[0109] Example 9:
[0110] A self-excited hydrophobic industrial solid waste-based cementitious material, the raw materials and their weight parts are the same as in Example 5, the only difference being that the auxiliary agent is 100% γ-methacryloyloxypropyltrimethoxysilane.
[0111] The preparation method of the above-mentioned cementitious material is the same as the preparation steps in Example 5.
[0112] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 5.
[0113] Example 10:
[0114] A self-excited hydrophobic industrial solid waste-based cementitious material, the raw materials and their weight parts are the same as in Example 5, the only difference being: the auxiliary agent is 100% γ-glycidoxypropyltrimethoxysilane.
[0115] The preparation method of the above-mentioned cementitious material is the same as the preparation steps in Example 5.
[0116] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 5.
[0117] Example 11:
[0118] A self-excited hydrophobic industrial solid waste-based cementitious material, the raw materials and their weight parts are the same as in Example 1, the only difference being that the active components include: 75 parts metakaolin and 10 parts silicate glass powder.
[0119] The preparation method of the above-mentioned cementitious material is the same as the preparation steps in Example 1.
[0120] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 1.
[0121] Example 12:
[0122] A self-excited hydrophobic industrial solid waste-based cementitious material, the raw materials and their weight parts are the same as in Example 1, the only difference being that the industrial solid waste includes: 60 parts of slag, 10 parts of red mud, 3 parts of phosphogypsum and 2 parts of fluorogypsum.
[0123] The preparation method of the above-mentioned cementitious material is the same as the preparation steps in Example 1.
[0124] The method of using the above-mentioned cementitious material is the same as the method of using it in Example 1.
[0125] Comparative Example 1:
[0126] A cementitious material comprises the following raw materials: slag material including 60% blast furnace slag, 10% copper slag, 15% tungsten slag, 9% fly ash, 5% phosphogypsum, and 1% grinding aid; and a composite activator comprising 35% SiO2 and 65% K2O. The aforementioned grinding aid consists of 25% anhydrous calcium chloride, 20% quicklime powder, and 55% a commonly used carrier.
[0127] The preparation method of the above-mentioned cementitious material includes the following steps: grinding 70 parts of slag and 30 parts of activator together, adding water and mixing to obtain the cementitious material.
[0128] Comparative Example 2:
[0129] A cementitious material comprises the following raw materials: 80 parts of industrial solid waste, 5 parts of active components, and 15 parts of activator. The industrial solid waste includes 65 parts of slag, 15 parts of tungsten slag, 10 parts of copper slag, 10 parts of red mud, and 5 parts of phosphogypsum; the active components include 15 parts of silica fume, 20 parts of metakaolin, and 65 parts of diatomaceous earth; the activator includes 20% sodium hydroxide, 15% potassium hydroxide, 15% sodium phosphate, and 50% water glass with a modulus of 3.5.
[0130] The preparation method of the above-mentioned gelling material includes the following steps: mixing 80 parts of industrial solid waste and 5 parts of active components evenly to obtain a mixture, then adding 15 parts of activator to the mixture and mixing evenly to obtain the gelling material.
[0131] Comparative Example 3:
[0132] A cementitious material comprises the following raw materials: slag material including 60% blast furnace slag, 10% tungsten slag, 15% red mud, 9% copper slag, 5% gypsum, and 1% grinding aid; a composite activator comprising 40% SiO2 and 60% K2O. The aforementioned grinding aid consists of 25% anhydrous calcium chloride, 20% quicklime powder, and 55% a commonly used carrier.
[0133] The preparation method of the above-mentioned cementitious material includes the following steps: 15 parts of composite activator are added to water to prepare a solution, left to stand for 24 hours, and then mixed and stirred with 85 parts of slag to obtain the cementitious material.
[0134] Experimental example:
[0135] The contact angle, 7-day and 28-day compressive strength, compressive strength in seawater erosion solution, and 28-day shrinkage rate of the cementitious materials obtained in the above embodiments and comparative examples were tested. The specific test methods are as follows:
[0136] The cementitious materials obtained in Examples 1-12 and Comparative Examples 1-3 were mixed with water at a water-cement ratio of 0.25, and then cast into molds with a mold size of 20×20×20mm. After curing at room temperature for 24 hours, the molded specimens were demolded and then water-cured to the specified age. Their 7-day and 28-day compressive strengths were measured. For specimens tested for seawater erosion resistance, they were first water-cured for 28 days, then cured in a seawater erosion solution for 180 days before being tested for compressive strength. For shrinkage testing, the specimens were cured in water for 2 days, then placed in a dry shrinkage curing chamber, and their shrinkage rate was measured at 25 days (28 days from molding). The contact angle between the cementitious material and water was measured using a JY-PHb contact angle tester, and the curing age of the specimens used in the contact angle test was 3 days. The compressive strength was determined according to GB / T17671-2021, and the seawater erosion solution was prepared according to the steps in GB / T38140-2019. Three replicates were prepared for each test case, and the average value was taken. The results are shown in Table 1.
[0137] Table 1
[0138]
[0139] As shown in Table 1, the 7-day compressive strength of the cementitious material obtained by this invention is not less than 40 MPa, and the 28-day compressive strength is not less than 70 MPa. Furthermore, its compressive strength continues to increase after prolonged immersion in seawater, indicating that the internal structure of the cementitious material becomes denser and its strength remains improved even after seawater erosion. The resulting cementitious material exhibits excellent resistance to salt erosion. Simultaneously, the 28-day shrinkage rate of the cementitious material of this invention does not exceed 0.080%, and its contact angle with water is not less than 90°, indicating that this cementitious material not only has a low shrinkage rate but also good hydrophobic properties, giving it a wider range of applications than general cementitious materials.
[0140] The 7-day and 28-day compressive strength and the compressive strength after seawater immersion of the cementitious materials obtained in each embodiment are significantly higher than those obtained in each comparative example. This is because industrial solid waste and active components can cooperate and complement each other. With the cooperation and synergy of catalysts and auxiliary agents, they can be activated and reacted by utilizing their own characteristics to form a more dense three-dimensional network gel structure with hydrophobic functional groups introduced at the ends of the molecular chains. This reduces the affinity of the cementitious material for water and reduces the diffusion coefficient of water and external ions in the cementitious material. This is beneficial to enhance the cementitious material's resistance to frost heave and erosion. At the same time, it can continuously provide strength development. Even in environments with high salt content, the strength can continue to increase in the later stage, increasing the durability of the cementitious material and the service life of the project.
[0141] Comparing the gelling materials of the various embodiments and comparative examples reveals that no auxiliary agents were added in the comparative examples, meaning no polymer chain segments were introduced into the gel structure. As a result, the materials still exhibit good hydrophilicity. Consequently, during the erosion process of seawater, the internal physicochemical environment undergoes significant changes. The reaction of ionic polymerization to form a gel is inhibited, and the already formed gel continuously disintegrates under the attack of ions. This leads to an increase in the porosity of the gelling material system, a rapid decrease in strength, and a significant reduction in durability and service life. This demonstrates that the introduction of the auxiliary agents in this invention has a significant beneficial effect on the hydrophobicity, strength, and salt erosion resistance of the gelling material.
[0142] Comparing the results of Examples 5 and 6-10, it was found that when the catalyst and auxiliary agent ratios were relatively simple, the reactivity of the raw materials could not be effectively activated, resulting in poor density of the cementitious material. Its early and later strengths were lower than those of the compounded cementitious material in Example 5, and its shrinkage rate was also greater. Although its strength increased after soaking in seawater, the increase was significantly less than that in Example 5. This further illustrates that when different types of catalysts and auxiliary agents are used in combination, they can more fully activate other types of raw materials, promoting a more complete reaction between different raw material components, thereby further improving the strength and durability of the cementitious material.
[0143] Comparing the results of Example 1 and Examples 11-12, it was found that the composition of industrial solid waste and active components in Examples 11 and 12 was not reasonable enough. They could not provide more active ions and other components in the gel, which easily led to the gel structure being not dense enough, failing to form a good complementary effect, and reducing the strength, water resistance and durability of the gelling material.
[0144] It should be noted that some detailed steps of the operation are not described in this invention, but are existing technologies known to those skilled in the art, and therefore will not be repeated here. Furthermore, in this invention, all features defined in the form of numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible secondary ranges and individual numerical values (including integers and fractions) within those ranges.
[0145] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. In this invention, not all possible combinations of the various technical features in each embodiment or implementation are described. As long as the combinations of these technical features do not contradict each other, the various technical features in each embodiment or implementation can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A self-excited hydrophobic industrial solid waste-based cementitious material, characterized in that, It consists of the following raw materials in parts by weight: 75-118 parts of component A and 3-6 parts of component B; Component A consists of: industrial solid waste, active components, and catalyst; Component B is an auxiliary agent; Component A comprises the following parts by weight: 50-70 parts of industrial solid waste, 20-40 parts of active components, and 5-8 parts of catalyst; The industrial solid waste comprises the following components by weight: 10-15 parts calcium carbide slag, 5-10 parts tungsten ore slag, 10-15 parts red mud, 5-10 parts copper slag, 20-60 parts ore slag, and 2-5 parts industrial by-product gypsum. The active component comprises the following components in parts by weight: 15-70 parts silica fume, 20-80 parts metakaolin, and 5-10 parts glass powder; The catalyst is a combination of phosphate, carbonate, and alkanolamine; the phosphate includes one or more of sodium pyrophosphate, sodium tripolyphosphate, sodium polyphosphate, potassium phosphate, and ammonium phosphate; the alkanolamine includes one or more of monoethanolamine, diethanolamine, triethanolamine, and monoisopropanolamine; the carbonate includes one or more of sodium carbonate, potassium carbonate, calcium carbonate, and sodium bicarbonate. The auxiliary agent is a combination of methyltrimethoxysilane, 3-aminopropyltriethoxysilane and γ-methacryloxypropyltrimethoxysilane, a combination of 3-aminopropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane, or a combination of methyltrimethoxysilane, 3-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.
2. A method for preparing a self-excited hydrophobic industrial solid waste-based cementitious material as described in claim 1, characterized in that, Includes the following steps: Industrial solid waste, active components, and catalysts are mixed to obtain component A; Mix the raw materials of each component in the auxiliary agent to obtain component B.
3. A method of using a self-activated hydrophobic industrial solid waste-based cementitious material, wherein the cementitious material is the self-activated hydrophobic industrial solid waste-based cementitious material according to claim 1, or the self-activated hydrophobic industrial solid waste-based cementitious material prepared by the preparation method according to claim 2, characterized in that... Includes the following steps: Step 1): Mix component A with water and stir for 5-10 minutes to obtain the cementitious material precursor; Step 2): Mix component B with water and stir for 10-30 minutes to obtain a mixture; Step 3): Add the mixture to the cementitious material precursor, mix evenly, and then cure and solidify to complete the use of the self-excited hydrophobic industrial solid waste-based cementitious material.
4. The method of using the self-activating hydrophobic industrial solid waste-based cementitious material according to claim 3, characterized in that, In the method of use, the ratio of total water consumption to the weight of the cementitious material is (0.2-0.3):1; In step 1), the amount of water used for component A is 65-75% of the total amount of water used, and the remaining water is used in step 2) to prepare the mixture from component B.
Citation Information
Patent Citations
High folding resistance road concrete material and preparing method thereof
CN101265066A
Cementing material and preparation method thereof
CN109231860A
Low-carbon cementing material and preparation method thereof
CN116874210A